Preparation method and application of conductive carbon black
By surface activation and grafting the carbon black, modified conductive carbon black was prepared for the positive electrode sheet of lithium-ion battery, which solved the problems of insufficient conductivity and manganese element migration, and significantly improved the circulation performance of lithium-ion battery .
Patent Information
- Application Number
- CN202411177717.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
AI Technical Summary
The conductive carbon black in existing lithium-ion batteries is insufficient, and the manganese element is dissolved in the positive electrode active material layer and migrates to the negative electrode surface to form an SEI film, affecting the cycling performance of the battery.
Modified conductive carbon black is prepared by surface activation of the carbon black raw material and grafting reaction with 1-aza-12-crown 4-ether, which is used in the positive electrode sheet of lithium-ion battery to prevent the migration of manganese elements to Negative electrode surface.
Modified conductive carbon black not only improves the conductivity, but also effectively captures the manganese element in the positive electrode active material layer, improves the circulation performance of the positive electrode of the lithium-ion battery and extends the battery's service life.
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of carbon materials, and in particular to a preparation method of conductive carbon black and application thereof. Background Art
[0002] Lithium ion secondary batteries are widely used as power sources for small electronic devices such as smartphones and tablet computers. Lithium ion secondary batteries are generally composed of electrodes, separators, and electrolytes. For electrodes, composite material slurry obtained by dispersing active materials, conductive agents, adhesives, etc. in a dispersion medium is applied to a metal plate for a current collector and dried to form a composite material layer for manufacturing.
[0003] Carbon black (CB) is one of the most commonly used black inorganic pigments, generally referring to aggregates with primary particle sizes of 10-400nm. Carbon black particles are statistical combinations of carbon layers, arranged in concentric graphite layers, and different types of carbon black only have different degrees of order. Carbon black is obtained by incomplete combustion or thermal decomposition of carbon-containing materials (coal, natural gas, heavy oil, fuel oil, etc.) under insufficient air conditions. The carbon, hydrogen, sulfur and ash contained in the raw materials react with oxygen in the surrounding air to generate a large number of acidic oxygen-containing groups on their surfaces, such as hydroxyl and carboxyl groups.
[0004] The conductivity of conductive carbon black is affected by factors such as its specific surface area, porosity, structural degree, surface composition and microstructure; therefore, by improving the preparation process, conductive carbon black with better conductive properties can be obtained. Summary of the invention
[0005] The present invention provides a preparation method of conductive carbon black and application thereof to solve the deficiencies in the related art.
[0006] According to a first aspect of an embodiment of the present disclosure, a method for preparing conductive carbon black is provided, the preparation method comprising the following steps:
[0007] Step 1: providing a carbon black raw material, and activating the surface of the carbon black raw material to obtain surface-activated carbon black;
[0008] Step 2: grafting the surface activated carbon black with 1-aza-12-crown-4-ether to obtain the modified carbon black.
[0009] In one aspect of the disclosed embodiments, the surface activated carbon black is prepared by following steps 1-A:
[0010] Step 1-A1: adding the carbon black raw material to a 15%-35% nitric acid solution, stirring at 50° C.-65° C. for 2-5 hours; obtaining nitric acid-treated carbon black;
[0011] Step 1-A2: Then add the carbon black treated with nitric acid into a dichloromethane solution, and under an inert gas atmosphere, dropwise add thionyl chloride with stirring. After the dropwise addition is completed, continue stirring for 0.5-2h, and obtain the surface-activated carbon black after washing and drying.
[0012] In one aspect of the disclosed embodiments, the surface activated carbon black is prepared by following steps 1-B:
[0013] Step 1-B1: dissolving ammonium persulfate in water to prepare an ammonium persulfate solution having a mass percentage of 1% to 3%;
[0014] Step 1-B2: Add the carbon black raw material to the ammonium persulfate solution, stir at room temperature for 1-3 hours, then continue stirring at 55° C.-75° C. for 3-6 hours, and obtain the surface-activated carbon black after washing and drying.
[0015] In one aspect of the embodiments of the present disclosure, the mass ratio of the surface activated carbon black to the 1-aza-12-crown 4-ether is selected from (20-50):1.
[0016] In one aspect of the disclosed embodiment, step 2 comprises: dissolving the 1-aza-12-crown-4-ether in a methanol solution, stirring for 0.5-2 hours, then adding the surface-activated carbon black thereto, reacting at 45°C-60°C for 2-5 hours, and then cooling, filtering, washing and drying to obtain the conductive carbon black.
