Wear-resistant insulating composite coating on surface of electromagnetic pure iron and preparation method of wear-resistant insulating composite coating
By forming a composite coating of TiN inner layer and Al2O3 outer layer on the surface of electromagnetic pure iron, it solves its easy wear and non-insulating problems, improves wear resistance and insulation performance, extends service life and expands the application field.
Patent Information
- Application Number
- CN202310603664.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
AI Technical Summary
Electromagnetic pure iron materials are prone to wear due to low hardness, and the existing surface reinforcement process cannot effectively improve its insulation performance, limiting its application in electrical appliances and communication systems.
The composite coating of TiN inner layer and Al2O3 outer layer was used to form TiN inner layer and Al2O3 outer layer on the surface of electromagnetic pure iron by chemical vapor precipitation. It has strong bonding force, good wear resistance and insulation performance, and the total thickness is 10μm-25μm. .
It significantly improves the wear resistance and insulation properties of electromagnetic pure iron, extends its service life, and expands its application range in electronics, electrical appliances, aerospace and other fields.
Smart Images

Figure CN119028696A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wear-resistant insulating coatings, and in particular relates to a wear-resistant insulating composite coating on the surface of electromagnetic pure iron and a preparation method thereof. Background Art
[0002] Electromagnetic pure iron is a high-quality steel with an iron content of more than 99.5%. Its components have low carbon, sulfur and phosphorus contents. It has the characteristics of high magnetic induction intensity, low price and simple heat treatment process. It is currently widely used as a soft magnetic material, such as the shell, armature, valve core, movable iron core and other parts of the solenoid valve. However, due to the extremely low content of alloy elements contained in electromagnetic pure iron materials, which is almost zero, and the absence of alloy strengthening phases, its hardness is extremely low. As a structural part or transmission part material, it often suffers from severe material wear due to mutual friction between workpieces, which greatly reduces the service life of the material. In addition, in recent years, soft magnetic materials represented by electromagnetic pure iron have gradually been applied to the fields of electrical circuits and communication systems, and their excellent magnetic properties are often limited by their conductivity. Therefore, improving the wear resistance and insulation properties of electromagnetic pure iron materials is an urgent problem to be solved.
[0003] Existing process methods such as surface nitriding can only improve the wear resistance of electromagnetic pure iron, but cannot achieve insulation protection. At the same time, the surface nitriding process has defects such as thin strengthening layer and weak strengthening effect, and its improvement on the wear resistance of electromagnetic pure iron is still limited.
[0004] Therefore, in response to the current problems of easy wear and non-insulation faced by electromagnetic pure iron, the field urgently needs to develop a coating with dense and uniform, strong bonding, good wear resistance and insulation properties and its preparation method, so as to overcome the shortcomings of the existing surface strengthening process such as thin strengthening layer, poor wear resistance and non-insulation, improve the wear resistance of electromagnetic pure iron and achieve insulation performance, and further expand the application of electromagnetic pure iron. Summary of the invention
[0005] The purpose of the present invention is to provide a wear-resistant insulating composite coating on the surface of electromagnetic pure iron and a preparation method thereof, so as to solve the technical problems that the surface of the existing electromagnetic pure iron is easy to wear and not insulated.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] In the first aspect, a wear-resistant insulating composite coating on the surface of electromagnetic pure iron comprises a TiN inner layer and an Al 2 O 3 The outer layer, the TiN inner layer is used to wrap the outer side of the electromagnetic pure iron, and the outer side of the TiN inner layer is wrapped with Al 2 O 3 Outer layer.
[0008] A further improvement of the present invention is that: the TiN inner layer and the Al 2 O 3 The total thickness of the outer layer is 10 μm-25 μm.
[0009] In a second aspect, a method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron comprises the following steps:
[0010] A nitrogen source, a titanium source and an auxiliary gas are introduced into the substrate, and a TiN inner layer is formed on the surface of the substrate by a chemical vapor deposition method;
[0011] Aluminum source, reaction gas and auxiliary gas are introduced into the substrate, and Al is generated on the outside of the TiN inner layer by chemical vapor deposition. 2 O 3 Outer layer.
[0012] A further improvement of the present invention is that the substrate is pre-treated in advance, and the pre-treatment includes grinding, cleaning, sandblasting and vacuum drying in sequence.
