Biochar synergistic flame-retardant silicone rubber and preparation method thereof

By adding modified biochar and expandable graphite to silicon rubber and using silicon nitride to form a dense carbon layer, the problem of poor flame retardant effect of silicon rubber is solved, the oxygen index and tensile strength are significantly improved, and better results are achieved flame retardant properties.

CN119039786APending Publication Date: 2024-11-29LIAONING MACROMOLECULE NEW MATERIAL TECHNOLOGY R&D CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411386527.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Silicone rubber has poor flame retardant effect, and the expansion layer structure is unstable when used alone, which affects its flame retardant effect.

Method used

Using biochar synergistic flame retardant silicone rubber, the addition of modified biochar filler and expandable graphite, and using silicon nitride to promote the formation of a dense carbon layer, combined with vulcanizing agent and structural adjusting agent, a good flame retardant performance is prepared. Silicone rubber.

Benefits of technology

It significantly improves the flame retardant performance of silicone rubber, forms a tight carbon layer structure, inhibits heat and oxygen transfer, improves the oxygen index and tensile strength, and achieves better vertical combustion flame retardant grade and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039786A_ABST
    Figure CN119039786A_ABST
Patent Text Reader

Abstract

The invention provides charcoal synergistic flame-retardant silicone rubber and a preparation method thereof, and belongs to the technical field of high polymer materials. The invention relates to biochar synergistic flame-retardant silicone rubber, which is prepared from the following ingredients in parts by mass: 100 parts of silicone rubber matrixes, 10 to 30 parts of white carbon black, 1 to 3 parts of structure regulators, 1 to 3 parts of coupling agents, 2 to 5 parts of zinc oxide, 1 to 2 parts of stearic acid, 1 to 3 parts of modified biochar fillers, 1 to 5 parts of expansible graphite and 1 to 2 parts of vulcanizing agents. Silicon nitride is adsorbed on the surface of the biochar, and a large amount of silicon nitride is deposited on the surface of the biochar in a combustion process to form a relatively compact expansion layer, so that heat can be blocked and decomposition of the silicon rubber can be inhibited during combustion of the silicon rubber; meanwhile, due to the porous characteristic of the biochar, a very good inhibition effect on heat and smoke can be achieved in the combustion behavior.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of polymer materials, and in particular to a biochar-synergistic flame-retardant silicone rubber and a preparation method thereof. Background Art

[0002] Silicone rubber is a polymer material with excellent high and low temperature resistance, good insulation and good chemical stability. It is widely used in electronic appliances, medical equipment, aerospace and other fields. Although silicone rubber has good high temperature resistance, it is very flammable, which greatly limits the application of silicone rubber in some important fields. Therefore, how to improve the flame retardant properties of silicone rubber is one of the main problems that need to be solved in the field of silicone rubber.

[0003] Biochar is a porous carbon material obtained by converting biomass (such as wood, agricultural waste, etc.) in an oxygen-deficient or low-oxygen environment through a pyrolysis process. It has excellent physical and chemical properties. At high temperatures, biochar can form a carbonized layer that can prevent the transfer of heat and oxygen, thereby inhibiting the spread of flames. In addition, biochar has high thermal stability, can withstand higher temperatures, and reduce the combustion rate under flames.

[0004] Existing silicone rubber flame retardants mainly include mineral, phosphorus-containing, nitrogen-containing and nanocomposites. Mineral flame retardants (such as aluminum hydroxide) are very effective in reducing fire hazards, but a large amount of mineral flame retardants must be added to achieve the desired flame retardant effect, and these high-load flame retardants will cause material defects; halogen-containing flame retardants are a cost-effective technology, but due to environmental and health considerations, the use of halogen flame retardants has been increasingly restricted. In recent years, halogen-free flame retardants have become the main research direction of scientific researchers, and expandable graphite is a type of halogen-free flame retardant. Expandable graphite has the advantages of being non-toxic, simple and easy to obtain raw materials, and good flame retardant effect, and is widely used as a flame retardant filler for polymers. However, when expandable graphite is used alone, its expansion during heating is uncontrollable, resulting in a loose carbon layer that is not dense enough, affecting its flame retardant effect. Silicon nitride is an inorganic material with excellent thermal and chemical stability, and is widely used in the field of flame retardancy. Silicon nitride has good thermal stability at high temperatures, and can promote the carbonization reaction of organic materials to form more stable carbonized products, further improving the flame retardant properties of the material. Therefore, silicon nitride and biochar have a good synergistic effect, which helps biochar form a dense carbon surrounding structure and then cooperate with expandable graphite to achieve a good flame retardant effect. Summary of the invention

[0005] A technical problem to be solved by the present disclosure is that silicone rubber has poor flame retardant effect, and when used alone with expandable graphite, the expansion layer structure is unstable, resulting in unsatisfactory flame retardant effect of silicone rubber, affecting the application of silicone rubber in flame retardancy.

