Large-particle-size magnetic polystyrene microspheres as well as preparation method and application thereof

The preparation of large-particle magnetic polystyrene microspheres by suspension polymerization method has solved the problem of particle size control and bond agglomeration in the prior art, and achieved uniformity and monodispersity of particle size between 30 μm and 60 μm. Super paramagnetic and corrosion resistance.

CN119039535AInactive Publication Date: 2024-11-29YANSHAN UNIV

Patent Information

Application Number
CN202411309033.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

It is difficult to prepare large-particle magnetic polystyrene microspheres in the prior art, and the existing methods have problems of bonding and agglomeration in the preparation of magnetic microspheres, and cannot effectively control the particle size and monodispersity.

Method used

Using suspension polymerization method, magnetic Fe3O4 particles are used as magnetic cores, surface adsorption initiators and monomers, and through mechanical stirring and dispersing agents, a large-size magnetic polystyrene microsphere is formed, with a particle size between 30μm and 60μm. The stability and spherical regularity of the suspended particles are ensured by controlling the reaction conditions such as the type of dispersant, the amount of monomer and initiator, the stirring strength and the polymerization temperature.

Benefits of technology

Large-size magnetic polystyrene microspheres with uniform particle size, regular and good monodispersity were successfully prepared, which had super paramagnetic properties and good corrosion resistance, simplifying the preparation process and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039535A_ABST
    Figure CN119039535A_ABST
Patent Text Reader

Abstract

The invention relates to a large-particle-size magnetic polystyrene microsphere as well as a preparation method and application thereof, and belongs to the technical field of magnetic material preparation. Magnetic Fe3O4 particles serve as magnetic cores, a large number of initiators and monomers are adsorbed on the surfaces of the magnetic Fe3O4 particles, the magnetic Fe3O4 particles are dispersed into tiny liquid drops under the action of mechanical stirring and a dispersing agent or a suspending agent and become centers for initiating polymerization, the monomers are mutually polymerized to form polymer molecular chains, the polymer molecular chains are wound outside the magnetic cores, Fe3O4 is wrapped in the polymer molecular chains, and the magnetic microspheres are formed through later curing. The particle size of the prepared magnetic polystyrene microspheres is 30 [mu] m-60 [mu] m. The preparation method is simple and short in time consumption, and the prepared microspheres are good in dispersity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of magnetic material preparation, and in particular relates to a method for preparing large-diameter magnetic polystyrene microspheres. Background Art

[0002] Magnetic polymer microspheres refer to a type of composite microspheres formed by the combination of inorganic nanomagnetic particles and organic polymer materials. They have both the magnetism of inorganic magnetic materials and the modifiability of organic polymers, and have the advantages of easy magnetic separation and good adsorption performance. They have broad application prospects in magnetic physics, chemical engineering, environmental monitoring, immobilized enzymes, protein separation, cell separation, targeted drugs, and immunoassay.

[0003] At present, the preparation of magnetic polymer microspheres mainly adopts polymer polymerization in the presence of magnetic particles, including emulsion polymerization, miniemulsion polymerization, dispersion polymerization, suspension polymerization, etc., that is, monomer polymerization in the presence of magnetic particles, initiators, dispersants, etc.

[0004] It is very necessary to provide a method for preparing large-size magnetic polystyrene microspheres. Summary of the invention

[0005] In view of the problems existing in the above-mentioned prior art, the object of the present invention is to design and provide a method for preparing large-size magnetic polystyrene microspheres.

[0006] The present invention uses magnetic Fe3O4 particles as magnetic cores, and a large amount of initiators and monomers are adsorbed on the surface of the particles. Under the action of mechanical stirring and a dispersant or a suspending agent, the particles are dispersed into tiny droplets, which become the center for initiating polymerization. The monomers polymerize with each other to form polymer molecular chains that wrap around the outside of the magnetic core, encapsulating the Fe3O4 therein, and are later solidified into magnetic microspheres.