[0013] A further improvement of the present invention is that the step of introducing a nitrogen source, a titanium source and an auxiliary gas into the substrate and forming a TiN inner layer on the surface of the substrate by chemical vapor deposition specifically includes:
[0014] placing the substrate into a CVD furnace;
[0015] evacuating the CVD furnace to a first pressure;
[0016] Introducing an auxiliary gas into the CVD furnace, and heating the CVD furnace to a first temperature at a first heating rate;
[0017] A nitrogen source, an auxiliary gas and a titanium source are introduced into the CVD furnace, and a TiN inner layer is deposited on the surface of the substrate.
[0018] A further improvement of the present invention is that: an aluminum source, a reaction gas and an auxiliary gas are introduced into the substrate, and an Al2O3 layer is formed on the outside of the TiN inner layer by chemical vapor deposition. 2 O 3 The outer steps specifically include:
[0019] heating the CVD furnace to a second temperature;
[0020] Aluminum source, reaction gas and auxiliary gas are introduced into the CVD furnace, and Al is deposited on the outside of the TiN inner layer. 2 O 3 Outer layer.
[0021] A further improvement of the present invention is that it also includes a cooling step, and the cooling step specifically includes:
[0022] Stop introducing the aluminum source and the reaction gas, and reduce the volume flow rate of the auxiliary gas to a sixth volume flow rate;
[0023] The CVD furnace is cooled to a third temperature at a first cooling rate, and the auxiliary gas volume flow rate is reduced again to a seventh volume flow rate;
[0024] When the CVD furnace is cooled to the fourth temperature, the introduction of hydrogen is stopped to allow the CVD to cool to room temperature.
[0025] A further improvement of the present invention is that the titanium source is one or more combinations of butyl titanate, titanium tetrachloride, titanium trichloride, titanium dichloride, titanium chloride and / or titanium powder.
[0026] A further improvement of the present invention is that the aluminum source is one or more combinations of aluminum powder, aluminum ingot, aluminum trichloride and / or aluminum pentachloride.
[0027] A further improvement of the present invention is that: the nitrogen, argon and / or hydrogen are one or more combinations.
[0028] Compared with the prior art, the present invention has at least the following beneficial effects:
[0029] 1. The present invention wraps a TiN inner layer on the outside of the electromagnetic pure iron as a transition layer to alleviate the electromagnetic pure iron and Al 2 O 3 The thermal expansion coefficient of the outer layer is mismatched, and the bonding strength between the coating and the substrate is enhanced; Al 2 O 3 The outer layer can effectively reduce the wear of the coating and give the base material excellent insulation properties. The composite coating is dense and uniform, with a controllable structure, and has the advantages of strong bonding, wear resistance, and good insulation performance. It can significantly improve the wear resistance and insulation performance of electromagnetic pure iron, extend its service life and expand its application field;
[0030] 2. The present invention has little effect on the dimensional accuracy of the electromagnetic pure iron substrate, and the substrate shape has good adaptability, which is suitable for the fields of electronics, electrical appliances, aerospace, etc. The coating has low production cost, simple process, strong controllability, and is suitable for industrial production;
[0031] 3. The present invention removes excess impurities by pre-treating the substrate to improve the coating quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0033] In the attached picture:
[0034] Figure 1This is a flow chart of a method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron according to the present invention;
[0035] Figure 2 The nano-TiN / Al composite on the surface of DT-4 electromagnetic pure iron prepared in Example 3 2 O 3 XRD test pattern of wear-resistant insulating composite coating.
[0036] Figure 3 This is a surface SEM test image of the TiN inner layer in the wear-resistant insulating composite coating on the surface of electromagnetic pure iron prepared in Example 3;
[0037] Figure 4 The Al in the wear-resistant insulating composite coating on the surface of electromagnetic pure iron prepared in Example 3 2 O 3 Surface SEM image of the outer layer;
[0038] Figure 5 This is a cross-sectional SEM test image of a wear-resistant insulating composite coating on the surface of electromagnetic pure iron prepared in Example 3.
[0039] Figure 6 This is a bonding strength test diagram of a wear-resistant insulating composite coating on the surface of electromagnetic pure iron prepared in Example 3.
[0040] Figure 7 This is a test chart of the friction coefficient of a wear-resistant insulating composite coating on the surface of electromagnetic pure iron prepared in Example 3.
[0041] Figure 8 This is a test chart of the average wear rate of an electromagnetic pure iron surface wear-resistant insulating composite coating prepared in Example 3.
