Modified assistant crosslinker, packaging adhesive film and photovoltaic module

By grafting the modified crosslinking agent of isocyanate groups on the surface of nano-oxide particles, combining ethylene-vinyl acetate copolymer and polyolefin elastomer, an ultraviolet-resistant packaging film is formed, which solves the poor UV resistance performance of the packaging material. The problems that are prone to precipitation of additives have significantly extended the life of photovoltaic modules.

CN119039901APending Publication Date: 2024-11-29FIRST (CHUZHOU) NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411387248.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing photovoltaic module packaging materials have poor UV resistance during long-term use, and additives are easy to precipitate, resulting in reduced power generation efficiency and shortened life of photovoltaic modules.

Method used

The modified crosslinking agent with isocyanate groups grafted on the surface of nano-oxide particles was used. There was a vibration peak in the range of 1640-1700cm-1 through the FTIR test. The modified crosslinking agent accounted for 0.5-15% of the weight of the matrix resin. , combined with ethylene-vinyl acetate copolymer and polyolefin elastomer, silane coupling agent, antioxidant and ultraviolet absorber are added to form an ultraviolet-resistant encapsulation film.

Benefits of technology

It significantly improves the UV resistance of the encapsulated adhesive film, reduces additive precipitation, extends the service life of photovoltaic modules, and maintains good mechanical properties and light transmittance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039901A_ABST
    Figure CN119039901A_ABST
Patent Text Reader

Abstract

The invention provides a modified assistant crosslinker, a packaging adhesive film and a photovoltaic module. The modified assistant crosslinker comprises a nano oxide and an isocyanate group grafted on the surface of the nano oxide; the grafting rate of an isocyanate group of the modified assistant crosslinker on the surface of the nano oxide is 5-20%; and the modified assistant crosslinking agent has a vibration peak in the range of 1640-1700cm <-1 > through FTIR (Fourier Transform Infrared Spectroscopy) test. According to the invention, the surfaces of the nano oxide particles are modified with isocyanate groups, so that the nano oxide particles have an assistant crosslinking effect, and the problem of precipitation of an assistant crosslinking agent in a storage process is solved. Meanwhile, due to the addition of the nano oxide particles, the adhesive film further has an excellent ultraviolet-resistant effect. The modified assistant crosslinker has the characteristics of low precipitation and ultraviolet resistance, and ensures the long-acting stability of a photovoltaic module.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of photovoltaic technology, and in particular to a modified co-crosslinking agent, a packaging adhesive film and a photovoltaic module. Background Art

[0002] In recent years, solar cells, as one of the representatives of clean energy, have received a lot of attention, and the installed capacity has continued to rise. With the continuous changes in solar cell technology, the research on related packaging materials and technologies has also received more and more attention from researchers. Packaging film is one of the key auxiliary materials for solar cell modules, which can isolate the modules from corrosion by water, oxygen, etc., and provide mechanical support. Among them, the film with ethylene-vinyl acetate copolymer (EVA) and polyolefin elastomer (POE) as the matrix resin is currently the most widely used packaging material. Although the packaging film accounts for a low proportion of the overall cost of the module, it is a key material that determines the performance of photovoltaic modules, such as product quality, power generation efficiency, and module life.

[0003] Photovoltaic modules are affected by factors such as temperature, humidity, ultraviolet rays, rain, snow, and hail during outdoor operation, which can easily cause module aging failure, power attenuation and other problems. Among them, the impact of ultraviolet radiation on photovoltaic modules and materials is particularly obvious. The short-wave radiation of ultraviolet rays has high energy, which can cause electron excitation and energy band changes in solar photovoltaic modules, thereby affecting their photoelectric conversion efficiency. This effect is more obvious on new N-type TOPCon cells and HJT cells. At the same time, long-term ultraviolet radiation will also cause aging of packaging materials, resulting in packaging failure and reduced power generation efficiency of photovoltaic modules. The packaging solution of the prior art that only adds ultraviolet absorbers and light stabilizers will also gradually fail over time and cannot guarantee long-term anti-ultraviolet requirements.

[0004] On the other hand, due to the poor compatibility of EVA and POE with some functional additives, the additives tend to migrate and accumulate on the film surface during storage, affecting the performance of the film and different substrates, resulting in quality problems such as bubbles, delamination, uneven cross-linking, and slippage with the battery cells. This impact will also reduce the power generation and life of the module. Summary of the invention

[0005] The main purpose of the present invention is to provide a modified co-crosslinking agent, a packaging film and a photovoltaic module to solve the problems of poor long-term UV resistance of packaging materials and easy precipitation of additives in the prior art.

[0006] In order to achieve the above object, according to one aspect of the present invention, a modified cross-linking agent is provided, comprising a nano-oxide and an isocyanate group grafted on the surface of the nano-oxide; the grafting rate of the isocyanate group of the modified cross-linking agent on the surface of the nano-oxide is 5 to 20%; the modified cross-linking agent is tested by FTIR at 1640 to 1700 cm-1 The range has vibration peaks.