[0017] In one aspect of the embodiments of the present disclosure, when the surface activated carbon black is prepared by step 1-A, step 2 is performed under an inert gas atmosphere.
[0018] In one aspect of the embodiments of the present disclosure, the aforementioned inert gases are all nitrogen.
[0019] According to a second aspect of an embodiment of the present disclosure, a conductive carbon black is provided, wherein the conductive carbon black is obtained by the aforementioned preparation method.
[0020] According to a third aspect of an embodiment of the present disclosure, a lithium-ion battery positive electrode plate is provided, the lithium-ion battery positive electrode plate comprising: a positive electrode current collector, a positive electrode active material layer disposed on the positive electrode current collector, the positive electrode active material layer comprising a positive electrode active material and the aforementioned conductive carbon black; the positive electrode active material comprising manganese element.
[0021] In one aspect of the embodiments of the present disclosure, the positive electrode active material is selected from lithium manganese iron phosphate.
[0022] According to a fourth aspect of the embodiments of the present disclosure, a lithium-ion battery is provided, wherein the lithium-ion battery comprises the aforementioned lithium-ion battery positive electrode plate; the lithium-ion battery also comprises a lithium battery negative electrode plate, a separator and an electrolyte.
[0023] The technical solution provided by the embodiments of the present disclosure may have the following beneficial effects:
[0024] It can be seen from the above embodiments that the present disclosure provides a conductive carbon black for use in the positive electrode plate of a manganese-containing lithium-ion battery, which can not only serve as a conductive agent material, but the 1-aza-12-crown-4-ether grafted on its surface can also effectively capture the manganese element dissolved in the positive electrode active material layer, preventing the manganese element from migrating to the negative electrode surface to form an SEI film, thereby improving the cycle performance of the positive electrode of the manganese-containing lithium-ion battery.
[0025] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. DETAILED DESCRIPTION
[0026] Here, exemplary embodiments will be described in detail, and the implementations described in the following exemplary embodiments do not represent all implementations consistent with the present disclosure.
[0027] The terms used in this disclosure are for the purpose of describing specific embodiments only and are not intended to limit the disclosure. The singular forms of "a", "said" and "the" used in this disclosure and the appended claims are also intended to include plural forms unless the context clearly indicates otherwise. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.
[0028] It should be understood that although the terms first, second, third, etc. may be used in the present disclosure to describe various information, such information should not be limited to these terms. These terms are only used to distinguish the same type of information from each other.
[0029] A list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single component or multiple components. Item B may contain a single component or multiple components. Item C may contain a single component or multiple components.
[0030] The present disclosure is further described below in conjunction with specific embodiments. It should be understood that these specific embodiments are only used to illustrate the present disclosure and are not used to limit the scope of the present disclosure.
[0031] Positive electrode:
[0032] The positive electrode sheet disclosed in the present invention comprises a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector; the positive electrode active material layer comprises a positive electrode active material, conductive carbon black and a binder.
[0033] In some embodiments of the present disclosure, the positive electrode current collector may be aluminum; specifically, the positive electrode current collector may be aluminum foil or carbon-coated aluminum foil, but is not limited thereto.
[0034] In some embodiments of the present disclosure, the positive electrode current collector can be arbitrarily selected according to actual needs; specifically, the thickness of the aluminum foil layer of the carbon-coated aluminum foil can be selected from 10-13 μm, and the thickness of the carbon coating layer can be selected from 1-2 μm, but is not limited thereto. Specifically, the thickness of the aluminum foil layer of the carbon-coated aluminum foil is 13 μm, and a 1 μm carbon layer is coated on both sides.
[0035] In some embodiments of the present disclosure, the positive electrode active material used in the present disclosure is a manganese-rich positive electrode active material.
[0036] In some embodiments of the present disclosure, the manganese-rich positive electrode active material can be selected from any positive electrode material containing manganese. Optionally, the positive electrode active material can be selected from lithium manganese iron phosphate, LiMn2O4, LiCo 1-y Mn y O2、LiNi 1-y Mn y O2、LiMn 2- y M y O4、LiNi x Co y Mn z M 1-x-y-z O2; wherein 0≤y≤1, 0≤x≤1, 0≤z≤1, x+y+z≤1; M is selected from one of Fe, Co, Ni, Mn, Mg, Cu, Zn, Al, Sn, B, Ga, Cr, Sr, V or Ti. Preferably, the manganese-rich positive electrode active material is selected from lithium manganese iron phosphate.