[0042] Fig. 9 This is a test diagram of the insulation performance of an electromagnetic pure iron surface wear-resistant insulating composite coating prepared in Example 3. DETAILED DESCRIPTION
[0043] The present invention will be described in detail below with reference to the accompanying drawings and in combination with embodiments. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict.
[0044] The following detailed description is an exemplary description, which is intended to provide further detailed description of the present invention. Unless otherwise specified, all technical terms used in the present invention have the same meaning as those generally understood by those skilled in the art to which the present invention belongs. The terms used in the present invention are only for describing specific embodiments, and are not intended to limit the exemplary embodiments according to the present invention.
[0045] Example 1
[0046] A wear-resistant insulating composite coating on the surface of electromagnetic pure iron, comprising a TiN inner layer and an Al 2 O 3 The outer layer, the surface of the electromagnetic pure iron is wrapped with a layer of TiN inner layer, and the outer side of the TiN inner layer is wrapped with a layer of Al 2 O 3 Outer layer.
[0047] Specifically, the TiN inner layer is a transition layer, which relieves the Al 2 O 3 The thermal expansion coefficient mismatch between the electromagnetic pure iron and the electromagnetic pure iron also improves the bonding strength between the two.
[0048] Specifically, Al 2 O 3 The outer layer can effectively reduce the wear of the coating and at the same time has excellent insulation properties, which can meet the insulation performance requirements of electromagnetic pure iron.
[0049] Specifically, the TiN inner layer is composed of nano-sized rice-grain TiN grains with a size of 50nm-300nm.
[0050] Preferably, the nano-scale rice-grained TiN grain size in the TiN inner layer is 100nm-200nm.
[0051] Specifically, Al 2 O 3 The outer layer is composed of nano-sized bulk Al 2 O 3 The grain size is 250nm-550nm.
[0052] Preferably, Al 2 O 3 Nano-sized bulk Al in the outer layer 2 O 3 The grain size is 300nm-400nm.
[0053] Specifically, the TiN inner layer and the Al 2 O 3 The total thickness of the outer layer is 10 μm-25 μm.
[0054] Preferably, the TiN inner layer and the Al 2 O 3 The total thickness of the outer layer is 14 μm-18 μm.
[0055] Specifically, the TiN inner layer and the Al 2 O 3 The friction coefficient of the outer layer ranges from 0.28 to 0.32.
[0056] Specifically, the TiN inner layer and the Al 2 O 3The average wear rate of the outer layer is 1.6×10 -7 mm 3 N -1 m -1 -1.9×10 -7 mm 3 N - 1 m -1 .
[0057] Specifically, the TiN inner layer and the Al 2 O 3 The bonding force of the outer layer is 80N-125N.
[0058] Specifically, the TiN inner layer and the Al 2 O 3 The resistance of the outer layer after bonding is 1.7×10 13 Ω-2×10 13 Ω.
[0059] Example 2
[0060] A method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron, such as Figure 1 As shown, the following steps are included:
[0061] A nitrogen source, a titanium source and an auxiliary gas are introduced into the substrate, and a TiN inner layer is formed on the surface of the substrate by a chemical vapor deposition method;
[0062] Aluminum source, reaction gas and auxiliary gas are introduced into the substrate, and Al is generated on the outside of the TiN inner layer by chemical vapor deposition. 2 O 3 Outer layer.
[0063] Specifically, the matrix includes but is not limited to one or more combinations of stainless steel, cemented carbide or electromagnetic pure iron, and electromagnetic pure iron is preferred as the matrix.
[0064] Specifically, before the step of introducing nitrogen source, titanium source and auxiliary gas into the substrate and forming a TiN inner layer on the substrate surface by chemical vapor deposition method begins, pretreatment is required, and the pretreatment includes polishing, cleaning, sandblasting and vacuum drying in sequence.
[0065] Specifically, the grinding step in the pretreatment is used to remove impurities from the surface of the substrate.
[0066] Specifically, during the sandblasting step in the substrate pretreatment, one or more combinations of white corundum sand (aluminum oxide sand), brown corundum sand and / or quartz sand are used.
[0067] As a preferred real-time method of this embodiment, white corundum sand is selected in the sandblasting step, and the particle size of the white corundum sand is 200 mesh-500 mesh.
[0068] Specifically, the cleaning step in the substrate pretreatment is ultrasonic cleaning, which effectively removes residual sand on the substrate surface to prevent spots, local shedding or point defects during the coating preparation process. In the cleaning step, one or more combinations of alcohol, acetone, deionized water and / or distilled water are selected as cleaning agents. The cleaning agents are not limited to one or more combinations mentioned above. The duration of the cleaning step is 60min-120min.