[0007] Further, the raw material of the isocyanurate group includes an isocyanate monomer containing a terminal double bond; preferably, the isocyanate monomer containing a terminal double bond includes one or more of triallyl isocyanurate, diallyl isocyanurate and tris(2-acryloxyethyl)isocyanurate; and / or the nano oxide includes one or more of nano silicon dioxide, nano titanium dioxide and nano aluminum oxide; preferably, the particle size of the nano oxide is 5 to 400 nm.

[0008] Furthermore, the preparation method of the modified cross-linking aid comprises the following steps: step S1, drying the nano oxide and dispersing it in a solvent to obtain a nano oxide solution; step S2, adding an isocyanurate monomer containing a terminal double bond and a catalyst to the nano oxide solution, and performing a grafting reaction under an inert atmosphere to obtain a modified cross-linking aid.

[0009] Furthermore, in step S1, the drying temperature is 100-150°C and the time is 4-12 hours; and / or the dried nano-oxide is mixed with a solvent and ultrasonicated for dispersion; preferably, the solvent includes toluene and / or ethyl acetate, and the ultrasonication time is 30-120 minutes.

[0010] Further, in step S2, the catalyst includes one or more of dibutyltin dilaurate, dibutyltin oxide and tetra-n-butyl lead; and / or the weight ratio of the nano oxide to the isocyanurate monomer containing a terminal double bond is (4-20):1; and / or the weight ratio of the isocyanurate monomer containing a terminal double bond to the catalyst is (50-500):1; and / or the temperature of the grafting reaction is 50-90°C and the time is 2-8h.

[0011] According to another aspect of the present invention, a packaging adhesive film is provided. The packaging adhesive film comprises a base resin and the modified auxiliary cross-linking agent of the present invention.

[0012] Furthermore, the weight percentage of the modified auxiliary cross-linking agent to the base resin is 0.5-15%; preferably, by weight, the encapsulation film includes 100 parts of base resin, 0.1-2 parts of cross-linking agent, 0-1 part of added auxiliary cross-linking agent, 0.5-15 parts of modified auxiliary cross-linking agent, 0.1-5 parts of silane coupling agent, 0.05-2 parts of antioxidant and 0-1 part of ultraviolet absorber.

[0013] Further, the base resin includes ethylene-vinyl acetate copolymer and / or polyolefin elastomer; preferably, the melt flow rate of the base resin is 1.0-30 g / 10 min, and the transmittance is ≥88%; and / or the added auxiliary cross-linking agent includes one or more of triallyl isocyanurate, triallyl cyanurate and trimethylolpropane triacrylate; and / or

[0014] Crosslinking agents include 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 1,1-(ditert-butylperoxy)3,3,5-trimethylcyclohexane, tert-butyl peroxybenzoate, triphenylmethane-4,4',4"-triisocyanate, diisopropylbenzene peroxide, bis(2-tert-butylperoxyisopropyl)benzene, tert-butyl peroxide, tert-amyl peroxybenzoate, di-tert-amyl peroxide, tert-butyl peroxybenzoate, One or more of tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxy-3,5,5-trimethylhexanoate, di(4-chlorobenzoyl)peroxide, di(2,4-dichlorobenzyl)peroxide, di(4-methylphenyl)peroxide, n-butyl-4,4-di(tert-butylperoxy)valerate, ethyl-3,3-di(tert-butylperoxy)butyrate, tert-butylperoxy-2-ethylhexylcarbonate; and / or

[0015] The silane coupling agent includes one or more of vinyl trimethoxysilane, vinyl triethoxysilane, γ-methacryloxypropyl trimethoxysilane, 3-(2,3-epoxypropoxy)propyl trimethoxysilane, methacrylate silane, and vinyl triisopropoxysilane; and / or the antioxidant includes one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate n-octadecyl alcohol ester, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl) isocyanuric acid species; and / or the ultraviolet absorber includes one or more of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate, bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate, poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinethanol) succinate, 2-hydroxy-4-n-octyloxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-2′-carboxybenzophenone, and 2,4-dihydroxybenzophenone.

[0016] Furthermore, the thickness of the packaging film is 0.01-1.0 mm; and / or the surface migration amount of the modified cross-linking agent is characterized by FTIR, and after the packaging film is sealed and stored at room temperature for 180 days, the migration amount of the modified cross-linking agent therein is ≤0.5%.

[0017] According to another aspect of the present invention, a photovoltaic module is provided, comprising the above-mentioned packaging film of the present invention.

[0018] By applying the technical solution of the present invention, the isocyanate groups are modified on the surface of the nano oxide particles, so that the nano oxide particles can have the effect of assisting cross-linking, thereby improving the precipitation problem of the cross-linking agent during storage. At the same time, the addition of nano oxide particles also further makes the film have excellent UV resistance. The modified cross-linking agent of the present invention can have the characteristics of low precipitation and UV resistance, ensuring the long-term stability of the photovoltaic module. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0020] Figure 1 The FTIR test graph of the modified auxiliary cross-linking agent prepared in Example 1 according to the present invention is shown; and

[0021] Figure 2 The FTIR test graphs of the packaging film according to Application Example 1 of the present invention before and after being sealed and stored at room temperature for 180 days are shown. DETAILED DESCRIPTION

[0022] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0023] As described in the background of the present invention, the prior art has the problem that the long-term UV resistance of the packaging material is poor and the additive is easy to precipitate. In order to solve the above problems, in a typical embodiment of the present invention, a modified co-crosslinking agent is provided, including a nano-oxide and an isocyanate group grafted on the surface of the nano-oxide; the grafting rate of the isocyanate group of the modified co-crosslinking agent on the surface of the nano-oxide is 5-20%; the modified co-crosslinking agent is tested by FTIR at 1640-1700cm -1 The grafting rate is the mass ratio of isocyanate groups anchored on the surface of nano-oxide to the mass ratio of nano-oxide.