[0037] In some embodiments of the present disclosure, the conductive carbon black used in the present disclosure can be prepared by the following steps:
[0038] Step 1-A1: adding the carbon black raw material to a 15%-35% nitric acid solution, stirring at 50° C.-65° C. for 2-5 hours; obtaining nitric acid-treated carbon black;
[0039] Step 1-A2: then adding the carbon black treated with nitric acid to a dichloromethane solution, and under an inert gas atmosphere, adding thionyl chloride dropwise with stirring, and continuing stirring for 0.5-2h after the addition is complete, and washing and drying to obtain the surface-activated carbon black;
[0040] Step 2: Dissolve the 1-aza-12-crown-4-ether in a methanol solution, stir for 0.5-2 hours under an inert gas atmosphere, then add the surface-activated carbon black, react at 45°C-60°C for 2-5 hours, and then cool, filter, wash and dry to obtain the conductive carbon black.
[0041] In some embodiments of the present disclosure, the conductive carbon black used in the present disclosure can also be prepared by the following steps:
[0042] Step 1-B1: dissolving ammonium persulfate in water to prepare an ammonium persulfate solution having a mass percentage of 1% to 3%;
[0043] Step 1-B2: adding the carbon black raw material to the ammonium persulfate solution, stirring at room temperature for 1-3 hours, and then continuing to stir at 55° C.-75° C. for 3-6 hours, washing and drying to obtain the surface-activated carbon black;
[0044] Step 2: dissolving the 1-aza-12-crown-4-ether in a methanol solution, stirring for 0.5-2 hours, then adding the surface-activated carbon black thereto, reacting at 45°C-60°C for 2-5 hours, and then cooling, filtering, washing and drying to obtain the conductive carbon black.
[0045] In the present disclosure, the carbon black raw material is selected from any one of carbon black N134, carbon black N110, carbon black N134, carbon black N121, carbon black N166, carbon black N219, carbon black N220, carbon black N231, carbon black N234, carbon black N242, carbon black N270, carbon black N285, carbon black N293, carbon black N294, carbon black N299, carbon black N326, carbon black N330, carbon black N332, carbon black N339, carbon black N347, carbon black N351, carbon black N356, carbon black N358, carbon black N363 or carbon black N375; preferably, the carbon black raw material used in the present disclosure is selected from carbon black N134.
[0046] In some embodiments of the present disclosure, non-limiting examples of binders include polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, and the like.
[0047] Negative electrode:
[0048] In some embodiments of the present disclosure, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector.
[0049] In the present disclosure, the specific types of negative electrode active materials are not subject to specific restrictions and can be selected according to needs. Specifically, the negative electrode active material is selected from one or more of natural graphite, artificial graphite, mesophase microcarbon beads (referred to as MCMB), hard carbon, soft carbon, silicon, silicon-carbon composites, Li-Sn alloys, Li-Sn-O alloys, Sn, SnO, SnO2, spinel-structured lithiated TiO2-Li4Ti5O12, and Li-Al alloys. Non-limiting examples of carbon materials include crystalline carbon, amorphous carbon, and mixtures thereof. Crystalline carbon can be amorphous or flaky, flake-shaped, spherical or fibrous natural graphite or artificial graphite. Amorphous carbon can be soft carbon, hard carbon, mesophase pitch carbide, calcined coke, etc.
[0050] In some embodiments of the present disclosure, the negative electrode active material layer may include a binder; the binder improves the bonding between negative electrode active material particles and the bonding between the negative electrode active material and the current collector.
[0051] In some embodiments of the present disclosure, non-limiting examples of binders include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc.
[0052] In some embodiments of the present disclosure, the negative electrode active material layer includes a conductive agent so that the electrode has conductivity. The conductive agent may include any conductive material as long as it does not cause chemical changes. Non-limiting examples of conductive materials include carbon-based materials (e.g., natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.), metal-based materials (e.g., metal powder, metal fiber, etc., such as copper, nickel, aluminum, silver, etc.), conductive polymers (e.g., polyphenylene derivatives) and mixtures thereof.
[0053] In some embodiments of the present disclosure, the negative electrode sheet of the present disclosure includes a negative electrode active material, a binder and a conductive agent.
[0054] In some embodiments of the present disclosure, the negative electrode active material of the present disclosure may also be selected from other materials that can electrochemically absorb and release metal ions such as lithium ions. Specifically, it can be selected from carbonaceous materials, silicon materials, alloy materials, lithium-containing metal oxide materials, etc. They can be used alone or in any combination of two or more.