[0007] In order to achieve the above purpose, the following technical solutions are adopted:

[0008] In the first aspect, the present invention provides a large-particle magnetic polystyrene microsphere, which uses magnetic Fe3O4 particles as magnetic cores, and a number of initiators and monomers are adsorbed on the surface of the magnetic Fe3O4 particles. The monomers polymerize with each other to form polymer molecular chains that are wrapped around the outside of the magnetic core; the particle size of the large-particle magnetic polystyrene microsphere is 30μm to 60μm.

[0009] In a second aspect, the present invention provides a method for preparing the large-size magnetic polystyrene microspheres, comprising the following steps:

[0010] (1) Nano-sized Fe3O4 particles are prepared by chemical coprecipitation method, dispersed in water and stored for later use to obtain magnetic fluid; (2) a dispersant or suspending agent is weighed in a dispersion medium, mixed with the magnetic fluid at 60° C. and stirred evenly to form an aqueous phase; (3) an oil phase composed of an initiator and a monomer is weighed and ultrasonically dispersed for 10 minutes, and then the oil phase is added to the aqueous phase. The two phases are reacted at 75° C. for 2 h to 4 h, and the product is repeatedly washed with water and alcohol to obtain the large-size magnetic polystyrene microspheres.

[0011] Furthermore, the step (1) specifically comprises: dissolving FeCl3·6H2O and FeCl2·4H2O in deionized water, stirring, adding SDS when heated to 50°C to 60°C, adding ammonia water after reacting for 10 minutes, heating to 80°C, reacting for 15 minutes, stopping stirring, naturally settling for 1 hour, cooling to room temperature, performing magnetic separation, washing, and obtaining magnetic Fe3O4 particles; preferably, the mass ratio of FeCl3·6H2O to FeCl2·4H2O is 0.27:1 to 0.9:1.

[0012] Furthermore, the volume ratio of the magnetic fluid to the dispersion medium added in step (2) is 1:500 to 1:200.

[0013] Furthermore, in step (2), the dispersant or suspending agent includes one or more of polyvinyl alcohol, gelatin, calcium hydroxyphosphate, carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose; and the dispersion medium includes one or more of deionized water, anhydrous ethanol, and methanol.

[0014] Furthermore, in step (2), the volume ratio of the dispersant or suspending agent to the dispersion medium is 1:100 to 1:15.

[0015] Furthermore, in the step (3), the initiator includes an oil-soluble initiator, preferably one or more of organic azo initiators such as azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptylnitrile, etc.; the monomer includes one or more of styrene, divinylbenzene, methacrylic acid, and acrylic acid.

[0016] Furthermore, the mass ratio of the initiator to the dispersant or suspending agent added in step (2) is 1:2 to 1:1.

[0017] Furthermore, the volume ratio of the monomer to the dispersion medium added in step (2) is 1:10 to 1:2.

[0018] In a third aspect, the present invention provides the application of the large-diameter magnetic polystyrene microspheres in the biomedical field.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention adopts a suspension polymerization method and utilizes a suitable dispersant (such as polyvinyl alcohol (PVA)) to control the polymerization reaction on the surface of magnetic particles and the miscibility of magnetic particles with olefin monomers, thereby ensuring the stability of suspended particles and preventing adhesion; and studies the effects of various reaction conditions (such as: the type and amount of dispersant, the amount of monomer and initiator, stirring intensity, polymerization temperature, polymerization time, etc.) on the production of microspheres.

[0021] The invention prepares the target large-size magnetic polystyrene microspheres by suspension polymerization, the particle size of which is between 30 μm and 60 μm, and the preparation method is simple, the microspheres have a relatively smooth and regular spherical shape, no large amount of agglomeration, good monodispersity, superparamagnetism and good corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A schematic diagram of a scanning electron microscope showing the large-size magnetic polystyrene microspheres prepared in Example 1;

[0023] Figure 2 This is a schematic diagram of a scanning electron microscope of large-size magnetic polystyrene microspheres prepared in Example 2;

[0024] Figure 3 This is a schematic diagram of a scanning electron microscope of large-size magnetic polystyrene microspheres prepared in Example 2;

[0025] Figure 4 This is a schematic diagram of a scanning electron microscope of large-size magnetic polystyrene microspheres prepared in Example 4. DETAILED DESCRIPTION

[0026] At present, suspension polymerization is an important polymerization method. The polymers produced by this method include polystyrene, polyvinyl chloride, vinylidene chloride copolymers, acrylate and methacrylate polymers, polyvinyl acetate, etc. Its output accounts for about 20% to 25% of the total polymer output. This shows the importance of suspension polymerization in the polymer industry.