[0024] The modified cross-linking agent of the present invention belongs to modified nano oxide particles, and the size is determined by the nano oxide particles, which is obviously larger than the conventional small molecule cross-linking agent. Based on the larger size, the migration ability is very weak, and it is not easy to migrate to the surface in the resin, and further, the surface migration problem of the encapsulating film will not occur during long-term storage or use. At the same time, the surface of the nano oxide particles is modified with isocyanate groups, and the compatibility of the obtained modified cross-linking agent with the matrix resin is greatly improved, and it is not easy to agglomerate, and it has a good cross-linking rate. When the modified cross-linking agent is used for the encapsulating film, it can have good anti-ultraviolet performance, reduce the power attenuation caused by long-term ultraviolet radiation of photovoltaic modules, improve the problem that the cross-linking agent is easy to precipitate to the film surface in the existing encapsulation technology solution, and has the characteristics of anti-ultraviolet, low water vapor transmission rate, etc., and further improves the reliability of the encapsulating film.

[0025] In order to better graft the isocyanate group to the surface of the nano oxide, thereby further improving the problem of additive precipitation during the storage of the packaging film, in a preferred embodiment, the raw material of the isocyanurate group includes an isocyanate monomer containing a terminal double bond; preferably, the isocyanate monomer containing a terminal double bond includes one or more of triallyl isocyanurate (TAIC), diallyl isocyanurate (TAC) and tris(2-acryloyloxyethyl) isocyanurate; more preferably, the isocyanurate monomer containing a terminal double bond is triallyl isocyanurate.

[0026] In a preferred embodiment, the nano-oxide includes one or more of nano-silicon dioxide, nano-titanium dioxide and nano-aluminum trioxide; preferably, the particle size of the nano-oxide is 5 to 400 nm. Under the above conditions, the nano-particles are less likely to migrate to the surface of the film due to their larger size, and are less likely to agglomerate, the isocyanurate groups are more evenly distributed in the nano-oxide particles, the modification reaction effect is better, and the problems of reaction product sedimentation and reduced light transmittance of the encapsulation film can be further reduced.

[0027] For the purpose of further improving the long-term UV resistance and additive precipitation performance of the packaging material, it is most preferred that the modified auxiliary cross-linking agent is nano-silicon dioxide modified with triallyl isocyanurate monomer, or nano-aluminum oxide modified with diallyl isocyanurate monomer.

[0028] Specifically, in a preferred embodiment, the preparation method of the modified cross-linking aid comprises the following steps: step S1, drying the nano-oxide and dispersing it in a solvent to obtain a nano-oxide solution; step S2, adding an isocyanurate monomer containing a terminal double bond and a catalyst to the nano-oxide solution, and performing a grafting reaction under an inert atmosphere to obtain a modified cross-linking aid.

[0029] The invention first dries the nano oxide and makes the nano oxide evenly dispersed to obtain a nano oxide solution; then adds an isocyanurate monomer containing a terminal double bond and a catalyst, and makes the isocyanate group (-NCO) in the isocyanurate monomer react with the hydroxyl group (-OH) on the surface of the nano oxide in an inert atmosphere, and increases the reaction rate by the catalyst, and the isocyanate group is grafted on the surface of the nano oxide, and solid-liquid separation is performed by filtering or centrifugation to obtain a solid product, i.e., a modified auxiliary cross-linking agent. The method of the invention greatly shortens the reaction process, can prepare the reaction product by a one-pot method, has a high product yield, and can have the characteristics of low precipitation and UV resistance, and is suitable for packaging adhesive films.

[0030] Taking nano-silica and triallyl isocyanurate as an example, the typical reaction formula is as follows:

[0031]

[0032] The number of hydroxyl groups on the surface of nano-silica is only for illustration. In actual nano-silica, the number of hydroxyl groups on the surface of nano-particles is generally more than one, so there are generally multiple grafted groups on the surface of nano-silica particles.

[0033] In a preferred embodiment, in step S1, the drying temperature is 100-150°C for 4-12 hours; and / or the dried nano-oxide is mixed with a solvent and ultrasonicated for dispersion; preferably, the solvent includes toluene and / or ethyl acetate, which does not participate in the nucleophilic reaction and does not affect the reaction result, and the ultrasonication time is 30-120 minutes. The above conditions are more conducive to uniformly dispersing the nano-oxide in the solution, which is conducive to the smooth progress of the subsequent grafting reaction.