[0055] In some embodiments of the present disclosure, the negative electrode current collector may be selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.
[0056] Electrolyte:
[0057] In some embodiments of the present disclosure, the electrolyte includes a lithium salt and a solvent.
[0058] In some embodiments of the present disclosure, the lithium salt includes at least one of an organic lithium salt or an inorganic lithium salt. In some embodiments, the lithium salt includes, but is not limited to: lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium bis(trifluoromethanesulfonyl)imide LiN(CF3SO2)2 (LiTFSI), lithium bis(fluorosulfonyl)imide Li(N(SO2F)2) (LiFSI), lithium bis(oxalatoborate) LiB(C2O4)2 (LiBOB) or lithium di(oxalatoborate) LiBF2(C2O4) (LiDFOB).
[0059] In some embodiments of the present disclosure, the solvent can be selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), cyclopentane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).
[0060] Diaphragm:
[0061] In some embodiments of the present disclosure, a lithium-ion secondary battery is provided with a separator between the positive electrode plate and the negative electrode plate to prevent short circuit. The material and shape of the separator used in the secondary battery are not particularly limited, and it can be any technology disclosed in the prior art.
[0062] In some embodiments of the present disclosure, the diaphragm may include a substrate layer and a surface treatment layer. The substrate layer is a non-woven fabric, a film or a composite film having a porous structure, and the material of the substrate layer is selected from at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. Specifically, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film can be selected. A surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer can be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. The inorganic layer includes inorganic particles and a binder, and the inorganic particles are selected from one or more combinations of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide and barium sulfate. The binder is selected from one or a combination of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene and polyhexafluoropropylene. The polymer layer contains a polymer, and the material of the polymer is selected from at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride and poly(vinylidene fluoride-hexafluoropropylene).
[0063] Lithium-ion battery:
[0064] In some embodiments of the present disclosure, the lithium-ion battery involved in the present disclosure can be made by stacking the above-mentioned positive and negative electrode sheets.
[0065] In some embodiments of the present disclosure, the lithium-ion battery involved in the present disclosure may include an outer packaging, and the outer packaging may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the lithium-ion battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.
[0066] In some embodiments of the present disclosure, the present disclosure further provides a battery module. The battery module includes the above-mentioned lithium-ion secondary battery. The battery module uses the above-mentioned lithium-ion battery, and therefore has at least the same advantages as the above-mentioned lithium-ion secondary battery. The number of lithium-ion secondary batteries contained in the battery module can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module.
[0067] In some embodiments of the present disclosure, the present disclosure further provides a battery pack, which includes the above-mentioned battery module. The number of battery modules included in the battery pack can be adjusted according to the application and capacity of the battery pack.
[0068] The present disclosure is further described below in conjunction with the examples. It should be understood that these examples are only used to illustrate the present disclosure and are not used to limit the scope of the present disclosure.
[0069] Example
[0070] Embodiment 1:
[0071] Embodiment 1 comprises the following steps:
[0072] 1. Preparation of conductive carbon black:
[0073] 10g of carbon black N134 was added to a 20% dilute nitric acid solution and stirred at 60°C for 3h to obtain carbon black treated with nitric acid; the carbon black treated with nitric acid was washed with deionized water and then dried; then the carbon black treated with nitric acid was added to 25mL of dichloromethane solution, and 8mL of thionyl chloride was slowly added dropwise under a nitrogen atmosphere at a stirring speed of 500r / min. After the addition was completed, stirring was continued for 1h, and the carbon black was washed with deionized water and then dried to obtain surface-activated carbon black;
[0074] 360 μL of 1-aza-12-crown 4-ether (0.4 g) was dissolved in a methanol solution and stirred for 1 h. Then, surface-activated carbon black was added thereto and reacted at 55° C. for 4 h. Then, the conductive carbon black of Example 1 was obtained by cooling, vacuum filtration, deionized water washing and drying.