[0006] In order to solve the above technical problems, the present disclosure provides a biochar-synergistic flame-retardant silicone rubber, which includes:

[0007] The following parts by mass: 100 parts of silicone rubber matrix, 10-30 parts of white carbon black, 1-3 parts of structure regulator, 1-3 parts of coupling agent, 2-5 parts of zinc oxide, 1-2 parts of stearic acid, 1-3 parts of modified biochar filler, 1-5 parts of expandable graphite, and 1-2 parts of vulcanizing agent.

[0008] In some embodiments, the aforementioned biochar synergistic flame retardant silicone rubber, wherein the silicone rubber matrix is ​​one of: methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, fluorosilicone rubber and dimethyl silicone rubber.

[0009] In some embodiments, the aforementioned biochar synergistic flame retardant silicone rubber, wherein the coupling agent is one of: γ-aminopropyltriethoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, and γ-mercaptopropyltrimethoxysilane.

[0010] In some embodiments, in the aforementioned biochar synergistic flame retardant silicone rubber, the vulcanizing agent is one of dicumyl peroxide, benzoyl peroxide, and dipentadienyl vulcanizing agent.

[0011] In some embodiments, in the aforementioned biochar synergistic flame retardant silicone rubber, the modified biochar filler is a composite system of biochar and silicon nitride.

[0012] In some embodiments, the aforementioned biochar synergistic flame retardant silicone rubber, wherein the preparation method of the modified biochar filler is: silicon nitride is placed in deionized water to prepare a silicon nitride suspension, the suspension is ultrasonically dispersed for 3 hours and then set aside, rice husks, wheat straw and other crop waste are physically washed to remove impurities and dirt, placed in an 80°C drying oven for 24 hours, and then crushed with a grinder, the crushed material is added to the silicon nitride suspension, magnetically stirred for 2 hours, and then filtered and dried, the dried sample is placed in a tubular furnace, nitrogen is introduced at a flow rate of 15 ml / min, and the temperature is increased to 500°C at a heating rate of 5°C / min, pyrolyzed for 1 hour, and the sample is taken out after the tubular furnace is cooled, and the product is a silicon nitride biochar composite material.

[0013] In some embodiments, in the aforementioned biochar synergistically flame-retardant silicone rubber, the mass concentration of silicon nitride in the silicon nitride suspension is 1%.

[0014] In some embodiments, the aforementioned biochar synergistic flame retardant silicone rubber, wherein the silicon nitride is hexagonal nano-scale silicon nitride, with a purity greater than or equal to 99.9%, a particle size of 500 nm, and a hexagonal crystal.

[0015] The second aspect of the present application provides a method for preparing a biochar-synergistic flame-retardant silicone rubber, which comprises the biochar-synergistic flame-retardant silicone rubber according to any one of claims 1 to 8, and the specific steps are as follows:

[0016] S1, kneading the silicone rubber matrix in a two-roll mill, and then adding hydroxy silicone oil of white carbon black for mixing;

[0017] S2, adding a coupling agent, modified biochar filler, expandable graphite, zinc oxide and stearic acid to the mixed material of S1 and continuing to mix to obtain a mixed rubber;

[0018] S3, cooling the mixed rubber in S2 for 24 hours, adding a vulcanizing agent and continuing to mix to obtain a first rubber compound;

[0019] S4, after the first rubber compound mixed in S3 is pressed into sheets, it is placed on a flat vulcanizer for heating and vulcanization, and then placed in an oven for two-stage vulcanization, and finally the biochar material synergistic flame retardant silicone rubber is obtained.

[0020] In some embodiments, the aforementioned method for preparing biochar-synergistic flame-retardant silicone rubber, wherein the temperature of the vulcanizer heating vulcanization is 160°C, the time is 30 minutes, and the pressure is 8-10MPa; the temperature of the secondary vulcanization is 200°C, and the time is 4 hours.