[0034] In order to further improve the reaction rate of the grafting reaction and make the isocyanate group more fully grafted with the hydroxyl group on the surface of the nano oxide particles, in a preferred embodiment, in step S2, the catalyst includes one or more of dibutyltin dilaurate, dibutyltin oxide and tetra-n-butyl lead; and / or the weight ratio of the nano oxide to the isocyanurate monomer containing a terminal double bond is (4-20):1; and / or the weight ratio of the isocyanurate monomer containing a terminal double bond to the catalyst is (50-500):1; and / or the temperature of the grafting reaction is 50-90°C and the time is 2-8h. Under the above conditions, the isocyanurate monomer reaction can be further made more fully and completely, and the occurrence of side reactions can be further reduced while the reaction rate is improved.

[0035] In another typical embodiment of the present invention, a packaging film is provided, which includes a base resin and the modified co-crosslinking agent of the present invention. Due to the use of the modified co-crosslinking agent of the present invention, the long-term UV resistance of the packaging film is improved, and the precipitation of the auxiliary agent is greatly reduced, and the life of the film is significantly increased.

[0036] In a preferred embodiment, the weight percentage of the modified cross-linking agent in the base resin is 0.5-15%, and the above range can be flexibly adjusted according to the usage scenario to meet the requirements of mechanical properties, water vapor barrier, UV resistance, etc. of the package.

[0037] Preferably, the encapsulation film comprises 100 parts of base resin, 0.1-2 parts of cross-linking agent, 0-1 parts of external auxiliary cross-linking agent, 0.5-15 parts of the modified auxiliary cross-linking agent of the present invention, 0.1-5 parts of silane coupling agent, 0.05-2 parts of antioxidant and 0-1 parts of ultraviolet absorber by weight. The addition of cross-linking agent and auxiliary cross-linking agent can help improve the cross-linking performance of the encapsulation film. Silane coupling agent can improve the corresponding mechanical properties of the film. Antioxidant and ultraviolet absorber can further improve the aging resistance of the film. The above-mentioned addition amount range can further improve the various properties of the cross-linked encapsulation film, and at the same time, it is more conducive to the role of the modified auxiliary cross-linking agent of the present invention, so that the film has better long-term ultraviolet resistance and further reduces the precipitation of auxiliary agents, and does not affect the light transmittance and mechanical properties of the film.

[0038] In order to further improve the comprehensive properties of the encapsulation film, such as mechanical properties, transparency, and encapsulation properties, in a preferred embodiment, the base resin includes ethylene-vinyl acetate copolymer (EVA) and / or polyolefin elastomer (POE); preferably, the melt flow rate of the base resin is 1.0-30 g / 10 min, and the transmittance is ≥88%; and / or the added auxiliary cross-linking agent includes one or more of triallyl isocyanurate, triallyl cyanurate, and trimethylolpropane triacrylate, which is more suitable as a material for the encapsulation film of photovoltaic modules.

[0039] In order to further improve the anti-aging performance of the packaging film, in a preferred embodiment, the crosslinking agent includes 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 1,1-(diperoxy-tert-butyl)3,3,5-trimethylcyclohexane, tert-butyl peroxybenzoate, triphenylmethane-4,4',4"-triisocyanate, diisopropyl peroxide, bis(2-tert-butylperoxyisopropyl)benzene, tert-butyl peroxide isopropyl benzene, tert-amyl peroxybenzoate, di-tert-amyl peroxide, tert-butyl peroxybenzoate. , tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxy-3,5,5-trimethylhexanoate, di(4-chlorobenzoyl)peroxide, di(2,4-dichlorobenzyl)peroxide, di(4-methylphenyl)peroxide, n-butyl-4,4-di(tert-butylperoxy)valerate, ethyl-3,3-di(tert-butylperoxy)butyrate, tert-butylperoxy-2-ethylhexylcarbonate; and / or silane coupling agents include vinyl trimethoxysilane, vinyl triethoxysilane, γ- Methacryloxypropyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methacrylate silane, vinyl triisopropoxysilane or one or more thereof; and / or antioxidants include pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate n-octadecyl alcohol ester, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid or one or more thereof; and / or ultraviolet absorbers include bis(2 ,2,6,6-tetramethyl-4-piperidinyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate, bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate, poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinethanol) succinate, 2-hydroxy-4-n-octyloxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-2′-carboxybenzophenone, 2,4-dihydroxybenzophenone.

[0040] In order to make the encapsulation film provided by the present invention more suitable for use as a photovoltaic module, in a preferred embodiment, the thickness of the encapsulation film is 0.01 to 1.0 mm. In the thermal curing system containing the above-mentioned modified co-crosslinking agent, the appropriate thickness can make the modified co-crosslinking agent more evenly distributed, and the curing is more complete, and the film also has a certain light transmittance. And / or the surface migration amount of the modified co-crosslinking agent is characterized by FTIR. After the encapsulation film is sealed and stored at room temperature for 180 days, the migration amount of the modified co-crosslinking agent therein is ≤0.5%, showing a significantly improved agent migration performance.

[0041] In a preferred embodiment, the preparation method of the encapsulation film includes the following steps: mixing a cross-linking agent, an additional auxiliary cross-linking agent, a modified auxiliary cross-linking agent, a silane coupling agent, an antioxidant and a UV absorber, and adding them to a matrix resin for mixing to obtain a mixed semi-finished product; sequentially melting and extruding the mixed semi-finished product, and casting it into a film to obtain a encapsulation film; preferably, the temperature of the mixture is 25 to 50°C, and the time is 0.5 to 2h; and / or the melting temperature is 75 to 90°C.

