Mn < 2 + >-doped non-spherical silicon oxide composite abrasive particle as well as preparation method and application thereof

By converting silicon oxide into an aphrodisiac structure and blending Mn2+ to form composite abrasive particles, the problem of insufficient polishing removal rate of traditional silicon oxide abrasive particles on the surface of silicon carbide is solved, and a more efficient silicon carbide material removal and polishing rate is achieved.

CN119039937APending Publication Date: 2024-11-29TAICANG SILICON SOURCE NANOMATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411286290.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The polishing removal rate of traditional silicon oxide abrasive particles on the surface of silicon carbide cannot meet the current industrial production requirements, and the hardness of silicon carbide is high and chemical inert, which makes processing difficult.

Method used

The anion-induced method is used to convert spherical silicon oxide into an asspherical structure, and the metal Mn2+ is incorporated into the asspherical silicon oxide to form composite abrasive particles, increase the contact sites with single-crystal silicon carbide wafers, improve the mechanical effect, and pass Mn2+ Accelerate the formation of the surface oxide layer of silicon carbide, and synergistically improve the removal rate.

Benefits of technology

The material removal rate of single-crystal silicon carbide wafers is significantly improved, the polishing rate is increased by 188%, and the processing difficulty is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039937A_ABST
    Figure CN119039937A_ABST
Patent Text Reader

Abstract

The invention discloses a Mn < 2 + >-doped non-spherical silicon oxide composite abrasive particle as well as a preparation method and application thereof, and belongs to the field of silicon carbide surface polishing processing. According to the non-spherical silicon oxide disclosed by the invention, the formation of spherical silicon oxide is induced by sodium metaaluminate, then Mn < 2 + > is further doped into the non-spherical silicon oxide, and the oxidation capacity of potassium permanganate is improved due to the addition of the Mn < 2 + >; the non-spherical structure of silicon oxide increases the contact area between the abrasive particles and the silicon carbide workpiece. Compared with conventional spherical silicon oxide abrasive particles, the Mn < 2 + >-doped non-spherical silicon oxide composite abrasive particles have the advantage that the material removal rate of silicon carbide can be maximally increased by 188%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a non-spherical nano-level abrasive grain and a preparation method thereof, in particular to a preparation method of a silicon oxide composite abrasive grain, which is used in the polishing process of silicon carbide round crystals and belongs to the field of surface polishing technology. Background Art

[0002] Compared with the first and second generation semiconductor materials, the third generation semiconductor material silicon carbide (SiC) has better physical properties, such as large bandgap, high breakdown voltage, high thermal conductivity, large electron saturation drift velocity and high melting point, and is therefore widely used in high-frequency and high-power devices. In order to achieve large-scale applications, the epitaxial layer requires the surface roughness of the SiC substrate to be less than 1nm and the surface to be defect-free and damage-free. However, silicon carbide has high hardness and high chemical inertness, resulting in high processing and difficulty.

[0003] Chemical mechanical polishing (CMP) is currently the only method that can achieve global polishing of SiC surfaces. Abrasive particles are the main component of polishing liquid. Commonly used abrasive particles for SiC polishing include aluminum oxide, silicon oxide, nano-diamond, etc. Among them, silicon dioxide (SiO2) is widely used in scientific research and industrial production because of its moderate hardness and good surface quality after polishing workpieces. However, the removal rate of traditional SiO2 abrasive particles for SiC polishing can no longer meet the current industrial production requirements. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the existing processing technology and provide a Mn 2+ Doped non-spherical silicon oxide abrasive particles and preparation method and application thereof. Compared with conventional silicon oxide abrasive particles, the present invention converts spherical silicon oxide into a non-spherical structure by anion induction method, and then adds metal Mn 2+ Added into non-spherical silicon oxide to form composite abrasives. The non-spherical silicon oxide structure increases the contact points with the single crystal silicon carbide wafer and improves the mechanical effect during the CMP process. 2+ The addition of improves the oxidation effect of potassium permanganate, accelerates the formation of oxide layer on the surface of silicon carbide, accelerates the chemical reaction in the CMP process, and the chemical action and mechanical action work together to improve the material removal rate of single crystal silicon carbide wafers to a certain extent.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] A Mn 2+ The method for preparing doped non-spherical silicon oxide abrasive particles comprises the following steps:

[0007] S1 preparation of non-spherical silicon oxide abrasive particles;

[0008] S2 Preparation of Mn 2+Doped non-spherical silicon oxide composite abrasive.