[0021] Through the above technical scheme, the present disclosure provides a biochar-synergistic flame-retardant silicone rubber, which can promote the biochar to form a dense and continuous carbon layer structure through silicon nitride. The adsorption of silicon nitride on the surface of the biochar can make a large amount of silicon nitride deposit on the surface of the biochar to form a relatively tight expansion layer during the combustion process, which helps to block heat and inhibit the decomposition of silicone rubber. In addition, due to the porous characteristics of biochar, it can also have a good inhibitory effect on heat and smoke during combustion. Then, in combination with expandable graphite, a good flame retardant effect is achieved. In addition, the added modified biochar material can ensure the mechanical properties of silicone rubber while also having the characteristics of low cost and simple and convenient synthesis, which provides a new direction for the selection of flame retardant fillers. Therefore, by adding biochar modified with silicon nitride, the flame retardant effect of silicone rubber is more significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present disclosure or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0023] Figure 1 It is a flow chart of a method for preparing biochar-synergistic flame-retardant silicone rubber disclosed in an embodiment of the present disclosure;

[0024] Figure 2 It is a mechanism diagram of the preparation of modified biochar in a method for preparing biochar-synergistic flame-retardant silicone rubber disclosed in an embodiment of the present disclosure. DETAILED DESCRIPTION

[0025] The following is a further detailed description of the embodiments of the present disclosure in conjunction with the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to exemplarily illustrate the principles of the present disclosure, but cannot be used to limit the scope of the present disclosure. The present disclosure can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

[0026] The present disclosure provides these embodiments to make the present disclosure thorough and complete, and to fully express the scope of the present disclosure to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of the materials, the numerical expressions and the numerical values ​​set forth in these embodiments should be interpreted as being merely exemplary, and not as limiting.

[0027] In addition, the words "first", "second" and similar words used in the present disclosure do not indicate any order, quantity or importance, but are only used to distinguish different parts. "Vertical" does not mean vertical in the strict sense, but is within the tolerance range. "Parallel" does not mean parallel in the strict sense, but is within the tolerance range. "Include" or "comprising" and similar words mean that the elements before the word include the elements listed after the word, and do not exclude the possibility of including other elements.

[0028] It should also be noted that in the description of the present disclosure, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present disclosure can be understood according to the specific circumstances. When a specific device is described as being located between a first device and a second device, there may or may not be an intermediate device between the specific device and the first device or the second device.

[0029] All terms used in the present disclosure have the same meanings as those understood by those of ordinary skill in the art to which the present disclosure belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, for example, should be interpreted as having meanings consistent with their meanings in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined as such herein.

[0030] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered part of the specification.

[0031] Embodiment 1

[0032] This embodiment discloses a biochar synergistic flame retardant silicone rubber, which includes 100 parts of silicone rubber matrix, 3 parts of expanded graphite, 2 parts of modified biochar, 2 parts of vulcanizing agent, 30 parts of white carbon black, 2 parts of coupling agent, 2 parts of zinc oxide, 1 part of stearic acid, and 1 part of structural adjustment agent. The specific preparation method is as follows: Figure 1 shown.

[0033] Embodiment 2

[0034] The present embodiment discloses a biochar synergistic flame retardant silicone rubber, which includes 100 parts of silicone rubber matrix, 5 parts of expanded graphite, 2 parts of modified biochar, 2 parts of vulcanizer, 30 parts of white carbon black, 2 parts of coupling agent, 2 parts of zinc oxide, 1 part of stearic acid, and 1 part of structure regulator.

[0035] The difference from Example 1 is that the amount of expanded graphite is 5 parts and the amount of modified biochar is 2 parts.

[0036] Comparative Example 1

[0037] The present embodiment discloses a biochar synergistic flame retardant silicone rubber, which includes 100 parts of silicone rubber matrix, 2 parts of vulcanizing agent, 30 parts of white carbon black, 2 parts of coupling agent, 2 parts of zinc oxide, 1 part of stearic acid, and 1 part of structure regulator.

[0038] The difference from Example 1 is that no expanded graphite and modified biochar are added.

[0039] Comparative Example 2

[0040] The present embodiment discloses a biochar synergistic flame retardant silicone rubber, which includes 100 parts of silicone rubber matrix, 1 part of expanded graphite, 2 parts of vulcanizer, 30 parts of white carbon black, 2 parts of coupling agent, 2 parts of zinc oxide, 1 part of stearic acid, and 1 part of structure regulator.

[0041] The difference from Example 1 is that the amount of expanded graphite is 1 part, and no modified biochar is added.

[0042] Comparative Example 3

[0043] The present embodiment discloses a biochar synergistic flame retardant silicone rubber, which includes 100 parts of silicone rubber matrix, 3 parts of expanded graphite, 2 parts of vulcanizer, 30 parts of white carbon black, 2 parts of coupling agent, 2 parts of zinc oxide, 1 part of stearic acid, and 1 part of structure regulator.

[0044] The difference from Example 1 is that the amount of expanded graphite is 3 parts, and no modified biochar is added.

