Preparation method of ultra-thin nickel-silver bimetallic coating of negative electrode of long-circulation metal battery

By preparing an ultrathin nickel-silver bimetallic coating using magnetron sputtering, the problems of cumbersome alloy coating preparation and uncontrollable composition were solved, achieving high-efficiency electrochemical performance and stability of long-life zinc-ion batteries, which are suitable for large-scale production.

CN119040806AActive Publication Date: 2024-11-29UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411169232.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

Existing alloy coating preparation methods are cumbersome, the composition is uncontrollable, and large-scale production is not possible. Furthermore, they have poor chemical stability in alkaline environments and cannot suppress side reactions such as hydrogen evolution and corrosion, resulting in short cycle life of zinc-ion batteries.

Method used

An ultrathin nickel-silver bimetallic coating was prepared by a one-step magnetron sputtering method. By adjusting the content of nickel and silver elements and utilizing a bimetallic synergistic strategy, the hydrogen evolution reaction was suppressed, and the adsorption and corrosion resistance of the negative electrode surface were improved, thus preparing a coating with controllable structure and adjustable composition.

Benefits of technology

A long-life zinc-ion battery with a cycle life of over 6800 hours and a coulombic efficiency of up to 99.7% has been achieved, making it suitable for mass production, reducing costs and improving electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040806A_ABST
    Figure CN119040806A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a long-circulation metal battery negative electrode ultrathin nickel-silver bimetallic coating, which comprises the following steps: 1) cleaning a chamber, loading a zinc foil on a sample table, adjusting the angle between a target material and a substrate, and vacuumizing the chamber by using a mechanical pump and a molecular pump; introducing argon, and removing impurities on the surface of the zinc foil by using an ion source cleaning technology; (2) argon is introduced, a nickel-silver alloy target material is sputtered, or nickel and silver metal target materials are co-sputtered, the power of the two target materials is adjusted to change the content of nickel and silver elements in the bimetallic coating, and nickel and silver bimetals are deposited on the surface of the zinc foil cleaned by the ion source at the same time; 3) standing the obtained nickel-silver bimetallic coating modified zinc foil for a period of time to obtain the component-adjustable nickel-silver bimetallic coating for the negative electrode of the zinc battery; according to the preparation method, zinc is guided to be uniformly deposited on the surface, the sputtering power of the two metal target materials is adjusted by utilizing a magnetron co-sputtering technology, the nickel content and the silver content of the nickel-silver double-metal coating are accurately controlled, and the preparation of the ultra-long-cycle stable metal battery negative electrode is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of secondary metal batteries, and in particular to a method for preparing an ultra-thin nickel-silver bimetallic coating on a negative electrode of a long-cycle metal battery. Background Art

[0002] Batteries are an important part of modern energy storage systems, which can convert electrical energy into chemical energy and store it for release when needed. High energy density, long life, lightweight rechargeable lithium-ion batteries have their own shortcomings such as resource shortage, high cost, harsh preparation conditions, and flammable organic electrolytes. There is an urgent need for a more environmentally friendly and sustainable energy storage device to replace lithium-ion batteries.

[0003] Aqueous zinc-ion batteries have the advantages of being green, safe, stable, and low-cost. As a new generation of energy storage technology, they have attracted much attention. Metal batteries can use aqueous electrolytes, making them very promising in portable electronic devices and ultra-large-scale energy storage systems.

[0004] However, in actual application, some reactions in the aqueous electrolyte solution will affect the metal deposition process, resulting in a decrease in the coulombic efficiency of zinc deposition / stripping and incomplete dissolution of the metal. As a result, metal ions will gradually deposit unevenly on the surface of the metal negative electrode to form needle-like dendrites. As dendrites continue to form and grow, their mechanical rigidity and uneven structure will cause them to fall off the negative electrode surface, resulting in a reduction in the active material of the battery and a decline in capacity. Dendrites may also pierce the diaphragm, causing an internal short circuit in the battery. In addition, the coexistence of active metals and water is thermodynamically unstable. During the electrochemical cycle, hydrogen evolution reactions often occur. Along with the hydrogen evolution reaction, side reactions such as corrosion pits and passivation will also appear on the negative electrode surface, resulting in a decrease in the coulombic efficiency of the battery, battery expansion, and reduced cycle stability.