[0009] Furthermore, the process of preparing the non-spherical silicon oxide in step S1 is:

[0010] S11: dispersing silica sol into deionized water, mixing well, placing under reflux and magnetic stirring at 100° C., adding sodium aluminate solution all at once, and obtaining a solution after the reaction is completed;

[0011] S12: The solution after the reaction is aged for 2 hours to obtain a solution containing Mn 2+ A solution doped with non-spherical silicon oxide composite abrasive particles.

[0012] Furthermore, in step S11, the concentration of the sodium aluminate solution is 0.3 wt. %; the particle size of the silica sol is 100 nm; the solid content of the silica sol is 40 wt. %, and the mass ratio of the sodium aluminate solution, the silica sol and the deionized water is 8:15:33.

[0013] Furthermore, in step S11, the heating method is oil bath heating; and the heating time is 3 hours.

[0014] Furthermore, during the aging process in step S12, the aging temperature is 100° C. and the aging time is 2 h.

[0015] Furthermore, in step S2, Mn is prepared 2+ The process of doping non-spherical silicon oxide composite abrasive is:

[0016] S21: adding manganese nitrate to deionized water, stirring at room temperature to obtain a manganese nitrate solution, adding sodium hydroxide solid to deionized water, stirring at room temperature to obtain a sodium hydroxide solution;

[0017] S22: adding manganese nitrate solution and sodium hydroxide solution dropwise to the solution containing non-spherical silicon oxide abrasive particles to adjust the solution pH to 9, and stirring under reflux at 100° C. after the addition is complete. After the reaction is complete, a solution containing Mn 2+ A solution doped with non-spherical silicon oxide composite abrasive particles.

[0018] Further, the preparation of the Mn 2+ During the process of doping the non-spherical silicon oxide composite abrasive grains, the concentration of sodium hydroxide was 1.0 wt.%, the mass ratio of the manganese nitrate solution to the solution containing the non-spherical silicon oxide abrasive grains was 1:7, and the reaction time was 5 hours.

[0019] The present application also provides a Mn 2+ Doped non-spherical silicon oxide composite abrasive grains, using a Mn 2+ The Mn 2+ The doped non-spherical silicon oxide composite abrasive grains have a non-spherical structure.

[0020] The present application also provides a Mn 2+ The application of doped non-spherical silicon oxide composite abrasive particles is used to prepare a polishing liquid for a single crystal silicon carbide wafer, specifically comprising: adding potassium permanganate and deionized water to a solution containing Mn 2+ A solution doped with non-spherical silicon oxide composite abrasive particles is ultrasonically prepared into a polishing liquid, wherein the mass fraction of the silicon oxide composite abrasive particles in the polishing liquid is 7.5wt.%, the mass fraction of the potassium permanganate is 1wt.%, and the pH of the polishing liquid is 9. The present invention has the following beneficial effects:

[0021] The present invention prepares Cr by oil bath method under mild conditions. 3+ The non-spherical silicon oxide composite abrasive is doped, and the hydroxyl groups generated by the hydrolysis of negatively charged aluminate anions in the aqueous solution undergo dehydration condensation with the hydroxyl groups on the surface of silicon oxide to form -Si-O-Al-O-Si-, so that the spherical silicon oxide particles are combined to form a non-spherical structure.

[0022] The Mn prepared by the present invention 2+ Compared with conventional commercially available silicon oxide abrasives, doped non-spherical silicon oxide composite abrasives greatly improve the material removal rate of single crystal silicon carbide wafers after CMP.

[0023] The silicon oxide composite abrasive polishing liquid prepared by the present invention is applied to the CMP process of single crystal SiC. Compared with conventional commercially available silicon oxide abrasives, Mn 2+ The polishing rate of doped non-spherical silicon oxide composite abrasive can be increased by 188%. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a graph showing the effect of different abrasive polishing solutions on the material removal rate of single crystal silicon carbide wafers. DETAILED DESCRIPTION

[0025] In order to make the objectives, technical solutions and advantages of the present invention more clear, the specific implementation modes of the present invention are further described in detail below with reference to the accompanying drawings.