[0075] 2. Preparation of positive electrode sheet:
[0076] The lithium iron manganese phosphate powder, the binder PVDF, the conductive carbon black prepared above and the solvent N-methylpyrrolidone are uniformly mixed to prepare a positive electrode slurry, wherein, based on the total mass of the positive electrode slurry, the mass percentage of lithium iron manganese phosphate is 95%, the mass percentage of PVDF is 2.5%, and the mass percentage of the conductive carbon black prepared above is 2.5%; the obtained positive electrode slurry is uniformly coated on the surface of the positive electrode collector, the positive electrode collector is a carbon-coated aluminum foil with a thickness of 15 μm, and is dried in a coating oven at a drying temperature of 95°C to obtain a positive electrode collector coated with a positive electrode active material layer, and the surface density of the positive electrode active material layer is selected from 25 mg / cm 2 ; The positive electrode current collector coated with the positive electrode active material layer is cold pressed by a roller press to obtain the positive electrode sheet of Example 1.
[0077] 3. Preparation of lithium-ion batteries:
[0078] The obtained positive electrode sheet is assembled with a graphite negative electrode sheet, a PE separator, a lithium hexafluorophosphate electrolyte, and a battery shell into a lithium-ion battery.
[0079] Embodiment 2:
[0080] Embodiment 2 comprises the following steps:
[0081] 1. Preparation of conductive carbon black:
[0082] 10g of carbon black N134 was added to a 40% dilute nitric acid solution and stirred at 60°C for 3h to obtain carbon black treated with nitric acid; the carbon black treated with nitric acid was washed with deionized water and then dried; then the carbon black treated with nitric acid was added to 25mL of dichloromethane solution, and 12mL of thionyl chloride was slowly added dropwise under a nitrogen atmosphere and stirred at 500r / min. After the addition was completed, stirring was continued for 1h, and the carbon black was washed with deionized water and then dried to obtain surface-activated carbon black;
[0083] 360 μL of 1-aza-12-crown 4-ether (0.4 g) was dissolved in a methanol solution and stirred for 1 h. Then, surface-activated carbon black was added thereto and reacted at 55° C. for 4 h. Then, the conductive carbon black of Example 2 was obtained by cooling, vacuum filtration, deionized water washing and drying.
[0084] 2. Preparation of positive electrode sheet:
[0085] The lithium iron manganese phosphate powder, the binder PVDF, the conductive carbon black prepared above and the solvent N-methylpyrrolidone are uniformly mixed to prepare a positive electrode slurry, wherein, based on the total mass of the positive electrode slurry, the mass percentage of lithium iron manganese phosphate is 95%, the mass percentage of PVDF is 2.5%, and the mass percentage of the conductive carbon black prepared above is 2.5%; the obtained positive electrode slurry is uniformly coated on the surface of the positive electrode collector, the positive electrode collector is a carbon-coated aluminum foil with a thickness of 15 μm, and is dried in a coating oven at a drying temperature of 95°C to obtain a positive electrode collector coated with a positive electrode active material layer, and the surface density of the positive electrode active material layer is selected from 25 mg / cm 2 ; The positive electrode current collector coated with the positive electrode active material layer is cold pressed by a roller press to obtain the positive electrode sheet of Example 2.
[0086] 3. Preparation of lithium-ion batteries:
[0087] The obtained positive electrode sheet is assembled with a graphite negative electrode sheet, a PE separator, a lithium hexafluorophosphate electrolyte, and a battery shell into a lithium-ion battery.
[0088] Embodiment 3:
[0089] Embodiment 3 comprises the following steps:
[0090] 1. Preparation of conductive carbon black:
[0091] Prepare an ammonium persulfate solution with a mass percentage of 2.5%; add 10g of carbon black N134 to the ammonium persulfate solution, stir at room temperature for 2h, then continue stirring at 60°C for 4h, wash with deionized water and dry to obtain surface-activated carbon black;
[0092] 360 μL of 1-aza-12-crown 4-ether (0.4 g) was dissolved in a methanol solution and stirred for 1 h. Then, surface-activated carbon black was added thereto and reacted at 55° C. for 4 h. Then, the conductive carbon black of Example 3 was obtained by cooling, vacuum filtration, deionized water washing and drying.
[0093] 2. Preparation of positive electrode sheet:
[0094] The lithium iron manganese phosphate powder, the binder PVDF, the conductive carbon black prepared above and the solvent N-methylpyrrolidone are uniformly mixed to prepare a positive electrode slurry, wherein, based on the total mass of the positive electrode slurry, the mass percentage of lithium iron manganese phosphate is 95%, the mass percentage of PVDF is 2.5%, and the mass percentage of the conductive carbon black prepared above is 2.5%; the obtained positive electrode slurry is uniformly coated on the surface of the positive electrode collector, the positive electrode collector is a carbon-coated aluminum foil with a thickness of 15 μm, and is dried in a coating oven at a drying temperature of 95°C to obtain a positive electrode collector coated with a positive electrode active material layer, and the surface density of the positive electrode active material layer is selected from 25 mg / cm 2 ; The positive electrode current collector coated with the positive electrode active material layer is cold pressed by a roller press to obtain the positive electrode sheet of Example 3.