[0005] The above-mentioned adverse side reactions on the negative electrode surface do not occur independently, but will affect and promote each other. Therefore, it is necessary to construct an artificial modification layer on the negative electrode surface to improve the cycle life of the aqueous metal ion battery by inhibiting the growth of dendrites and the occurrence of side reactions; at the same time, the construction of the negative electrode modification layer makes the electrochemical performance of the whole battery, such as the cycle and capacity retention rate, more stable.

[0006] To address these daunting challenges, metal-based coatings have been used to tune the performance of anodes in metal batteries. The affinity and conductivity of specific metal-based coatings on the anode surface for the anode metal contribute to a more uniform deposition distribution during the charge / discharge cycle of metal batteries. This modification not only facilitates dendrite-free deposition but also suppresses side reactions, thereby improving the safety and stability of metal batteries. Among various metal-based coatings, alloy anodes have been widely explored and implemented. The three-dimensional Ni-Zn anode with a multi-channel lattice structure and a superhydrophilic surface constructed by Zhang et al. can effectively improve the electric field distribution and induce the uniform deposition of metals, thereby inhibiting the growth of dendrites. At the same time, Zheng et al. found that the use of Ag metal coating modification, especially the in-situ generated AgZn 3 The existence of alloy form is of great significance for promoting uniform surface deposition and inhibiting side reactions such as hydrogen evolution.

[0007] At present, research on electrode modification using alloy materials has made certain progress. However, due to limitations in conductive materials, thin film structures and preparation processes, the reliability and stability of existing alloy materials still cannot meet the requirements: 1) Due to the many steps in alloy preparation and the complex composition, it is difficult to precisely control the preparation process and obtain the target sample in one go, thus making large-scale production impossible; 2) The optimization effect of some binary alloy modification layers is limited, and their chemical stability is poor in alkaline environments. They cannot produce good results in inhibiting side reactions such as hydrogen evolution and corrosion, and thus cannot produce long-cycle stable batteries. Summary of the invention

[0008] In view of the above problems, the present invention prepares the coating by a one-step magnetron sputtering method to solve the problems of cumbersome preparation methods and uncontrollable composition of existing alloy coatings; at the same time, a bimetallic synergistic strategy is proposed to utilize the characteristics of different metals to simultaneously enhance the adsorption and corrosion resistance of the negative electrode surface and inhibit the hydrogen evolution reaction, so as to realize the preparation of a metal battery negative electrode with ultra-long cycle stability.

[0009] The present invention adopts the following technical solutions:

[0010] A method for preparing an ultra-thin nickel-silver bimetallic coating for a negative electrode of a long-cycle metal battery comprises: 1) cleaning a chamber, loading a zinc foil on a sample stage, adjusting the angle between a target material and a substrate, and evacuating the chamber with a mechanical pump and a molecular pump; introducing argon gas, and removing impurities on the surface of the zinc foil using an ion source cleaning technology;

[0011] 2) introducing argon gas to sputter a single target of a magnetic metal and a B11 group metal or a bimetallic alloy target; or co-sputter a magnetic metal and a B11 group metal target, adjust the power of the two targets to change the content of nickel and silver elements in the bimetallic coating, and simultaneously deposit the bimetallic on the surface of the zinc foil after being cleaned by the ion source;

[0012] 3) The obtained zinc foil modified with the bimetallic coating is allowed to stand for a period of time to obtain a bimetallic coating with adjustable components for the negative electrode of a zinc battery.

[0013] Furthermore, the magnetic metal is one of Fe, Co and Ni.

[0014] Furthermore, the B11 group metal is one of Cu, Ag and Au.

[0015] Furthermore, in step 1), the angle between the target and the substrate is 60-90°.

[0016] Furthermore, in the step 1), the specific conditions for introducing argon gas and using the ion source cleaning technology can be: the argon gas flow rate is set to 115 sccm, the pressure in the chamber is adjusted to 15 Pa, and the ion source cleaning time is 10 to 20 minutes.

[0017] Further, in step 2), the specific conditions for the single target sputtering of the nickel-silver bimetallic alloy target by introducing argon gas are: introducing argon gas, adjusting the alloy target power to 20-80W, maintaining the sputtering pressure at 0.4Pa, and the sputtering time is 10min; or the specific conditions for co-sputtering the nickel and silver metal targets are: introducing argon gas, with a total gas flow rate of 120sccm; adjusting the nickel metal target power to 20-80W, adjusting the silver target power to 20-80W, maintaining the sputtering pressure at 0.4Pa, and the sputtering time is 10min;

[0018] Furthermore, the thickness of the nickel-silver bimetallic coating is 0.1 to 1 μm;

[0019] Furthermore, the content ratio of nickel to silver elements is 1:15 to 1:4.