[0026] The present application provides a Mn 2+ The method for preparing doped non-spherical silicon oxide abrasive particles comprises the following steps:

[0027] S1 prepares non-spherical silicon oxide abrasive particles; specifically comprising:

[0028] S11: Disperse the silica sol in deionized water, mix well, place under reflux magnetic stirring and heating at 100°C, add the sodium aluminate solution at one time, and obtain a solution after the reaction is completed; wherein the concentration of the sodium aluminate solution is 0.3wt.%; the silica sol particle size is 100nm; the silica sol solid content is 40wt.%, and the mass ratio of the sodium aluminate solution, the silica sol, and the deionized water is 8:15:33. The heating method in this step is oil bath heating; the heating time is 3h.

[0029] S12: The solution after the reaction is aged for 2 hours to obtain a solution containing Mn 2+ The solution doped with non-spherical silicon oxide composite abrasive particles, wherein the aging temperature is 100°C and the aging time is 2 hours.

[0030] S2 Preparation of Mn 2+ Doped non-spherical silicon oxide composite abrasive; specifically comprising:

[0031] S21: adding manganese nitrate to deionized water, stirring at room temperature to obtain a manganese nitrate solution, adding sodium hydroxide solid to deionized water, stirring at room temperature to obtain a sodium hydroxide solution;

[0032] S22: adding manganese nitrate solution and sodium hydroxide solution dropwise to the solution containing non-spherical silicon oxide abrasive particles to adjust the solution pH to 9, and stirring under reflux at 100° C. after the addition is complete. After the reaction is complete, a solution containing Mn 2+ The solution doped with non-spherical silicon oxide composite abrasive particles has a sodium hydroxide concentration of 1.0 wt.%, a mass ratio of the manganese nitrate solution to the solution containing the non-spherical silicon oxide abrasive particles is 1:7, and the reaction time is 5 hours.

[0033] The present application also provides a Mn 2+ Doped non-spherical silicon oxide composite abrasive grains, using a Mn 2+ The Mn 2+ The doped non-spherical silicon oxide composite abrasive grains are non-spherical in structure. The hydroxyl groups generated by the hydrolysis of negatively charged aluminate anions in the aqueous solution of the present invention undergo dehydration condensation with the hydroxyl groups on the surface of silicon oxide to form -Si-O-Al-O-Si-, so that the spherical silicon oxide particles are combined to form a non-spherical structure. The non-spherical silicon oxide structure increases the contact points with the single crystal silicon carbide wafer and improves the mechanical action during the CMP process. Mn 2+ The addition of improves the oxidation effect of potassium permanganate, accelerates the formation of oxide layer on the surface of silicon carbide, accelerates the chemical reaction in the CMP process, and the chemical action and mechanical action work together to improve the material removal rate of single crystal silicon carbide wafers to a certain extent.

[0034] The present application also provides a Mn 2+The application of doped non-spherical silicon oxide composite abrasive particles is used to prepare a polishing liquid for a single crystal silicon carbide wafer, specifically comprising: adding potassium permanganate and deionized water to a solution containing Mn 2+ A polishing solution is prepared by ultrasonically mixing the non-spherical silicon oxide composite abrasive grains into a solution, wherein the mass fraction of the silicon oxide composite abrasive grains in the polishing solution is 7.5wt.%, the mass fraction of the potassium permanganate is 1wt.%, and the pH value of the polishing solution is 9.

[0035] Example 1

[0036] This embodiment provides Mn 2+ The preparation method of doped non-spherical silicon oxide composite abrasive particles comprises the following steps:

[0037] S1 preparation of non-spherical silicon oxide abrasive particles;

[0038] S2 Preparation of Mn 2+ Doped non-spherical silicon oxide composite abrasive;

[0039] Wherein, in step S1, the preparation process of the non-spherical silicon oxide abrasive particles is as follows:

[0040] S01: 93.75 g of silica sol was diluted to 300 g and placed in a three-necked flask. Under magnetic stirring and 100° C. oil bath reflux heating, sodium aluminate solution was added into the three-necked flask at once and reacted for 3 h.

[0041] S02: After the reaction is completed, turn off the stirring device and age at 100°C for 2h.

[0042] Wherein, in step S1, the step of preparing the sodium aluminate solution is:

[0043] Dissolve 0.15 g of sodium aluminate in 50 g of deionized water and disperse by ultrasonic for later use.

[0044] In step S2, Mn is prepared 2+ Doping non-spherical silicon oxide composite abrasive grains, the specific steps are:

[0045] 0.75 g of Mn(NO3)2 (mass fraction: 50%) was dispersed in 50 mL of pure water, and after ultrasonic dispersion, it was added dropwise into a three-necked flask filled with non-spherical silica. After the addition was completed, the reaction was allowed to proceed for 5 h.