[0027] Compared with emulsion polymerization and dispersion polymerization, suspension polymerization has many advantages, such as: ① Water is used as the medium, which is cheap, does not require recycling, is safe, and the product is easy to separate, and the production cost is low; ② The viscosity of the suspension polymerization system is low, the temperature is easy to control, and the product quality is stable; ③ The amount of dispersant adsorbed on the suspension polymer is small, and some are easy to remove, and the product contains fewer impurities. It is precisely because of these advantages that suspension polymerization has been widely used in industry. In addition, due to the influence of the mechanism in the preparation process of magnetic microspheres, emulsion polymerization and dispersion polymerization cannot prepare magnetic polystyrene microspheres with large particle sizes of tens of microns to hundreds of microns.

[0028] In view of this, the present application provides a large-particle magnetic polystyrene microsphere, which is prepared by suspension polymerization to obtain the target microsphere, with a particle size between 30μm and 60μm, and the preparation method is simple, with a relatively smooth and regular spherical shape, no large amount of agglomeration, and good monodispersity; and has superparamagnetism and good corrosion resistance.

[0029] The present invention is described in detail below in conjunction with specific implementation modes.

[0030] Embodiment 1:

[0031] Embodiment 1 provides a method for preparing large-size magnetic polystyrene microspheres by suspension polymerization, the preparation method comprising:

[0032] (1) Preparation of magnetic Fe3O4 particles: Weigh 2 g of FeCl3·6H2O and 2.5 g of FeCl2·4H2O and dissolve them in 50 mL of water. Heat to 56°C, add 0.2 g of SDS, stir and react at 400 rpm for 10 min, then add 30 mL of ammonia water, heat to 80°C, react for 15 min, stop stirring, and let stand for 1.5 h. After the reaction is completed, use a magnet for magnetic separation, wash with deionized water and ethanol alternately for multiple times to remove the reaction residual components and by-products, and store in deionized water to obtain magnetic Fe3O4 particles.

[0033] (2) Preparation of magnetic polystyrene microspheres: Weigh 3g polyvinyl alcohol, 75ml deionized water and 75ml alcohol to form the water phase, stir at a constant speed in a 55°C water bath, add 0.3g magnetic fluid at 60°C, weigh 3g initiator, 10ml monomer, 1ml comonomer and 2ml AA to form the oil phase, ultrasonically disperse for 10 minutes and add to the water phase, place the mixed two phases in a 75°C water bath for reaction, and stir for 2h-4h. Apply an external magnetic field, and repeatedly wash the product with water and alcohol to remove the non-magnetic microspheres, stabilizer and a small amount of unreacted monomer to obtain large-size magnetic polystyrene microspheres. Its scanning electron micrograph is as follows Figure 1 , it can be seen that the particle size range is 40-50μm.

[0034] Embodiment 2:

[0035] Embodiment 2 provides a method for preparing large-size magnetic polystyrene microspheres by suspension polymerization, the preparation method comprising:

[0036] (1) Preparation of magnetic Fe3O4 particles: Weigh 2 g of FeCl3·6H2O and 2.5 g of FeCl2·4H2O and dissolve them in 50 mL of water. Heat to 56°C, add 0.2 g of SDS, stir and react at 400 rpm for 10 min, then add 30 mL of ammonia water, heat to 80°C, react for 15 min, stop stirring, and let stand for 1.5 h. After the reaction is completed, use a magnet for magnetic separation, wash with deionized water and ethanol alternately for multiple times to remove the residual components and by-products of the reaction, and store in deionized water to obtain superparamagnetic Fe3O4 nanoparticles.