[0020] Furthermore, in step 3), the specific time for standing the obtained zinc foil modified with the nickel-silver bimetallic coating is 20 to 60 minutes.

[0021] The beneficial effects of the present invention are:

[0022] 1. The present invention prepares a coating with controllable structure and adjustable components. Silver has a strong adsorption capacity for hydrogen and can effectively inhibit the surface hydrogen evolution reaction. Adding a small amount of nickel into silver can improve the oxidation resistance of the plated metal, reduce the amount of silver used and save costs. The bimetallic synergistic strategy is used to achieve a long-life zinc ion battery with stronger electrochemical performance.

[0023] 2. The present invention is the first to prepare an ultra-thin nickel-silver bimetallic coating with a thickness of about 200 nm on zinc foil by magnetron co-sputtering. This helps to further optimize the electrochemical interface, promote stable electrode / electrolyte interaction, and inhibit harmful side reactions. The symmetrical battery has a current density of 1 mA cm-2 The Ni-Ag-Zn-based symmetric battery exhibits an excellent cycle life of more than 6800 hours with a Coulombic efficiency of 99.7%. For the cycle life at various current densities, the Ni-Ag-Zn-based symmetric battery exceeds most reported binary alloy-based / ternary alloy-based symmetric batteries.

[0024] 3. The one-step preparation method of the present invention can avoid the pretreatment of the negative electrode substrate foil, such as grinding, polishing, chemical treatment, and post-treatment such as annealing. While reducing the steps and improving efficiency, it saves material resources. Different substrates and coatings can be processed in a simple and fast way, which is suitable for large-scale production and manufacturing, and is conducive to industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings of the embodiments will be briefly introduced below. Obviously, the drawings in the following description only relate to some embodiments of the present invention, but are not intended to limit the present invention.

[0026] Figure 1 XRD spectra of negative electrode modified with nickel-silver coating for comparative example;

[0027] Figure 2 For comparison and example, zinc foil was used as the negative electrode of the half-cell at 1 mA cm -2 Coulomb efficiency diagram under current density;

[0028] Figure 3 For the comparison example and the example, zinc foil is used as the negative electrode of the symmetrical battery at 1 mA cm -2 Cycle life diagram under current density;

[0029] Figure 4 The SEM morphology images of the zinc foils of the comparative example and the example 4 after being used in the symmetrical battery for 20 hours and 50 hours of cycling;

[0030] Figure 5 For comparison with Example 4, zinc foil is used in a full battery at 1A·g -1 Charge and discharge cycle diagram under current density; DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] As shown in the figure, the present invention provides a technical solution: a method for preparing an ultra-thin nickel-silver bimetallic coating for a negative electrode of a long-cycle metal battery, comprising:

[0033] Comparative Example 1

[0034] 1. Preparation of blank zinc anode

[0035] A 0.08 mm thick commercial zinc foil was wiped with ethanol and then placed in a vacuum drying oven.

[0036] 2. Activated Carbon Electrode Preparation

[0037] Activated carbon (AC), polyvinylidene fluoride (PVDF) and acetylene black were mixed and ground in a ratio of 8:1:1, and a drop of N-methylpyrrolidone (NMP) was added to disperse the mixture evenly and then coated on a stainless steel mesh. After drying at 80°C overnight, AC / / stainless steel mesh was obtained.

[0038] 3. Characterization of zinc foil phase structure using XRD

[0039] Figure 1 The lower middle curve is the XRD spectrum of blank zinc foil

[0040] 4. Zinc-copper half-cell cycle test

[0041] Figure 2 For the Zn-Cu half-cell cycle test, blank Zn foil and Cu foil were used as negative electrode and positive electrode respectively. -2 , 1mAh cm -2 The cycle test was carried out under the same conditions as that in 2 mol / L ZnSO4. It can be seen from the figure that the half-cell cycle number of the blank zinc foil as the negative electrode is only about 75 times, proving that its stability during the cycle process is poor.

[0042] 5. Zinc-zinc symmetric battery performance test

[0043] The blank zinc foil was assembled into a CR-2032 symmetrical battery for cycle stability test. In the CR-2032 battery, glass fiber was used as the separator of the negative electrode. The electrolyte used was 100 μL of 2 mol / L ZnSO4 solution. The test parameters were set to constant current charge and constant current discharge, with a current density of 1 mA cm -2 . Figure 5 It is proved that the effective cycle time of blank zinc foil under the above current density is about 200h. It can be seen that the blank sample without coating protection fails in a shorter time and has poor stability.