[0046] Comparative Example 1

[0047] Commercially available silica sol with an average particle size of 100 nm was directly used as a spherical silicon oxide comparison sample.

[0048] Comparative Example 2

[0049] The preparation method of the non-spherical silicon oxide abrasive particles provided in this comparative example has the following steps:

[0050] S1 preparation of non-spherical silicon oxide abrasive particles;

[0051] Wherein, in step S1, the preparation process of the non-spherical silicon oxide abrasive particles is as follows:

[0052] S01: 93.75 g of silica sol was diluted to 300 g and placed in a three-necked flask. Under magnetic stirring and 100° C. oil bath reflux heating, sodium aluminate solution was added into the three-necked flask at once and reacted for 3 h.

[0053] S02: After the reaction is completed, turn off the stirring device and age at 100°C for 2h.

[0054] Wherein, in step S1, the step of preparing the sodium aluminate solution is:

[0055] Dissolve 0.15 g of sodium aluminate in 50 g of deionized water and disperse by ultrasonic for later use.

[0056] The following describes the process of preparing the non-spherical silicon oxide abrasive grains prepared by different types of abrasive grains in the above-mentioned embodiment 1 and comparative example 1 and comparative example 2 into a polishing liquid, and the specific steps are as follows:

[0057] 5 g potassium permanganate and an appropriate amount of deionized water were added to the mixture containing Mn in Example 1. 2+ The solution doped with non-spherical silicon oxide composite abrasive, the solution containing spherical silicon oxide in comparative example 1, and the solution containing non-spherical silicon oxide abrasive in comparative example 2 were ultrasonically prepared into 500 g of polishing liquid, the mass fraction of the abrasive in the polishing liquid was 7.5 wt.%, the mass fraction of the potassium permanganate was 1 wt.%, the pH of the polishing liquid was adjusted to 9 with sodium hydroxide, and the ultrasonic time was 10 min.

[0058] The following polishing tests were conducted on the above-mentioned different silicon oxide abrasives and the corresponding polishing solutions:

[0059] 2. Comparative experiment on polishing effect of polishing liquid on silicon carbide

[0060] The experimental steps are:

[0061] The above three polishing solutions were used to carry out polishing tests on single crystal silicon carbide under certain polishing conditions.

[0062] The polishing liquid configuration for the polishing test is as follows:

[0063] Total mass of polishing liquid: 500g;

[0064] Abrasive: 7.5wt.%;

[0065] Potassium permanganate: 1wt.%;

[0066] pH: 9;

[0067] The polishing conditions of the polishing test are as follows:

[0068] Polishing machine: UNIPOL-1502 automatic pressure grinding and polishing machine;

[0069] Workpiece: Si surface of single crystal silicon carbide wafer with a diameter of 50 mm;

[0070] Polishing pad: polyurethane polishing pad;

[0071] Polishing pressure: 6kg;

[0072] Polishing disc speed: 70rpm;

[0073] Polishing time: 1h;

[0074] After polishing, the single crystal silicon carbide wafer was washed and dried in the order of acetone, cleaning solution, deionized water, and anhydrous ethanol, and the mass of the single crystal silicon carbide wafer before and after polishing was weighed with a precision analytical balance to calculate the material removal rate (MRR).

[0075] The polishing effects of the polishing liquids of Example 1, Example 2 and Comparative Example 1 on silicon carbide are shown in Table 1.

[0076] like Figure 1 As shown in Table 1, under the same polishing conditions, the material removal rate of the non-spherical silicon oxide polishing liquid formed after induction by sodium metaaluminate is improved compared with the spherical silicon oxide polishing liquid. 2+ Compared with non-spherical silicon oxide abrasive grains, the material removal rate of the doped non-spherical silicon oxide composite abrasive grains after polishing is increased by 62%, and compared with spherical silicon oxide abrasive grains, the material removal rate of the doped non-spherical silicon oxide composite abrasive grains after polishing is increased by 188%.