[0045] Comparative Example 4

[0046] The present embodiment discloses a biochar synergistic flame retardant silicone rubber, which includes 100 parts of silicone rubber matrix, 5 parts of expanded graphite, 2 parts of vulcanizer, 30 parts of white carbon black, 2 parts of coupling agent, 2 parts of zinc oxide, 1 part of stearic acid, and 1 part of structure regulator.

[0047] The difference from Example 1 is that the amount of expanded graphite is 3 parts, and no modified biochar is added.

[0048] Comparative Example 5

[0049] The present embodiment discloses a biochar synergistic flame retardant silicone rubber, which includes 100 parts of silicone rubber matrix, 5 parts of expanded graphite, 1 part of biochar, 2 parts of vulcanizer, 30 parts of white carbon black, 2 parts of coupling agent, 2 parts of zinc oxide, 1 part of stearic acid, and 1 part of structure regulator.

[0050] The difference from Example 1 is that the amount of expanded graphite is 3 parts and the amount of biochar is 1 part.

[0051] Comparative Example 6

[0052] The present embodiment discloses a biochar synergistic flame retardant silicone rubber, which includes 100 parts of silicone rubber matrix, 5 parts of expanded graphite, 2 parts of biochar, 2 parts of vulcanizer, 30 parts of white carbon black, 2 parts of coupling agent, 2 parts of zinc oxide, 1 part of stearic acid, and 1 part of structure regulator.

[0053] The difference from Example 1 is that the amount of expanded graphite is 5 parts and the amount of biochar is 2 parts.

[0054] Specifically, the oxygen index, vertical combustion effect and tensile strength of the above embodiments and comparative examples were tested, wherein the oxygen index and tensile strength were tested by corresponding instruments, and the specific steps of the vertical combustion test are as follows:

[0055] During the test, the flame height is 20±1mm, the Bunsen burner is placed at the center below the sample, the burner is 10±1mm away from the bottom of the sample, the ignition time is 10±0.5s, 10±0.5s after ignition, move the burner away at least 150mm at a speed of 300mm / sec, and start recording the afterflame time t1. When the afterflame stops, it should be ignited immediately for 10±0.5s, 10±0.5s after ignition, move the burner away at least 150mm at a speed of 300mm / sec, and record the afterflame time t2 and afterburning time t3. The flame level is evaluated as shown in Table 1 below:

[0056] Table 1

[0057]

[0058] The experimental comparison table of the comparative example and the embodiment is shown in Table 2 below:

[0059] Table 2

[0060]

[0061] As shown in Table 2 above, it can be seen from the comparison between Comparative Example 1 and Comparative Examples 2-4 that when only expanded graphite is added as a flame retardant filler, the expanded graphite fuel has a certain flame retardant effect on silicone rubber. Specifically, when no expanded graphite is added, the silicone rubber does not have a vertical combustion coefficient level. Among them, Comparative Examples 2-4 are silicone rubbers with 1 part of expanded graphite, 3 parts of expanded graphite and 5 parts of expanded graphite added respectively. Specifically, as the proportion of expanded graphite increases, the oxygen index in the properties of silicone rubber increases successively. The silicone rubber with 5 parts of expanded graphite has the highest oxygen index, that is, more oxygen is needed during combustion, so the oxygen inhibition effect is gradually improved, and the vertical combustion level is V-0. The silicone rubber with 3 parts of expanded graphite has better tensile strength, which is because too much expanded graphite filler is not conducive to the mechanical properties of silicone rubber. .

[0062] It can be seen from Comparative Examples 3 and 5 that when ordinary biochar is added to synergistically with expanded graphite for flame retardancy, the flame retardancy level of the vertical combustion of biochar silicone rubber is not improved, and the oxygen index is almost unchanged. The same is true for Comparative Examples 4 and 6. It can be seen that when ordinary biochar is added to synergistically with expanded graphite for flame retardancy, the flame retardant effect on silicone rubber is not obvious.

[0063] However, by comparing Comparative Example 5 with Example 1, the biochar added in Example 1 is modified with silicon nitride. After adding 1 part of modified biochar, the flame retardant grade of the silicone rubber in vertical combustion is improved from V-1 to V-0, and the oxygen index is also increased from 29% to 31.7%. In addition, it can be observed from the tensile strength that the tensile strength of the material is significantly improved after the modified biochar is added. Similarly, comparing Comparative Example 6 with Example 2, the oxygen index of the silicone rubber after adding 2 parts of modified biochar is significantly improved, and it is more difficult to burn; therefore, the modified biochar synergistic expanded graphite flame retardant silicone rubber system has better performance in oxygen index, vertical combustion and tensile strength. This is because the modified biochar is a combination of biochar and silicon nitride. The specific mechanism process is as follows Figure 2 As shown, the presence of silicon nitride improves the stability of the carbon layer structure formed on the outside of biochar, which can then work well with expanded graphite to exert a good flame retardant effect of silicone rubber.