[0042] After the components other than the matrix resin are mixed in a prescribed proportion according to weight parts, they are added to the matrix resin in batches to obtain the corresponding mixed semi-finished products, and the premix is ​​melted at 75-90° C., and a film is prepared by extrusion casting to obtain the corresponding encapsulation film. The cross-linked encapsulation film prepared according to the above method can further solve the problem of easy precipitation of the cross-linking agent of the encapsulation film in the prior art, which leads to easy slippage of the film and uneven cross-linking.

[0043] In another typical embodiment of the present invention, a photovoltaic module is also provided, comprising the above-mentioned encapsulation film of the present invention. Specifically, the above-mentioned encapsulation film of the present invention is laminated with the module material, the lamination temperature is 140-155°C, the time is 15-20 minutes, the cross-linking rate and cross-linking degree are more suitable, and the occurrence of adverse reactions such as bubbles can be further reduced. Since the above-mentioned encapsulation film will not have the problem of surface migration during long-term storage, and has good anti-ultraviolet performance, the power attenuation phenomenon of the photovoltaic module caused by long-term ultraviolet radiation can be greatly reduced, and the service life of the photovoltaic module can be significantly extended.

[0044] Typically but not limiting, the particle size of the nano-oxide is 5 nm, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm or a range consisting of any two of these values.

[0045] Typically but not limiting, the grafting rate of the isocyanate groups of the modified auxiliary cross-linking agent on the surface of the nano-oxide is 5%, 10%, 15%, 20% or a range consisting of any two of these values.

[0046] Typically but not limiting, the weight ratio of the nano oxide to the isocyanurate monomer containing a terminal double bond is 4:1, 8:1, 10:1, 15:1, 18:1, 20:1 or a range consisting of any two of them.

[0047] Typically, but not limiting, the weight ratio of the isocyanurate monomer containing a terminal double bond to the catalyst is 50:1, 100:1, 200:1, 300:1, 400:1, 500:1 or a range consisting of any two of these values.

[0048] Typically but not limiting, the grafting reaction temperature is 50°C, 60°C, 70°C, 80°C, 90°C or a range consisting of any two of them, and the time is 2h, 3h, 4h, 5h, 6h, 7h, 8h or a range consisting of any two of them.

[0049] Typically but not limiting, the weight percentage of the modified auxiliary cross-linking agent to the base resin is 0.5%, 1%, 5%, 8%, 10%, 12%, 15% or a range consisting of any two of these values.

[0050] Typically, but not limiting, the encapsulating film includes 100 parts of a base resin, 0.1, 0.5, 1, 1.5, 2 parts or a range consisting of any two of a crosslinking agent, 0, 0.2, 0.5, 0.8, 1 part or a range consisting of any two of a crosslinking agent, 0.5, 1, 5, 8, 10, 12, 15 parts or a range consisting of any two of a modified crosslinking agent, 0.1, 1, 2, 3, 4, 5 parts or a range consisting of any two of a silane coupling agent, 0.05, 0.1, 0.5, 1, 1.5, 2 parts or a range consisting of any two of an antioxidant, and 0, 0.2, 0.5, 0.8, 1 part or a range consisting of any two of a UV absorber.

[0051] Typically but not limiting, the thickness of the packaging film is 0.01 mm, 0.1 mm, 0.2 mm, 0.5 mm, 0.8 mm, 1.0 mm or a range consisting of any two of these values.

[0052] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0053] Preparation Example 1

[0054] Step S1, drying nano silicon dioxide with a particle size of 200 nm at a temperature of 120° C. for 8 hours, mixing the dried nano oxide with toluene, and performing ultrasonic treatment for 80 minutes to disperse the nano oxide solution;

[0055] Step S2, adding triallyl isocyanurate and dibutyltin dilaurate catalyst to the nano oxide solution, carrying out grafting reaction under nitrogen atmosphere, the reaction temperature is 70° C., the reaction time is 5 hours, and a modified auxiliary cross-linking agent is obtained, and the grafting rate is 12%.

[0056] The weight ratio of the nano-oxide to the isocyanurate monomer containing a terminal double bond is 10:1; the weight ratio of the isocyanurate monomer containing a terminal double bond to the catalyst is 300:1.

[0057] Preparation Example 2

[0058] Step S1, drying nano titanium dioxide with a particle size of 5 nm at a temperature of 100° C. for 12 h, mixing the dried nano titanium dioxide with toluene, and performing ultrasonic treatment for 30 min to disperse the nano titanium dioxide to obtain a nano titanium dioxide solution;

[0059] Step S2, adding diallyl isocyanurate and dibutyltin oxide catalyst to the nano oxide solution, carrying out grafting reaction under nitrogen atmosphere, the reaction temperature is 50° C., the reaction time is 8 hours, and a modified auxiliary cross-linking agent is obtained, and the grafting rate is 5%.

[0060] The weight ratio of the nano-oxide to the isocyanurate monomer containing a terminal double bond is 20:1; the weight ratio of the isocyanurate monomer containing a terminal double bond to the catalyst is 500:1.