[0095] 3. Preparation of lithium-ion batteries:
[0096] The obtained positive electrode sheet is assembled with a graphite negative electrode sheet, a PE separator, a lithium hexafluorophosphate electrolyte, and a battery shell into a lithium-ion battery.
[0097] Embodiment 4:
[0098] Embodiment 4 comprises the following steps:
[0099] 1. Preparation of conductive carbon black:
[0100] Prepare an ammonium persulfate solution with a mass percentage of 0.5%; add 10g of carbon black N134 to the ammonium persulfate solution, stir at room temperature for 2h, then continue to stir at 60°C for 4h, wash with deionized water and dry to obtain surface-activated carbon black;
[0101] 360 μL of 1-aza-12-crown 4-ether (0.4 g) was dissolved in a methanol solution and stirred for 1 h. Then, surface-activated carbon black was added thereto and reacted at 55° C. for 4 h. Then, the conductive carbon black of Example 4 was obtained by cooling, vacuum filtration, deionized water washing and drying.
[0102] 2. Preparation of positive electrode sheet:
[0103] The lithium iron manganese phosphate powder, the binder PVDF, the conductive carbon black prepared above and the solvent N-methylpyrrolidone are uniformly mixed to prepare a positive electrode slurry, wherein, based on the total mass of the positive electrode slurry, the mass percentage of lithium iron manganese phosphate is 95%, the mass percentage of PVDF is 2.5%, and the mass percentage of the conductive carbon black prepared above is 2.5%; the obtained positive electrode slurry is uniformly coated on the surface of the positive electrode collector, the positive electrode collector is a carbon-coated aluminum foil with a thickness of 15 μm, and is dried in a coating oven at a drying temperature of 95°C to obtain a positive electrode collector coated with a positive electrode active material layer, and the surface density of the positive electrode active material layer is selected from 25 mg / cm 2 ; The positive electrode current collector coated with the positive electrode active material layer is cold pressed by a roller press to obtain the positive electrode sheet of Example 4.
[0104] 3. Preparation of lithium-ion batteries:
[0105] The obtained positive electrode sheet is assembled with a graphite negative electrode sheet, a PE separator, a lithium hexafluorophosphate electrolyte, and a battery shell into a lithium-ion battery.
[0106] Embodiment 5:
[0107] Embodiment 5 comprises the following steps:
[0108] 1. Preparation of conductive carbon black:
[0109] Prepare a 5% ammonium persulfate solution; add 10 g of carbon black N134 to the ammonium persulfate solution, stir at room temperature for 2 hours, then continue stirring at 60° C. for 4 hours, wash with deionized water and dry to obtain surface-activated carbon black;
[0110] 360 μL of 1-aza-12-crown 4-ether (0.4 g) was dissolved in a methanol solution and stirred for 1 h. Then, surface-activated carbon black was added thereto and reacted at 55° C. for 4 h. Then, the conductive carbon black of Example 5 was obtained by cooling, vacuum filtration, deionized water washing and drying.
[0111] 2. Preparation of positive electrode sheet:
[0112] The lithium iron manganese phosphate powder, the binder PVDF, the conductive carbon black prepared above and the solvent N-methylpyrrolidone are uniformly mixed to prepare a positive electrode slurry, wherein, based on the total mass of the positive electrode slurry, the mass percentage of lithium iron manganese phosphate is 95%, the mass percentage of PVDF is 2.5%, and the mass percentage of the conductive carbon black prepared above is 2.5%; the obtained positive electrode slurry is uniformly coated on the surface of the positive electrode collector, the positive electrode collector is a carbon-coated aluminum foil with a thickness of 15 μm, and is dried in a coating oven at a drying temperature of 95°C to obtain a positive electrode collector coated with a positive electrode active material layer, and the surface density of the positive electrode active material layer is selected from 25 mg / cm 2 ; The positive electrode current collector coated with the positive electrode active material layer is cold pressed by a roller press to obtain the positive electrode sheet of Example 5.
[0113] 3. Preparation of lithium-ion batteries:
[0114] The obtained positive electrode sheet is assembled with a graphite negative electrode sheet, a PE separator, a lithium hexafluorophosphate electrolyte, and a battery shell into a lithium-ion battery.