[0064] In summary, the modified biochar prepared by the present invention can cooperate well with expanded graphite to improve the flame retardant properties.

[0065] So far, various embodiments of the present disclosure have been described in detail. In order to avoid obscuring the concept of the present disclosure, some details known in the art are not described. Based on the above description, those skilled in the art can fully understand how to implement the technical solution disclosed here.

[0066] Although some specific embodiments of the present disclosure have been described in detail by way of examples, it should be understood by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present disclosure. It should be understood by those skilled in the art that the above embodiments may be modified or some technical features may be replaced by equivalents without departing from the scope and spirit of the present disclosure. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there is no structural conflict.

Claims

1. A biochar-synergistic flame-retardant silicone rubber, characterized in that: include: The following parts by mass: 100 parts of silicone rubber matrix, 10-30 parts of white carbon black, 1-3 parts of structure regulator, 1-3 parts of coupling agent, 2-5 parts of zinc oxide, 1-2 parts of stearic acid, 1-3 parts of modified biochar filler, 1-5 parts of expandable graphite, and 1-2 parts of vulcanizing agent.

2. The biochar-synergistic flame-retardant silicone rubber according to claim 1, characterized in that: The silicone rubber matrix is ​​one of methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, fluorosilicone rubber and dimethyl silicone rubber.

3. The biochar-synergistic flame-retardant silicone rubber according to claim 1, characterized in that: The coupling agent is one of: γ-aminopropyltriethoxysilane, 3-(2,3-epoxypropyloxy)propyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, and γ-mercaptopropyltrimethoxysilane.

4. The biochar-synergistic flame-retardant silicone rubber according to claim 1, characterized in that: The vulcanizing agent is one of dicumyl peroxide, benzoyl peroxide and dipentadienyl vulcanizing agent.

5. The biochar-synergistic flame-retardant silicone rubber according to claim 1, characterized in that: The modified biochar filler is a composite system of biochar and silicon nitride.

6. The biochar-synergistic flame-retardant silicone rubber according to claim 5, characterized in that: The preparation method of the modified biochar filler is as follows: silicon nitride is placed in deionized water to prepare a silicon nitride suspension, the suspension is ultrasonically dispersed for 3 hours and then set aside, rice husks, wheat straws and other crop wastes are physically washed to remove impurities and dirt, placed in an 80°C drying oven for 24 hours, then crushed with a pulverizer, the crushed material is added to the silicon nitride suspension, magnetically stirred for 2 hours, then filtered and dried, the dried sample is placed in a tubular furnace, nitrogen is introduced at a flow rate of 15 ml / min, and the temperature is increased to 500°C at a heating rate of 5°C / min, pyrolyzed for 1 hour, and the sample is taken out after the tubular furnace is cooled, and the product is a silicon nitride biochar composite material.

7. The biochar-synergistic flame-retardant silicone rubber according to claim 6, characterized in that: The mass concentration of silicon nitride in the silicon nitride suspension is 1%.

8. The biochar-synergistic flame-retardant silicone rubber according to claim 5, characterized in that: The silicon nitride is hexagonal nano-scale silicon nitride with a purity greater than or equal to 99.9%, a particle size of 500 nm, and a hexagonal crystal shape.

9. A method for preparing biochar-synergistic flame-retardant silicone rubber, characterized in that: The method comprises the biochar-synergistic flame-retardant silicone rubber according to any one of claims 1 to 8, and the specific steps are as follows: S1, kneading the silicone rubber matrix in a two-roll mill, and then adding hydroxy silicone oil of white carbon black for mixing; S2, adding a coupling agent, modified biochar filler, expandable graphite, zinc oxide and stearic acid to the mixed material of S1 and continuing to mix to obtain a mixed rubber; S3, cooling the mixed rubber in S2 for 24 hours, adding a vulcanizing agent and continuing to mix to obtain a first rubber compound; S4, after the first rubber compound mixed in S3 is pressed into sheets, it is placed on a flat vulcanizer for heating and vulcanization, and then placed in an oven for two-stage vulcanization, and finally the biochar material synergistic flame retardant silicone rubber is obtained.

10. The method for preparing biochar-synergistic flame-retardant silicone rubber according to claim 9, characterized in that: The temperature of the vulcanizer heating vulcanization is 160℃, the time is 30min, and the pressure is 8-10MPa; the temperature of the secondary vulcanization is 200℃, and the time is 4h.