[0069] Specifically, the cleaning agent is preferably acetone and / or alcohol, or a combination of both.
[0070] Specifically, the temperature of the vacuum drying step is 60°C-80°C, and the vacuum degree is 10 -2 Pa-10 -1 Pa, the processing time of the vacuum drying step is 20min-60min.
[0071] Specifically, the step of introducing a nitrogen source, a titanium source and an auxiliary gas into a substrate and forming a TiN inner layer on the surface of the substrate by chemical vapor deposition comprises:
[0072] placing the substrate into a CVD furnace;
[0073] evacuating the CVD furnace to a first pressure;
[0074] Introducing an auxiliary gas into the CVD furnace, and heating the CVD furnace to a first temperature at a first heating rate;
[0075] A nitrogen source, an auxiliary gas and a titanium source are introduced into the CVD furnace, and a TiN inner layer is deposited on the surface of the substrate.
[0076] Specifically, the CVD furnace is a chemical vapor deposition furnace;
[0077] Specifically, the first pressure is 10 -3 Pa-10 -1 Pa.
[0078] Specifically, the titanium source is one or more combinations of butyl titanate, titanium tetrachloride, titanium trichloride, titanium dichloride, titanium chloride and / or titanium powder;
[0079] Specifically, the auxiliary gas is one or more combinations of nitrogen, argon and / or hydrogen;
[0080] Specifically, the nitrogen source is one or more combinations of nitrogen, ammonia, nitrogen dioxide and / or nitric oxide;
[0081] The titanium source is preferably titanium tetrachloride; the nitrogen source is preferably nitrogen; the auxiliary gas is preferably a combination of hydrogen and argon;
[0082] Specifically, in the step of introducing an auxiliary gas into the CVD furnace and heating the CVD furnace to a first temperature at a first heating rate, the auxiliary gas is introduced into the CVD furnace at a first volume flow rate;
[0083] The first volume flow rate is 400 sccm-1300 sccm;
[0084] The first heating rate is 5°C / min-8°C / min;
[0085] The first temperature is 900°C-1050°C;
[0086] Specifically, in the step of introducing an auxiliary gas into the CVD furnace and heating the CVD furnace to a first temperature at a first heating rate, in the step of introducing the auxiliary gas into the CVD furnace at a first volume flow rate, the auxiliary gas is a mixture of hydrogen and argon, wherein the volume flow rate of the hydrogen is 200 sccm-500 sccm, and the volume flow rate of the argon is 200 sccm-800 sccm;
[0087] Specifically, in the step of introducing a nitrogen source, an auxiliary gas and a titanium source into a CVD furnace, and depositing a TiN inner layer on the surface of the substrate, the nitrogen source is introduced into the CVD furnace at a second volume flow rate, the auxiliary gas is introduced into the CVD furnace at a third volume flow rate, and the titanium source is carried into the CVD furnace by the auxiliary gas;
[0088] The second volume flow rate is 1000 sccm-2000 sccm;
[0089] The third volume flow rate is 1500sccm-2500sccm;
[0090] Specifically, in the step of introducing a nitrogen source, an auxiliary gas and a titanium source into a CVD furnace and depositing a TiN inner layer on the surface of the substrate, the time required for depositing the TiN inner layer is a first deposition time, and the first deposition time is 120 min-240 min;
[0091] The first deposition time is preferably 150 min-200 min;
[0092] The first deposition time is preferably 160 min-180 min.
[0093] Specifically, an aluminum source, a reaction gas, and an auxiliary gas are introduced into the substrate, and an Al2O3 layer is formed on the outside of the TiN inner layer by chemical vapor deposition. 2 O 3 The outer layer steps include the following steps:
[0094] heating the CVD furnace to a second temperature;
[0095] Aluminum source, reaction gas and auxiliary gas are introduced into the CVD furnace, and Al is deposited on the outside of the TiN inner layer.2 O 3 Outer layer.
[0096] Specifically, the aluminum source is one or more combinations of aluminum powder, aluminum ingot, aluminum trichloride and / or aluminum pentachloride;
[0097] The aluminum source is preferably aluminum trichloride.
[0098] Specifically, the reaction gas is one or more combinations of carbon monoxide, carbon dioxide, oxygen and / or water vapor;
[0099] The reaction gas is preferably a mixed gas of carbon monoxide and carbon dioxide.