[0044] 6. Observe the structure of zinc foil using SEM

[0045] The blank zinc foil was assembled into a symmetrical battery at 1 mA cm -2 After cycling for 20h and 50h at a current density of Figure 4 It can be seen that a large number of by-products and protruding lamellar dendrites are generated.

[0046] 7.Zn-AC battery performance test

[0047] The blank zinc foil was used as the negative electrode and the AC electrode as the positive electrode to assemble a CR-2032 button battery for full battery cycle performance test. In the CR-2032 battery, glass fiber was used as the positive and negative electrode separators. The electrolyte used was 2 mol / L ZnSO4. The test parameters were set to 1A·g -1 Constant current charging and constant current discharging. Figure 5 This is the charge and discharge curve corresponding to the full battery cycle with blank zinc foil as the negative electrode. When blank zinc foil is used as the negative electrode, the capacity is lower and has a tendency to decay.

[0048] Example 1

[0049] 1. Substrate pretreatment

[0050] (1) Wipe a 0.08 mm thick zinc foil with ethanol and place it in a vacuum drying oven.

[0051] (2) The electrode substrate prepared in step (1) was cut into pieces of 5x5 cm and placed on a sample stage in a chamber of a magnetron sputtering device, and then bombarded and cleaned using an ion source. The chamber pressure was 1.5 Pa, the argon gas flow rate was 112 sccm, and the cleaning process lasted for 10 min.

[0052] 2. Preparation of nickel-silver bimetallic coating

[0053] Confirm that the angle between the nickel target base and the plane is 75°, and use a mechanical pump and a molecular pump to evacuate the chamber to a vacuum of ≤1.0×10 - 3 Pa; introduce Ar gas with a flow rate set to 120sccm, and adjust the deposition pressure in the chamber to 0.4Pa; adjust the power of the nickel metal and silver metal targets to 40W, and perform pre-sputtering for 5 minutes; after the pre-sputtering is completed, open the baffle, rotate the sample stage, keep the power and gas pressure unchanged, and sputter for 10 minutes to obtain a coating with a thickness of about 200nm, in which the nickel-silver content ratio is about 1:10.

[0054] 3. Zinc-copper half-cell cycle test

[0055] Figure 2 For the zinc-copper half-cell cycle test, the zinc foil and copper foil coated with the coating prepared in step 2 were used as the negative electrode and the positive electrode, respectively. -2 , 1mAh cm -2 The cycle test was carried out under the conditions of 2 mol / L ZnSO4. It can be seen from the figure that the zinc-copper battery with the zinc foil prepared in step 2 as the negative electrode can be stably cycled for more than 300 times.

[0056] 4. Zinc-zinc symmetric battery performance test

[0057] The blank zinc foil was assembled into a CR-2032 symmetrical battery for cycle stability test. In the CR-2032 battery, glass fiber was used as the separator of the negative electrode. The electrolyte used was 100 μL of 2 mol / L ZnSO4 solution. The test parameters were set to constant current charge and constant current discharge, with a current density of 1 mA cm -2 . Figure 5 It is proved that the effective cycle time of blank zinc foil at the above current density reaches 6800h, which shows that the nickel-silver bimetallic coating greatly improves the cycle stability of the battery.

[0058] Example 2

[0059] 5. Substrate pretreatment

[0060] (3) Wipe a 0.08 mm thick zinc foil with ethanol and place it in a vacuum drying oven.

[0061] (4) The electrode substrate prepared in step (1) was cut into pieces of 5x5 cm and placed on the sample stage in the chamber of the magnetron sputtering equipment, and then bombarded and cleaned with an ion source. The chamber pressure was 1.5 Pa, the argon gas flow rate was 112 sccm, and the cleaning time was 10 min.

[0062] 6. Preparation of nickel-silver bimetallic coating

[0063] Confirm that the angle between the nickel target base and the plane is 65°, and use a mechanical pump and a molecular pump to evacuate the chamber to a vacuum of ≤1.0×10 - 3 Pa; introduce Ar gas with a flow rate set to 120 sccm, and adjust the deposition pressure in the chamber to 0.4 Pa; adjust the power of the nickel metal and silver metal targets to 40 W, and perform pre-sputtering for 5 minutes; after the pre-sputtering is completed, open the baffle, rotate the sample stage, keep the power and gas pressure unchanged, and sputter for 10 minutes to obtain a coating with a thickness of about 200 nm, in which the nickel-silver content ratio is about 1:4.