[0077] Table 1 Polishing effect of three polishing fluids on silicon carbide

[0078]

[0079] In summary, compared with conventional commercially available silica sol (silicon oxide) abrasive grains, the Mn 2+ The doped non-spherical silicon oxide composite abrasive increases the contact sites with the single crystal silicon carbide wafer and improves the mechanical action during the CMP process. 2+ The addition of Mn increases the oxidation effect of potassium permanganate, accelerates the formation of the oxide layer on the surface of silicon carbide, and accelerates the chemical reaction during the CMP process. The chemical action and mechanical action work together to improve the material removal rate of single crystal silicon carbide wafers to a certain extent. 2+ The material removal rate of doped non-spherical silicon oxide composite abrasive is increased by 222% compared with spherical silicon oxide abrasive.

[0080] The above description is only a preferred embodiment of the present invention, and the embodiment is not intended to limit the patent protection scope of the present invention. Therefore, all equivalent structural changes made using the description and drawings of the present invention should be included in the protection scope of the claims attached to the present invention.

Claims

1. A Mn 2+ Preparation method of doped non-spherical silicon oxide composite abrasive particles, It is characterized in that The following steps are involved: S1 preparation of non-spherical silicon oxide abrasive particles; S2 Preparation of Mn 2+ Doped non-spherical silicon oxide composite abrasive.

2. A Mn as claimed in claim 1 2+ Preparation method of doped non-spherical silicon oxide composite abrasive particles, It is characterized in that The process of preparing the non-spherical silicon oxide in step S1 is: S11: dispersing silica sol into deionized water, mixing well, placing under reflux at 100° C. with magnetic stirring, adding sodium aluminate solution all at once, and obtaining a solution after the reaction is completed; S12: The solution after the reaction is aged for 2 hours to obtain a solution containing Mn 2+ A solution doped with non-spherical silicon oxide composite abrasive particles.

3. A Mn as claimed in claim 2 2+ Preparation method of doped non-spherical silicon oxide composite abrasive particles, It is characterized in that In step S11, the concentration of the sodium aluminate solution is 0.3 wt. %; the particle size of the silica sol is 100 nm; the solid content of the silica sol is 40 wt. %, and the mass ratio of the sodium aluminate solution, the silica sol and the deionized water is 8:15:

33.

4. A Mn as claimed in claim 2 2+ Preparation method of doped non-spherical silicon oxide composite abrasive particles, It is characterized in that In step S11, the heating method is oil bath heating; the heating time is 3 hours.

5. A Mn as claimed in claim 2 2+ Preparation method of doped non-spherical silicon oxide composite abrasive particles, It is characterized in that During the aging process in step S12, the aging temperature is 100° C. and the aging time is 2 hours.

6. A Mn as claimed in claim 1 2+ Preparation method of doped non-spherical silicon oxide composite abrasive particles, It is characterized in that Preparation of Mn in step S2 2+ The process of doping non-spherical silicon oxide composite abrasive is: S21: adding manganese nitrate to deionized water, stirring at room temperature to obtain a manganese nitrate solution, adding sodium hydroxide solid to deionized water, stirring at room temperature to obtain a sodium hydroxide solution; S22: adding manganese nitrate solution and sodium hydroxide solution dropwise to the solution containing non-spherical silicon oxide abrasive particles to adjust the solution pH to 9, and stirring under reflux at 100° C. after the addition is complete. After the reaction is complete, a solution containing Mn 2+ A solution doped with non-spherical silicon oxide composite abrasive particles.

7. A Mn as claimed in claim 6 2+ Preparation method of doped non-spherical silicon oxide composite abrasive particles, It is characterized in that Preparation of the Mn 2+ During the process of doping the non-spherical silicon oxide composite abrasive grains, the concentration of sodium hydroxide was 1.0 wt.%, the mass ratio of the manganese nitrate solution to the solution containing the non-spherical silicon oxide abrasive grains was 1:7, and the reaction time was 5 hours.

8. A kind of Mn 2+ Doped non-spherical silicon oxide composite abrasive, It is characterized in that A Mn according to any one of claims 1 to 7 is used 2+ The Mn 2+ The doped non-spherical silicon oxide composite abrasive grains have a non-spherical structure.

9. A Mn as claimed in claim 8 2+ Application of doped non-spherical silicon oxide composite abrasives, It is characterized in that The polishing liquid for preparing a single crystal silicon carbide wafer specifically comprises: adding potassium permanganate and deionized water into a solution containing Mn 2+ A polishing solution is prepared by ultrasonically mixing the non-spherical silicon oxide composite abrasive grains into a solution, wherein the mass fraction of the silicon oxide composite abrasive grains in the polishing solution is 7.5wt.%, the mass fraction of the potassium permanganate is 1wt.%, and the pH value of the polishing solution is 9.