[0100] Specifically, an aluminum source, a reaction gas, and an auxiliary gas are introduced into a CVD furnace, and Al is deposited on the outside of the TiN inner layer. 2 O 3 In the outer layer step, the auxiliary gas is introduced into the CVD furnace at a fourth volume flow rate, the reaction gas is introduced into the CVD furnace at a fifth volume flow rate, and the aluminum source is introduced into the CVD furnace using the auxiliary gas as a carrier;
[0101] The fourth volume flow rate is 800 sccm-1500 sccm;
[0102] The fifth volume flow rate is 1000sccm-3000sccm;
[0103] Specifically, the second temperature is 950°C-1050°C;
[0104] Specifically, the second temperature is greater than the first temperature.
[0105] Specifically, an aluminum source, a reaction gas, and an auxiliary gas are introduced into a CVD furnace, and Al is deposited on the outside of the TiN inner layer. 2 O 3 In the outer layer step, Al is deposited on the outside of the TiN inner layer. 2 O 3 The time required in the process of the outer layer is the second deposition time, and the second deposition time is 240 min-480 min, preferably 300 min-450 min.
[0106] Specifically, an aluminum source, a reaction gas, and an auxiliary gas are introduced into a CVD furnace, and Al is deposited on the outer side of the TiN inner layer. 2 O 3 After the outer layer step is completed, a cooling step is also included;
[0107] The cooling step specifically includes:
[0108] Stop introducing the aluminum source and the reaction gas, and reduce the volume flow rate of the auxiliary gas to a sixth volume flow rate;
[0109] The CVD furnace is cooled to a third temperature at a first cooling rate, and the auxiliary gas volume flow rate is reduced again to a seventh volume flow rate;
[0110] When the CVD furnace is cooled to the fourth temperature, the introduction of hydrogen is stopped to allow the CVD to cool to room temperature.
[0111] Specifically, the sixth volume flow rate is 300 sccm-500 sccm;
[0112] The first cooling rate is 3℃ / min-5℃ / min;
[0113] The third temperature is 400°C-450°C;
[0114] The seventh volume flow rate is 100 sccm-300 sccm;
[0115] The fourth temperature is 50°C-100°C.
[0116] Specifically, the titanium source refers to a raw material that provides the titanium element in the coating.
[0117] Aluminum source refers to the raw material that provides aluminum element in the coating.
[0118] Example 3
[0119] A method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron comprises the following steps:
[0120] DT-4 with a size of 10mm*10mm*5mm is used as the substrate;
[0121] The substrate surface was polished and cleaned, and quartz sand was used for surface blasting. After blasting, acetone was used as a cleaning agent for ultrasonic cleaning. -2 -10 -1 Pa, vacuum dried at 60-80℃ for 40min and then placed in a CVD furnace;
[0122] The CVD furnace was evacuated to 10 -2 Pa, then hydrogen and argon are introduced simultaneously, with a hydrogen flow rate of 200 sccm and an argon flow rate of 200 sccm. The CVD furnace heating program is started, the heating rate is set to 8°C / min, and the deposition temperature is set to 1015°C.
[0123] The CVD device was heated to 1015°C to enter the coating deposition process, and titanium tetrachloride, nitrogen and auxiliary gases were introduced. The nitrogen flow rate was 1500 sccm, and the deposition time was 180 min. Titanium tetrachloride was carried into the CVD device with hydrogen as the auxiliary gas, and the hydrogen flow rate was 2000 sccm.
[0124] After the TiN inner layer is deposited, the Al 2 O3 During the outer layer preparation stage, the CVD furnace was heated to 1020°C to enter the coating deposition process, and aluminum chloride, carbon dioxide, carbon monoxide and auxiliary gas were introduced. The carbon dioxide flow rate was 500 sccm, the carbon monoxide flow rate was 200 sccm, and the deposition time was 300 minutes. Aluminum chloride was carried into the CVD device with hydrogen as the auxiliary gas, and the hydrogen flow rate was 1600 sccm.
[0125] Al 2 O 3 After the outer layer deposition is completed, the CVD device enters a controllable cooling mode, stops introducing the aluminum source and the reaction gas, reduces the hydrogen flow rate to 300-500sccm, and cools to 400-450°C at a cooling rate of 3-5°C / min. After that, the hydrogen flow rate is reduced to 100-300sccm. When the temperature drops to 50-100°C, stop introducing hydrogen, and then cool to room temperature. A wear-resistant insulating composite coating on the surface of electromagnetic pure iron is obtained.