[0037] (2) Preparation of magnetic polystyrene microspheres: Weigh 3g polyvinyl alcohol, 0.25g polyvinyl pyrrolidone, 50ml deionized water and 100ml alcohol to form the aqueous phase, stir at a constant speed in a 55°C water bath, add 0.3g magnetic fluid at 70°C, weigh 1g initiator, 10ml monomer, 3ml comonomer and 2ml AA to form the oil phase, ultrasonically disperse for 10 minutes and add to the aqueous phase, place the mixed two phases in a 75°C water bath for reaction, and stir for 2h-4h. Apply an external magnetic field, and repeatedly wash the product with water and alcohol to remove the non-magnetic microspheres, stabilizer and a small amount of unreacted monomer to obtain large-size magnetic polystyrene microspheres. Its scanning electron micrograph is as follows Figure 2 , Figure 3 , it can be seen that the particle size ranges from 50 to 70 μm.

[0038] Embodiment 3:

[0039] Example 3 provides a method for preparing large-size magnetic polystyrene microspheres by suspension polymerization, the preparation method comprising:

[0040] (1) Preparation of magnetic Fe3O4 particles: Weigh 2 g of FeCl3·6H2O and 2.5 g of FeCl2·4H2O and dissolve them in 50 mL of water. Heat to 56°C, add 0.2 g of SDS, stir and react at 400 rpm for 10 min, then add 30 mL of ammonia water, heat to 80°C, react for 15 min, stop stirring, and let stand for 1.5 h. After the reaction is completed, use a magnet for magnetic separation, wash with deionized water and ethanol alternately for multiple times to remove the residual components and by-products of the reaction, and store in deionized water to obtain superparamagnetic Fe3O4 nanoparticles.

[0041] (2) Preparation of magnetic polystyrene microspheres: 3g polyvinyl alcohol, 50ml deionized water and 100ml alcohol were weighed to form the water phase, stirred at a constant speed in a water bath at 55°C, 0.3g magnetic fluid was added at 60°C, 3g initiator, 15ml monomer, 1ml comonomer and 4ml AA were weighed to form the oil phase, ultrasonically dispersed for 10min, and added to the water phase. The mixed two phases were placed in a 75°C water bath for reaction and stirred for 2h-4h. An external magnetic field was applied, and the product was repeatedly washed with water and alcohol to remove the non-magnetic microspheres, stabilizer and a small amount of unreacted monomers, and large-size magnetic polystyrene microspheres were obtained.

[0042] Embodiment 4:

[0043] Example 4 provides a method for preparing large-size magnetic polystyrene microspheres by suspension polymerization, the preparation method comprising:

[0044] (1) Preparation of magnetic Fe3O4 particles: Weigh 2 g of FeCl3·6H2O and 2.5 g of FeCl2·4H2O and dissolve them in 50 mL of water. Heat to 56°C, add 0.2 g of SDS, stir and react at 400 rpm for 10 min, then add 30 mL of ammonia water, heat to 80°C, react for 15 min, stop stirring, and let stand for 1.5 h. After the reaction is completed, use a magnet for magnetic separation, wash with deionized water and ethanol alternately for multiple times to remove the residual components and by-products of the reaction, and store in deionized water to obtain superparamagnetic Fe3O4 nanoparticles.

[0045] (2) Preparation of magnetic polystyrene microspheres: Weigh 3g polyvinyl alcohol, 50ml deionized water and 75ml alcohol to form the water phase, stir at a constant speed in a 55°C water bath, add 0.2g magnetic fluid at 60°C, weigh 1g initiator, 10ml monomer, and 3ml comonomer to form the oil phase, ultrasonically disperse for 10 minutes, and add to the water phase. The mixed two phases are placed in a 75°C water bath for reaction and stirred for 2h-4h. Apply an external magnetic field, and repeatedly wash the product with water and alcohol to remove the non-magnetic microspheres, stabilizer and a small amount of unreacted monomer to obtain large-size magnetic polystyrene microspheres. Its scanning electron micrograph is as follows Figure 4 , it can be seen that the particle size range is 40-50μm.