[0115] Comparative Example 1:
[0116] Comparative Example 1 comprises the following steps:
[0117] 1. Preparation of positive electrode sheet:
[0118] The lithium iron manganese phosphate powder, the binder PVDF, the carbon black N134 and the solvent N-methylpyrrolidone are uniformly mixed to prepare a positive electrode slurry, wherein, based on the total mass of the positive electrode slurry, the mass percentage of lithium iron manganese phosphate is 95%, the mass percentage of PVDF is 2.5%, and the mass percentage of carbon black N134 is 2.5%; the obtained positive electrode slurry is uniformly coated on the surface of the positive electrode collector, the positive electrode collector is a carbon-coated aluminum foil with a thickness of 15 μm, and is dried in a coating oven at a drying temperature of 95°C to obtain a positive electrode collector coated with a positive electrode active material layer, and the surface density of the positive electrode active material layer is selected from 25 mg / cm 2 ; The positive electrode current collector coated with the positive electrode active material layer was cold pressed by a roller press to obtain the positive electrode sheet of Comparative Example 1.
[0119] 2. Preparation of lithium-ion batteries:
[0120] The obtained positive electrode sheet is assembled with a graphite negative electrode sheet, a PE separator, a lithium hexafluorophosphate electrolyte, and a battery shell into a lithium-ion battery.
[0121] Comparative Example 2:
[0122] Comparative Example 2 comprises the following steps:
[0123] 1. Preparation of conductive carbon black:
[0124] 360 μL of 1-aza-12-crown 4-ether (0.4 g) was dissolved in a methanol solution and stirred for 1 h. Unactivated carbon black N134 was then added thereto. The mixture was reacted at 55° C. for 4 h. The mixture was then cooled, vacuum filtered, washed with deionized water and dried to obtain the conductive carbon black of Comparative Example 2.
[0125] 2. Preparation of positive electrode sheet:
[0126] The lithium iron manganese phosphate powder, the binder PVDF, the conductive carbon black prepared above and the solvent N-methylpyrrolidone are uniformly mixed to prepare a positive electrode slurry, wherein, based on the total mass of the positive electrode slurry, the mass percentage of lithium iron manganese phosphate is 95%, the mass percentage of PVDF is 2.5%, and the mass percentage of the conductive carbon black prepared above is 2.5%; the obtained positive electrode slurry is uniformly coated on the surface of the positive electrode collector, the positive electrode collector is a carbon-coated aluminum foil with a thickness of 15 μm, and is dried in a coating oven at a drying temperature of 95°C to obtain a positive electrode collector coated with a positive electrode active material layer, and the surface density of the positive electrode active material layer is selected from 25 mg / cm 2 ; The positive electrode current collector coated with the positive electrode active material layer was cold pressed by a roller press to obtain the positive electrode sheet of Comparative Example 2.
[0127] 3. Preparation of lithium-ion batteries:
[0128] The obtained positive electrode sheet is assembled with a graphite negative electrode sheet, a PE separator, a lithium hexafluorophosphate electrolyte, and a battery shell into a lithium-ion battery.
[0129] Electrochemical testing:
[0130] Electrochemical tests were performed on Examples 1 to 5, and Comparative Examples 1 and 2, and the results are shown in Table 1. The electrochemical test method is as follows:
[0131] Cycle capacity retention rate test: At 25°C, charge the lithium-ion battery to 4.5V at 0.7C, and charge to 0.05C at 4.5V. Then discharge to 3.0V at 0.7C, and cycle 200 times at 0.7C charge and 1C discharge. The discharge capacity at the third cycle is used as the benchmark, and the capacity retention rate is used as an indicator to evaluate the cycle performance of lithium-ion batteries.
[0132] Cycle capacity retention rate = discharge capacity at the 200th cycle / discharge capacity at the 3rd cycle×100%.
[0133] Test of discharge rate capacity retention rate: At 25℃, the lithium-ion battery is charged to 4.5V at 0.5C, and charged to 0.025C at constant voltage at 4.5V. Then it is discharged to 3.0V at 0.2C, and the discharge capacity is D0. Then the lithium-ion battery is charged to 4.5V at 0.5C, and charged to 0.025C at constant voltage at 4.5V. Then it is discharged to 3.0V at 5C, and the discharge capacity is D1.
[0134] Discharge rate capacity retention rate = D1 / D0×100%.