[0126] The wear-resistant insulating composite coating on the surface of the electromagnetic pure iron prepared in Example 3 is as follows Figure 2-5 As shown, Figure 2 This is the XRD test diagram of the wear-resistant insulating composite coating on the surface of electromagnetic pure iron. Figure 2 It can be seen that the wear-resistant insulating composite coating on the surface of electromagnetic pure iron is composed of TiN phase and Al 2 O 3 Phase composition;
[0127] according to Figure 3 It can be seen that the surface of the TiN inner layer is dense and uniform, and the coating is composed of TiN grains with a rice-like appearance, which are aggregated and piled together. The grain size is 100-200nm.
[0128] according to Figure 4 It can be seen that Al 2 O 3 The outer surface is dense and uniform, and the coating is composed of Al with a block shape. 2 O 3 Grain composition, grain size is 300-400nm.
[0129] according to Figure 5 It can be seen that TiN / Al 2 O 3 The wear-resistant insulating composite coating is tightly bonded to the substrate, and the coating thickness is 14-18μm.
[0130] The wear-resistant insulating composite coating on the surface of the electromagnetic pure iron prepared in Example 3 was tested, including: coating bonding performance test, friction performance test, wear performance test and insulation performance test;
[0131] Specifically, the coating bonding performance test adopts the Revetest scratch test system, through the Rockwell round diamond tip, the curvature radius is 0.2mm, the scratch length is 3mm, the scratch rate is 3mm / min, the test load range is 1N~150N, and the loading rate is 99N / min. Each sample is tested 3 times, and the average value of the results is taken.
[0132] Coating bonding performance test results:
[0133] like Figure 6 As shown, the bonding force of the wear-resistant insulating composite coating on the surface of the electromagnetic pure iron obtained in Example 3 is 118.5N.
[0134] Specifically, the friction performance test uses an Rtec friction and wear tester. The test mode is: a 6mm SiC ball is used to perform XY bidirectional linear non-lubricated reciprocating friction on the sample at room temperature. The specific test parameters are: normal load 5-20N, friction speed 20mm / s, friction distance 5mm, time 20min, frequency 2Hz. Each sample is tested 3 times and the average value of the results is taken.
[0135] Friction performance test results:
[0136] like Figure 7 As shown, the friction coefficient of the wear-resistant insulating composite coating on the surface of the electromagnetic pure iron obtained in Example 3 is 0.28.
[0137] Specifically, the wear performance test of the Rtec friction and wear tester firstly conducts a wear scar volume test through a surface profiler to obtain the wear scar volume data; secondly, the wear scar volume data is integrated and calculated through analysis software to obtain the wear scar volume value; finally, the wear rate is calculated according to the wear rate calculation formula:
[0138]
[0139] Where, W: volume wear rate; V: wear volume; S: load size; L: total friction distance.
[0140] Wear performance test results:
[0141] like Figure 8 As shown in the figure, the average wear rate of the wear-resistant insulating composite coating on the surface of the electromagnetic pure iron obtained in Example 3 is 1.6×10 -7 mm 3 N -1 m -1 .
[0142] Specifically, the insulation performance test uses a Keithley power meter model 4200-SCS / F to test the maximum resistance of the material by continuously increasing the voltage until the material is broken down. The maximum resistance value when the material is broken down is used to characterize the insulation performance of the material.
[0143] Insulation performance test results:
[0144] like Fig. 9 As shown, the resistance of the wear-resistant insulating composite coating on the surface of the electromagnetic pure iron obtained in Example 3 is 2×10 13 Ω.
[0145] Example 4
[0146] A method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron, wherein the deposition temperature of the TiN inner layer is modified to 1000°C, and the other parameters remain unchanged. After the preparation is completed, the coating bonding performance test, friction performance test, wear performance test and insulation performance test are performed again;
[0147] The test results show that the surface of the TiN inner layer is dense and uniform, and the TiN layer grains show a rice-like structure; the size of the rice-like grains is 200-250nm; the bonding force of the composite coating is 110N; the friction coefficient of the composite coating is 0.30, and the average wear rate is 1.8×10 -7 mm 3 N -1 m -1 ; The maximum resistance of the composite coating is 1.8×10 13 Ω.