[0061] Preparation Example 3

[0062] Step S1, drying nano-aluminum oxide with a particle size of 400 nm at a temperature of 150° C. for 4 hours, mixing the dried nano-aluminum oxide with ethyl acetate, and performing ultrasonic treatment for 120 minutes to disperse the nano-aluminum oxide to obtain a nano-aluminum oxide solution;

[0063] Step S2, adding tri(2-acryloyloxyethyl)isocyanurate and tetra-n-butyl lead catalyst to the nano oxide solution, carrying out grafting reaction under nitrogen atmosphere, the reaction temperature is 90° C., the reaction time is 2 h, and a modified auxiliary cross-linking agent is obtained, and the grafting rate is 20%.

[0064] The weight ratio of the nano-oxide to the isocyanurate monomer containing a terminal double bond is 4:1; the weight ratio of the isocyanurate monomer containing a terminal double bond to the catalyst is 50:1.

[0065] Application Example 1

[0066] The encapsulation film includes 100 parts of a base resin (ethylene-vinyl acetate copolymer, melt flow rate of 16.0 g / 10 min, transmittance ≥ 88%), 1 part of a cross-linking agent (1,1-(ditert-butylperoxide) 3,3,5-trimethylcyclohexane), 0 parts of an added auxiliary cross-linking agent, 5 parts of a modified auxiliary cross-linking agent (Preparation Example 1), 2 parts of a silane coupling agent (vinyl trimethoxysilane), 0.1 parts of an antioxidant (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) and 0 parts of a UV absorber.

[0067] After mixing the above raw materials except the matrix resin, add them to the matrix resin for mixing, the mixing temperature is 30℃, and the time is 1h. After mixing evenly, put it into the extruder. After melting at 80℃, extrusion, film casting, cooling, winding and other processes are performed to prepare the corresponding encapsulation film with a thickness of 0.05mm. When laminating the components, place the tempered glass, encapsulation film, crystalline silicon cell, encapsulation film, and backplane in order from top to bottom, and place them at 150℃ and laminate for 18 minutes to obtain the corresponding photovoltaic components.

[0068] Application Example 2

[0069] The difference from Application Example 1 is that the composition of the encapsulation film is different:

[0070] The encapsulation film includes 100 parts of a base resin (ethylene-vinyl acetate copolymer, melt flow rate of 16.0 g / 10 min, transmittance ≥ 88%), 1 part of a cross-linking agent (1,1-(ditert-butylperoxide) 3,3,5-trimethylcyclohexane), 0.5 parts of an added auxiliary cross-linking agent (triallyl isocyanurate), 5 parts of a modified auxiliary cross-linking agent (Preparation Example 1), 2 parts of a silane coupling agent (vinyl trimethoxysilane), 0.1 parts of an antioxidant (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) and 0 parts of a UV absorber.

[0071] Application Example 3

[0072] The difference from Application Example 1 is that the composition of the encapsulation film is different:

[0073] The encapsulation film includes 100 parts of a base resin (ethylene-vinyl acetate copolymer, melt flow rate of 16.0 g / 10 min, transmittance ≥ 88%), 1 part of a cross-linking agent (1,1-(ditert-butylperoxide) 3,3,5-trimethylcyclohexane), 0.5 parts of an added auxiliary cross-linking agent (triallyl isocyanurate), 5 parts of a modified auxiliary cross-linking agent (Preparation Example 2), 2 parts of a silane coupling agent (vinyl trimethoxysilane), 0.1 parts of an antioxidant (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) and 0 parts of a UV absorber.

[0074] Application Example 4

[0075] The difference from Application Example 1 is that the composition of the encapsulation film is different:

[0076] The encapsulation film includes 100 parts of a base resin (ethylene-vinyl acetate copolymer, melt flow rate of 16.0 g / 10 min, transmittance ≥ 88%), 1 part of a cross-linking agent (1,1-(ditert-butylperoxide) 3,3,5-trimethylcyclohexane), 0.5 parts of an added auxiliary cross-linking agent (triallyl isocyanurate), 5 parts of a modified auxiliary cross-linking agent (Preparation Example 3), 2 parts of a silane coupling agent (vinyl trimethoxysilane), 0.1 parts of an antioxidant (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) and 0 parts of a UV absorber.

[0077] Application Example 5

[0078] The difference from Application Example 1 is that the composition of the encapsulation film is different:

[0079] The encapsulation film includes 100 parts of a base resin (ethylene-vinyl acetate copolymer, melt flow rate of 1.0 g / 10 min, transmittance ≥ 88%), 0.1 parts of a cross-linking agent (2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane), 0 parts of an added auxiliary cross-linking agent, 0.5 parts of a modified auxiliary cross-linking agent (Preparation Example 1), 0.1 parts of a silane coupling agent (vinyl trimethoxysilane), 0.05 parts of an antioxidant (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) and 0 parts of a UV absorber.

[0080] Application Example 6

[0081] The difference from Application Example 1 is that the composition of the encapsulation film is different:

[0082] The encapsulation film includes 100 parts of a base resin (polyolefin elastomer, melt flow rate of 30g / 10min, transmittance ≥88%), 2 parts of a cross-linking agent (1,1-(ditert-butylperoxide) 3,3,5-trimethylcyclohexane), 1 part of an additional auxiliary cross-linking agent (triallyl cyanurate), 15 parts of a modified auxiliary cross-linking agent (Preparation Example 1), 5 parts of a silane coupling agent (vinyl triethoxysilane), 2 parts of an antioxidant (β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) and 1 part of an ultraviolet absorber (bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate).