[0064] 7. Zinc-copper half-cell cycle test

[0065] Figure 2 For the zinc-copper half-cell cycle test, the zinc foil and copper foil coated with the coating prepared in step 2 were used as the negative electrode and the positive electrode, respectively. -2 , 1mAh cm -2 The cycle test was carried out under the conditions of 2 mol / L ZnSO4. It can be seen from the figure that the zinc-copper battery with the zinc foil prepared in step 2 as the negative electrode can be stably cycled for more than 300 times.

[0066] 8. Zinc-zinc symmetric battery performance test

[0067] The blank zinc foil was assembled into a CR-2032 symmetrical battery for cycle stability test. In the CR-2032 battery, glass fiber was used as the separator of the negative electrode. The electrolyte used was 100 μL of 2 mol / L ZnSO4 solution. The test parameters were set to constant current charge and constant current discharge, with a current density of 1 mA cm -2 . Figure 5 It is proved that the effective cycle time of blank zinc foil at the above current density reaches 6800h, which shows that the nickel-silver bimetallic coating greatly improves the cycle stability of the battery.

[0068] Example 3

[0069] 1. Substrate pretreatment

[0070] (1) Wipe a 0.08 mm thick zinc foil with ethanol and place it in a vacuum drying oven.

[0071] (2) The electrode substrate prepared in step (1) was cut into pieces of 5x5 cm and placed on a sample stage in a chamber of a magnetron sputtering device, and then bombarded and cleaned using an ion source. The chamber pressure was 1.5 Pa, the argon gas flow rate was 112 sccm, and the cleaning process lasted for 10 min.

[0072] 2. Activated Carbon Electrode Preparation

[0073] Activated carbon (AC), polyvinylidene fluoride (PVDF) and acetylene black were mixed and ground in a ratio of 8:1:1, and a drop of N-methylpyrrolidone (NMP) was added to disperse the mixture evenly and then coated on a stainless steel mesh. After drying at 80°C overnight, AC / / stainless steel mesh was obtained.

[0074] 3. Preparation of nickel-silver bimetallic coating

[0075] Confirm that the angle between the target base and the plane is 85°, and use a mechanical pump and a molecular pump to evacuate the chamber to a vacuum of ≤1.0×10 -3 Pa; introduce Ar gas with a flow rate set to 120sccm, and adjust the deposition pressure in the chamber to 0.4Pa; adjust the power of the nickel metal and silver metal targets to 40W, and perform pre-sputtering for 5min; after the pre-sputtering is completed, open the baffle, rotate the sample stage, keep the power and gas pressure unchanged, and sputter for 10min to obtain a coating with a thickness of about 200nm, in which the nickel-silver content ratio is about 1:14.

[0076] 4. Characterization of the Ni-Ag-Zn negative electrode phase structure using XRD

[0077] Figure 1 The upper middle curve is the XRD spectrum of the nickel-silver-zinc negative electrode

[0078] 5. Zinc-copper half-cell cycle test

[0079] Figure 2For the zinc-copper half-cell cycle test, the zinc foil and copper foil coated with the coating prepared in step 3 were used as the negative electrode and the positive electrode, respectively. -2 , 1mAh cm -2 The cycle test was carried out under the conditions of 2 mol / L ZnSO4. It can be seen from the figure that the zinc-copper battery with the zinc foil prepared in step 2 as the negative electrode can be stably cycled for more than 300 times, and the coulombic efficiency is as high as 99.7%.

[0080] 6. Zinc-zinc symmetric battery performance test

[0081] The blank zinc foil was assembled into a CR-2032 symmetrical battery for cycle stability test. In the CR-2032 battery, glass fiber was used as the separator of the negative electrode. The electrolyte used was 100 μL of 2 mol / L ZnSO4 solution. The test parameters were set to constant current charge and constant current discharge, with a current density of 1 mA cm -2 . Figure 5 It is proved that the effective cycle time of the blank zinc foil at the above current density reaches 6800h. It can be seen that when the ratio of nickel-silver bimetallic is 1:14, the prepared coating greatly improves the cycle stability of the battery.