[0148] Example 5
[0149] A method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron, wherein the titanium source is changed to titanium trichloride, and other parameters remain unchanged. After the preparation is completed, the coating bonding performance test, friction performance test, wear performance test and insulation performance test are performed again;
[0150] The test results show that the composite coating is dense and uniform, the surface of the TiN inner layer is dense and uniform, and the TiN layer grains show a rice-like structure; the size of the rice-like grains is 230-300nm; the bonding force of the composite coating is 109N; the friction coefficient of the composite coating is 0.32, and the average wear rate is 1.9×10 -7 mm 3 N -1 m -1 ;The maximum resistance of the composite coating is 1.7×10 13 Ω.
[0151] Example 6
[0152] A method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron, wherein the outer layer Al2 O 3 After the deposition temperature was changed to 1030°C and the other parameters remained unchanged, the coating bonding performance test, friction performance test, wear performance test and insulation performance test were carried out again;
[0153] The test results show that Al 2 O 3 The outer surface is dense and uniform, and the outer Al 2 O 3 The grains show a nano-block structure, in which the size of the blocky grains is 450-550nm; the bonding force of the composite coating is 112N; the friction coefficient of the composite coating is 0.29, and the average wear rate is 1.6×10 -7 mm 3 N -1 m -1 ; The maximum resistance of the composite coating is 1.9×10 13 Ω.
[0154] Example 7
[0155] A method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron, wherein the reaction gas is changed to oxygen, and other parameters remain unchanged. After the preparation is completed, the coating bonding performance test, friction performance test, wear performance test and insulation performance test are performed again;
[0156] The test results show that Al 2 O 3 The outer surface is dense and uniform, and the outer Al 2 O 3 The grains show a nano-block structure, in which the size of the blocky grains is 350-450nm; the bonding force of the composite coating is 114N; the friction coefficient of the composite coating is 0.31, and the average wear rate is 1.7×10 -7 mm 3 N -1 m -1 ; The maximum resistance of the composite coating is 1.9×10 13 Ω.
[0157] Example 8
[0158] A method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron, using the data and method in Example 3, modifying one parameter, the modified parameter exceeds the range given in Example 2, and the preparation results after the parameter modification are shown in Table 1. According to Table 1, it can be seen that the test results of each comparative example after the parameter modification are not as good as those in Example 3, thereby proving that exceeding the range given in Example 2 will lead to a decrease in the performance of the wear-resistant insulating composite coating on the surface of electromagnetic pure iron.
[0159]
[0160]
[0161] It can be seen from Table 1 that the grain size of the nano-TiN inner layer of the electromagnetic pure iron surface wear-resistant insulating composite coating prepared in Examples 3-7 is significantly smaller than that of the electromagnetic pure iron surface wear-resistant insulating composite coating prepared in Comparative Examples 1-5.
[0162] Al of the wear-resistant insulating composite coating on the surface of electromagnetic pure iron prepared in Example 3-7 2 O 3 The grain size of the outer layer is significantly smaller than that of the wear-resistant insulating composite coating on the surface of electromagnetic pure iron prepared in Comparative Examples 1-5.
[0163] The bonding force of the wear-resistant insulating composite coating on the surface of electromagnetic pure iron prepared in Examples 1-5 is significantly greater than that of the wear-resistant insulating composite coating on the surface of electromagnetic pure iron prepared in Comparative Examples 1-5.
[0164] The friction coefficient of the wear-resistant insulating composite coating on the surface of electromagnetic pure iron prepared in Examples 1-5 is significantly smaller than that of the wear-resistant insulating composite coating on the surface of electromagnetic pure iron prepared in Comparative Examples 1-5.
[0165] The wear rate of the wear-resistant insulating composite coating on the surface of electromagnetic pure iron prepared in Examples 1-5 is significantly lower than that of the wear-resistant insulating composite coating on the surface of electromagnetic pure iron prepared in Comparative Examples 1-5.
[0166] The insulation performance of the electromagnetic pure iron surface wear-resistant insulating composite coating prepared in Examples 1-5 is significantly greater than that of the electromagnetic pure iron surface wear-resistant insulating composite coating prepared in Comparative Examples 1-5.
[0167] Therefore, compared with comparative examples 1-5, the wear-resistant insulating composite coating on the surface of electromagnetic pure iron prepared in Examples 3-7 of the present invention has excellent bonding performance, friction and wear resistance and insulation performance, and the numerical range given in Example 2 can effectively improve the performance of the wear-resistant insulating composite coating on the surface of electromagnetic pure iron.