[0135] Table 1
[0136] Example Cycle capacity retention rate Discharge rate capacity retention rate Example 1 200 weeks 86.3% 91.2% Comparative Example 2 200 weeks 84.5% 87.3% Example 3 200 weeks 95.6% 96.9% Comparative Example 4 200 weeks 89.3% 92.5% Example 5 200 weeks 92.3% 93.0% Comparative Example 1 200 weeks 70.8% 68.3% Comparative Example 2 200 weeks 80.6% 82.6%
[0137] It can be seen that the present disclosure grafts 1-aza-12-crown-4-ether having the function of inhibiting the dissolution of manganese element with conductive carbon black, and the modified conductive carbon black can be used as a conductive agent material, and can also prevent the manganese element from migrating to the surface of the negative electrode to form an SEI film, thereby improving the cycle performance of the positive electrode of the manganese-containing lithium ion battery; by comparing Examples 1-5 and Comparative Example 2, it can be seen that the carbon black that has not been surface activated cannot be well combined with 1-aza-12-crown-4-ether; its improvement in the cycle performance of the positive electrode of the manganese-containing lithium ion battery is relatively limited; and by comparing Examples 1-2 and Examples 3-5, it can be seen that the carbon black modified for surface activity using ammonium persulfate solution (i.e., step 1-B) has better combination with 1-aza-12-crown-4-ether than the carbon black modified for surface activity using nitric acid and thionyl chloride (i.e., step 1-A).
[0138] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the disclosure disclosed herein. The present disclosure is intended to cover any variations, uses or adaptations of the present disclosure, which follow the general principles of the present disclosure and include common knowledge or customary technical means in the art that are not disclosed in the present disclosure, and the description and examples are only considered to be exemplary.
Claims
1. A method for preparing conductive carbon black, characterized in that: The preparation method comprises the following steps: Step 1: providing a carbon black raw material, and activating the surface of the carbon black raw material to obtain surface-activated carbon black; Step 2: grafting the surface activated carbon black with 1-aza-12-crown-4-ether to obtain the modified carbon black.
2. The preparation method according to claim 1, characterized in that: The surface activated carbon black is prepared by the following steps 1-A: Step 1-A1: adding the carbon black raw material to a 15%-35% nitric acid solution, stirring at 50° C.-65° C. for 2-5 hours; obtaining nitric acid-treated carbon black; Step 1-A2: Then add the carbon black treated with nitric acid into a dichloromethane solution, and under an inert gas atmosphere, dropwise add thionyl chloride with stirring. After the dropwise addition is completed, continue stirring for 0.5-2h, and obtain the surface-activated carbon black after washing and drying.
3. The preparation method according to claim 1, characterized in that: The surface activated carbon black is prepared by the following steps 1-B: Step 1-B1: dissolving ammonium persulfate in water to prepare an ammonium persulfate solution having a mass percentage of 1% to 3%; Step 1-B2: Add the carbon black raw material to the ammonium persulfate solution, stir at room temperature for 1-3 hours, then continue stirring at 55° C.-75° C. for 3-6 hours, and obtain the surface-activated carbon black after washing and drying.
4. The preparation method according to claim 1, characterized in that: The mass ratio of the surface activated carbon black to the 1-aza-12-crown-4-ether is selected from (20-50):
1.
5. The preparation method according to claim 1, characterized in that: Step 2 comprises: dissolving the 1-aza-12-crown-4-ether in a methanol solution, stirring for 0.5-2 hours, then adding the surface activated carbon black thereto, reacting at 45°C-60°C for 2-5 hours, and then cooling, filtering, washing and drying to obtain the conductive carbon black.
6. The preparation method according to claim 1 or 2, characterized in that: When the surface activated carbon black is prepared through step 1-A, step 2 is carried out under an inert gas atmosphere.
7. A conductive carbon black, characterized in that The conductive carbon black is obtained by the preparation method according to any one of claims 1 to 6.
8. A positive electrode plate for a lithium-ion battery, characterized in that: The positive electrode plate of the lithium-ion battery comprises: a positive electrode current collector, a positive electrode active material layer disposed on the positive electrode current collector, the positive electrode active material layer comprising a positive electrode active material and the conductive carbon black according to claim 7; the positive electrode active material comprises manganese element.
9. The positive electrode sheet of a lithium-ion battery according to claim 8, characterized in that: The positive electrode active material is selected from lithium manganese iron phosphate.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the lithium-ion battery positive electrode plate according to claim 8 or 9; the lithium-ion battery also comprises a lithium-ion battery negative electrode plate, a separator and an electrolyte.