[0082] 7. Observe the structure of zinc foil using SEM

[0083] Figure 4 The SEM morphology of the zinc foil prepared in step 2 after cyclic charging and discharging in a symmetrical battery is compared with the blank zinc foil reacted under the same conditions in comparative example 1. Zinc is uniformly deposited on the surface of nickel-silver without obvious dendrites and corrosion pits.

[0084] 8. Nickel silver zinc-AC battery performance test

[0085] The zinc foil modified with nickel silver coating was used as the negative electrode and the AC electrode as the positive electrode to assemble into a CR-2032 button battery for full battery cycle performance test. In the CR-2032 battery, glass fiber was used as the positive and negative electrode separators. The electrolyte used was 2 mol / L ZnSO4. The test parameters were set to 1A·g -1 Constant current charging and constant current discharging. Figure 5 This is the charge and discharge curve corresponding to the full battery cycle with zinc foil modified with nickel-silver coating as the negative electrode. The capacity is higher when blank zinc foil is used as the negative electrode and has not decayed after 20,000 cycles.

[0086] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing an ultra-thin nickel-silver bimetallic coating for a negative electrode of a long-cycle metal battery, characterized in that: The method comprises: 1) cleaning the chamber, loading the zinc foil on the sample stage, adjusting the angle between the target material and the substrate to 60-90 degrees, evacuating the chamber with a mechanical pump and a molecular pump; introducing argon gas, and removing impurities on the surface of the zinc foil by using an ion source cleaning technology; 2) introducing argon gas, sputtering a single target of a magnetic metal and a B11 group metal, or a bimetallic alloy target material; or co-sputtering a magnetic metal and a B11 group metal target material, adjusting the power of the two targets to change the content of the magnetic metal element and the B11 group metal element in the bimetallic coating, and simultaneously depositing the bimetal on the surface of the zinc foil after being cleaned by the ion source; 3) letting the obtained zinc foil modified by the bimetallic coating stand for a period of time to obtain a bimetallic coating with adjustable components for the negative electrode of a zinc battery.

2. The method for preparing an ultra-thin nickel-silver bimetallic coating for a negative electrode of a long-cycle metal battery according to claim 1, characterized in that: The magnetic metal is one of Fe, Co and Ni.

3. The method for preparing an ultra-thin nickel-silver bimetallic coating for a negative electrode of a long-cycle metal battery according to claim 1, characterized in that: The B11 group metal is one of Cu, Ag and Au.

4. The method for preparing an ultra-thin nickel-silver bimetallic coating for a negative electrode of a long-cycle metal battery according to claim 1, characterized in that: In the step 1), the angle between the target and the substrate is 60-90°.

5. The method for preparing an ultra-thin nickel-silver bimetallic coating for a negative electrode of a long-cycle metal battery according to claim 4, characterized in that: In the step 1), argon gas is introduced, and the specific conditions of using the ion source cleaning technology can be: the argon gas flow rate is set to 115 sccm, the pressure in the chamber is adjusted to 15 Pa, and the ion source cleaning time is 10 to 20 minutes.

6. The method for preparing an ultra-thin nickel-silver bimetallic coating for a negative electrode of a long-cycle metal battery according to claim 5, characterized in that: In step 2), the specific conditions for introducing argon gas and co-sputtering nickel and silver metal targets are: introducing argon gas; adjusting the power of the nickel metal target to 20-80W, the power of the silver target to 20-80W, maintaining the sputtering pressure at 0.4Pa, and the sputtering time is 10min.

7. The method for preparing an ultra-thin nickel-silver bimetallic coating for a negative electrode of a long-cycle metal battery according to claim 1, characterized in that: The thickness of the nickel-silver bimetallic coating is 0.1-1 μm.

8. The method for preparing an ultra-thin nickel-silver bimetallic coating for a negative electrode of a long-cycle metal battery according to claim 7, characterized in that: The content ratio of nickel to silver elements is 1:15 to 1:

4.

9. The method for preparing an ultra-thin nickel-silver bimetallic coating for a negative electrode of a long-cycle metal battery according to claim 9, characterized in that: In step 3), the specific time for standing the obtained zinc foil modified with the nickel-silver bimetallic coating is 20 to 60 minutes.

Citation Information

Patent Citations

  • Zinc-based battery negative electrode and preparation and application thereof

    CN111224115A

  • Water-based rechargeable zinc ion battery alloy type negative electrode material and preparation method and application thereof

    CN111916720A

  • Application of metal material and zinc-based battery taking metal material as negative electrode

    CN112164802A

  • High-discharge-depth zinc negative electrode and preparation method and application thereof

    CN117096256A