[0083] Application Example 7

[0084] The composition of the packaging film is the same as that of Application Example 1.

[0085] After mixing the above raw materials except the matrix resin, add them to the matrix resin for mixing, the mixing temperature is 25℃, and the time is 2h. After mixing evenly, put it into the extruder. After melting at 75℃, extrusion, film casting, cooling, winding and other processes are performed to prepare the corresponding encapsulation film with a thickness of 0.01mm. When laminating the components, place the tempered glass, encapsulation film, crystalline silicon cell, encapsulation film, and backplane in order from top to bottom, and place them at 140℃ for 20 minutes to obtain the corresponding photovoltaic components.

[0086] Application Example 8

[0087] The composition of the packaging film is the same as that of Application Example 1.

[0088] After mixing the above raw materials except the matrix resin, add them to the matrix resin for mixing, the mixing temperature is 50℃, and the time is 0.5h. After mixing evenly, put it into the extruder. After melting at 90℃, extrusion, film casting, cooling, winding and other processes are performed to prepare the corresponding encapsulation film with a thickness of 1.0mm. When laminating the components, place the tempered glass, encapsulation film, crystalline silicon cell, encapsulation film, and backplane in order from top to bottom, and place them at 155℃ for lamination for 15 minutes to obtain the corresponding photovoltaic components.

[0089] Comparative Example 1

[0090] The difference from Application Example 1 is that the composition of the encapsulation film is different:

[0091] The encapsulation film includes 100 parts of a base resin (ethylene-vinyl acetate copolymer, melt flow rate of 16.0 g / 10 min, transmittance ≥ 88%), 1 part of a cross-linking agent (1,1-(ditert-butylperoxide) 3,3,5-trimethylcyclohexane), 0.5 parts of an additional auxiliary cross-linking agent (triallyl isocyanurate), 0 parts of a modified auxiliary cross-linking agent, 2 parts of a silane coupling agent (vinyl trimethoxysilane), 0.1 parts of an antioxidant (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) and 0 parts of a UV absorber.

[0092] Comparative Example 2

[0093] The difference from Application Example 1 is that the composition of the encapsulation film is different:

[0094] The encapsulation film includes 100 parts of a base resin (ethylene-vinyl acetate copolymer, melt flow rate of 16.0 g / 10 min, transmittance ≥ 88%), 6 parts of a cross-linking agent (nano hybrid cross-linking agent of specific embodiment eight of Chinese patent CN 111621076 A), 2 parts of a silane coupling agent (vinyl trimethoxy silane), 0.1 parts of an antioxidant (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) and 0 parts of a UV absorber.

[0095] Performance Test:

[0096] The photovoltaic modules of the above application examples and application comparison examples were subjected to the following tests, and the results are shown in Table 1.

[0097] The FTIR test graph of the modified cross-linking agent prepared in Example 1 is shown in Figure 1 ,Depend on Figure 1 It can be seen that the modified cross-linking agent is tested by FTIR at 1640-1700 cm -1 The range has vibration peaks.

[0098] The FTIR test graphs of the encapsulation film of Application Example 1 before and after sealed storage at room temperature for 180 days are shown in Figure 2 ,Depend on Figure 2 It can be seen that the surface migration amount of the modified co-crosslinking agent is characterized by FTIR. After the encapsulation film is sealed and stored at room temperature for 180 days, the migration amount of the modified co-crosslinking agent therein is ≤0.5%.

[0099] Peel strength: refer to standard GB / T29848 "Ethylene-vinyl acetate copolymer film for photovoltaic encapsulation".

[0100] ΔYI: Refer to the standard GB / T29848 "Ethylene-vinyl acetate copolymer film for photovoltaic encapsulation", the test temperature is 85°C, the test relative humidity is 85%, and the aging time is 1000h. Before and after the test, the yellowing index (ΔYI) is measured according to the national standard GB2409 "Plastic Yellow Index Test Method".

[0101] PID attenuation: Refer to standard GB / T29848 "Ethylene-vinyl acetate copolymer film for photovoltaic encapsulation".

[0102] Cross-linking degree: refer to standard GB / T29848 "Ethylene-vinyl acetate copolymer film for photovoltaic encapsulation".

[0103] Light transmittance: Refer to standard GB / T29848 "Ethylene-vinyl acetate copolymer film for photovoltaic encapsulation".

[0104] Table 1

[0105]

[0106]

[0107] As can be seen from the above, compared with the comparative example, the present invention modifies the isocyanate group on the surface of the nano oxide particles, which can make the nano oxide particles have the effect of assisting cross-linking, thereby improving the precipitation problem of the cross-linking agent during storage. At the same time, the addition of nano oxide particles also further makes the film have excellent UV resistance. The modified cross-linking agent of the present invention can have the characteristics of low precipitation and UV resistance, ensuring the long-term stability of the photovoltaic module.