[0046] Those skilled in the art can understand that the above-mentioned embodiments are specific examples for implementing the present application, and in practical applications, various changes can be made to them in form and detail without departing from the spirit and scope of the present application. Any person skilled in the art can make their own changes and modifications without departing from the spirit and scope of the present application, so the scope of protection of the present application shall be based on the scope defined in the claims.

Claims

1. A large-size magnetic polystyrene microsphere, characterized in that: The large-size magnetic polystyrene microspheres have magnetic Fe3O4 particles as magnetic cores, and the surfaces of the magnetic Fe3O4 particles are adsorbed with a number of initiators and monomers, and the monomers are polymerized to form polymer molecular chains that are wrapped around the outside of the magnetic cores; The particle size of the large-particle magnetic polystyrene microspheres is 30 μm to 60 μm.

2. The method for preparing large-size magnetic polystyrene microspheres according to claim 1, characterized in that: The following steps are involved: (1) preparing nanometer-sized Fe3O4 particles by chemical coprecipitation method, dispersing them in water and preserving them for later use, thereby obtaining magnetic fluid; (2) weighing a dispersant or a suspending agent into a dispersion medium, mixing it with the magnetic fluid at 60° C., and stirring it evenly to form an aqueous phase; (3) Weighing an oil phase composed of an initiator and a monomer and ultrasonically dispersing the oil phase for 10 minutes, then adding the oil phase to the water phase, and reacting the two phases at 75° C. for 2 h to 4 h. The product is repeatedly washed with water and alcohol to obtain the large-size magnetic polystyrene microspheres.

3. The method for preparing large-size magnetic polystyrene microspheres according to claim 2, characterized in that: The step (1) specifically comprises: Dissolve FeCl3·6H2O and FeCl2·4H2O in deionized water, stir, and add SDS when heated to 50℃~60℃. After reacting for 10 minutes, add ammonia water, heat to 80℃, react for 15 minutes, stop stirring, and naturally settle for 1 hour, then cool to room temperature, perform magnetic separation, and wash to obtain magnetic Fe3O4 particles. Preferably, the mass ratio of FeCl3·6H2O to FeCl2·4H2O is 0.27:1 to 0.9:

1.

4. The method for preparing large-size magnetic polystyrene microspheres according to claim 2, characterized in that: The volume ratio of the magnetic fluid to the dispersion medium added in step (2) is 1:500 to 1:

200.

5. The method for preparing large-size magnetic polystyrene microspheres according to claim 2, characterized in that: In the step (2), the dispersant or suspending agent includes one or more of polyvinyl alcohol, gelatin, calcium hydroxyphosphate, carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose; The dispersion medium includes one or more of deionized water, anhydrous ethanol and methanol.

6. The method for preparing large-size magnetic polystyrene microspheres according to claim 2, characterized in that: In the step (2), the volume ratio of the dispersant or suspending agent to the dispersion medium is 1:100 to 1:

15.

7. The method for preparing large-size magnetic polystyrene microspheres according to claim 2, characterized in that: In the step (3), the initiator comprises an oil-soluble initiator, preferably one or more organic azo initiators such as azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, etc.; The monomers include one or more of styrene, divinylbenzene, methacrylic acid, and acrylic acid.

8. The method for preparing large-size magnetic polystyrene microspheres according to claim 2, characterized in that: The mass ratio of the initiator to the dispersant or suspending agent added in step (2) is 1:2 to 1:

1.

9. The method for preparing large-size magnetic polystyrene microspheres according to claim 2, characterized in that: The volume ratio of the monomer to the dispersion medium added in step (2) is 1:10 to 1:

2.

10. Use of the large-diameter magnetic polystyrene microspheres according to claim 1 in the biomedical field.

Citation Information

Patent Citations

  • Method for preparing magnetic-targeted thermochemotherapy gold shell nano-drug delivery system

    CN101954085A

  • Preparation method of micron-sized acrylic acid-rosin magnetic polymer microballoon

    CN102344536A

  • Method for preparing magnetic porous polystyrene microspheres on basis of suspension polymerization

    CN103627022A

  • Magnetic resin microspheres and preparation method thereof

    CN104072659A

  • Magnetic solid-phase extraction microspheres and preparation method thereof

    CN115894978A