[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A modified co-crosslinking agent, It is characterized in that It comprises a nano oxide and an isocyanate group grafted on the surface of the nano oxide; the grafting rate of the isocyanate group of the modified auxiliary cross-linking agent on the surface of the nano oxide is 5 to 20%; The modified auxiliary cross-linking agent is tested by FTIR at 1640-1700 cm -1 The range has vibration peaks.

2. The modified crosslinking aid according to claim 1, It is characterized in that The raw material of the isocyanurate group includes an isocyanate monomer containing a terminal double bond; preferably, the isocyanate monomer containing a terminal double bond includes one or more of triallyl isocyanurate, diallyl isocyanurate and tris(2-acryloyloxyethyl)isocyanurate; and / or The nano-oxide includes one or more of nano-silicon dioxide, nano-titanium dioxide and nano-aluminum oxide; preferably, the particle size of the nano-oxide is 5 to 400 nm.

3. The modified crosslinking aid according to claim 2, It is characterized in that The preparation method of the modified cross-linking aid comprises the following steps: Step S1, drying the nano-oxide and dispersing it in a solvent to obtain a nano-oxide solution; Step S2, adding the isocyanurate monomer containing a terminal double bond and a catalyst into the nano-oxide solution, and performing a grafting reaction under an inert atmosphere to obtain the modified auxiliary cross-linking agent.

4. The modified crosslinking aid according to claim 3, It is characterized in that In the step S1, The drying temperature is 100-150°C and the drying time is 4-12 hours; and / or The dried nano-oxide is mixed with the solvent and subjected to ultrasonic treatment to perform the dispersion. Preferably, the solvent includes toluene and / or ethyl acetate, and the ultrasonic treatment time is 30 to 120 minutes.

5. The modified co-crosslinking agent according to claim 3 or 4, It is characterized in that In the step S2, The catalyst comprises one or more of dibutyltin dilaurate, dibutyltin oxide and tetra-n-butyl lead; and / or The weight ratio of the nano oxide to the isocyanurate monomer containing a terminal double bond is (4-20):1; and / or The weight ratio of the isocyanurate monomer containing a terminal double bond to the catalyst is (50-500):1; and / or The grafting reaction temperature is 50-90° C. and the time is 2-8 hours.

6. A packaging film, It is characterized in that The packaging adhesive film comprises a base resin and the modified co-crosslinking agent according to any one of claims 1 to 5.

7. The encapsulation film according to claim 6, It is characterized in that The weight percentage of the modified cross-linking aid in the base resin is 0.5-15%; Preferably, in parts by weight, the encapsulation film includes 100 parts of base resin, 0.1-2 parts of cross-linking agent, 0-1 parts of external auxiliary cross-linking agent, 0.5-15 parts of the modified auxiliary cross-linking agent, 0.1-5 parts of silane coupling agent, 0.05-2 parts of antioxidant and 0-1 parts of ultraviolet absorber.

8. The encapsulation film according to claim 7, It is characterized in that The matrix resin comprises ethylene-vinyl acetate copolymer and / or polyolefin elastomer; preferably, the matrix resin has a melt flow rate of 1.0 to 30 g / 10 min and a light transmittance of ≥88%; and / or The external auxiliary cross-linking agent includes one or more of triallyl isocyanurate, triallyl cyanurate and trimethylolpropane triacrylate; and / or The crosslinking agent includes 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 1,1-(ditert-butylperoxy)3,3,5-trimethylcyclohexane, tert-butyl peroxybenzoate, triphenylmethane-4,4',4"-triisocyanate, diisopropylbenzene peroxide, bis(2-tert-butylperoxyisopropyl)benzene, tert-butyl peroxyisopropylbenzene, tert-amyl peroxybenzoate, ditert-amyl peroxide, tert-butyl peroxybenzoate , tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxy-3,5,5-trimethylhexanoate, di(4-chlorobenzoyl)peroxide, di(2,4-dichlorobenzyl)peroxide, di(4-methylphenyl)peroxide, n-butyl-4,4-di(tert-butylperoxy)valerate, ethyl-3,3-di(tert-butylperoxy)butyrate, tert-butylperoxy-2-ethylhexylcarbonate; and / or The silane coupling agent includes one or more of vinyl trimethoxy silane, vinyl triethoxy silane, γ-methacryloxypropyl trimethoxy silane, 3-(2,3-epoxypropoxy)propyl trimethoxy silane, methacrylate silane, and vinyl triisopropoxy silane; and / or The antioxidant includes one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, n-octadecylβ-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, and 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl) isocyanuric acid; and / or The ultraviolet absorber includes one or more of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate, bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate, poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinethanol) succinate, 2-hydroxy-4-n-octyloxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-2′-carboxybenzophenone, and 2,4-dihydroxybenzophenone.

9. The encapsulation film according to any one of claims 6 to 8, It is characterized in that The thickness of the packaging film is 0.01-1.0 mm; and / or The surface migration amount of the modified auxiliary cross-linking agent is characterized by FTIR. After the packaging film is sealed and stored at room temperature for 180 days, the migration amount of the modified auxiliary cross-linking agent is ≤0.5%.

10. A photovoltaic module, comprising the encapsulation film according to any one of claims 6 to 9.