[0168] It is known from common technical knowledge that the present invention can be implemented by other embodiments that do not deviate from its spirit or essential features. Therefore, the above disclosed embodiments are only illustrative in all respects and are not exclusive. All changes within the scope of the present invention or within the scope equivalent to the present invention are included in the present invention.
[0169] Those skilled in the art will appreciate that embodiments of the present invention may be provided as methods, systems, or computer program products. Therefore, the present invention may take the form of a complete hardware embodiment, a complete software embodiment, or an embodiment combining software and hardware. Moreover, the present invention may take the form of a computer program product implemented on one or more computer-usable storage media (including but not limited to disk storage, CD-ROM, optical storage, etc.) containing computer-usable program code.
[0170] The present invention is described with reference to flowcharts and / or block diagrams of methods, devices (systems), and computer program products according to embodiments of the present invention. It should be understood that each process and / or block in the flowchart and / or block diagram, as well as the combination of processes and / or blocks in the flowchart and / or block diagram, can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, a special-purpose computer, an embedded processor, or other programmable data processing device to produce a machine, so that the instructions executed by the processor of the computer or other programmable data processing device generate instructions for implementing the processes in the flowchart and / or block diagram. Figure 1 A process or multiple processes and / or boxes Figure 1 A device that provides the functions specified in a block or multiple blocks.
[0171] These computer program instructions may also be stored in a computer-readable memory capable of directing a computer or other programmable data processing device to operate in a specific manner, so that the instructions stored in the computer-readable memory produce an article of manufacture comprising an instruction device, which implements the process Figure 1 A process or multiple processes and / or boxes Figure 1 A function specified in one or more boxes.
[0172] These computer program instructions can also be loaded onto a computer or other programmable data processing device so that a series of operating steps are executed on the computer or other programmable device to produce a computer-implemented process, thereby providing instructions for implementing the process. Figure 1 A process or multiple processes and / or boxes Figure 1 The steps for the functions specified in one or more boxes.
[0173] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A wear-resistant insulating composite coating on the surface of electromagnetic pure iron, It is characterized in that Including TiN inner layer and Al 2 O 3 The outer layer, the TiN inner layer is used to wrap the outer side of the electromagnetic pure iron, and the outer side of the TiN inner layer is wrapped with Al 2 O 3 Outer layer.
2. The wear-resistant insulating composite coating on the surface of electromagnetic pure iron according to claim 1, It is characterized in that The TiN inner layer and Al 2 O 3 The total thickness of the outer layer is 10 μm-25 μm.
3. A method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron, It is characterized in that The following steps are involved: A nitrogen source, a titanium source and an auxiliary gas are introduced into the substrate, and a TiN inner layer is formed on the surface of the substrate by a chemical vapor deposition method; Aluminum source, reaction gas and auxiliary gas are introduced into the substrate, and Al is generated on the outside of the TiN inner layer by chemical vapor deposition. 2 O 3 Outer layer.
4. The method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron according to claim 3, It is characterized in that The substrate is pre-treated in advance, and the pre-treatment includes grinding, cleaning, sandblasting and vacuum drying in sequence.
5. The method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron according to claim 3, It is characterized in that The step of introducing a nitrogen source, a titanium source and an auxiliary gas into the substrate and forming a TiN inner layer on the surface of the substrate by chemical vapor deposition method specifically includes: placing the substrate into a CVD furnace; evacuating the CVD furnace to a first pressure; Introducing an auxiliary gas into the CVD furnace, and heating the CVD furnace to a first temperature at a first heating rate; A nitrogen source, an auxiliary gas and a titanium source are introduced into the CVD furnace, and a TiN inner layer is deposited on the surface of the substrate.
6. The method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron according to claim 3, It is characterized in that Aluminum source, reaction gas and auxiliary gas are introduced into the substrate, and Al is generated on the outside of the TiN inner layer by chemical vapor deposition. 2 O 3 The outer steps specifically include: heating the CVD furnace to a second temperature; Aluminum source, reaction gas and auxiliary gas are introduced into the CVD furnace, and Al is deposited on the outside of the TiN inner layer. 2 O 3 Outer layer.
7. The method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron according to claim 3, It is characterized in that The cooling step further comprises: Stop introducing the aluminum source and the reaction gas, and reduce the volume flow rate of the auxiliary gas to a sixth volume flow rate; The CVD furnace is cooled to a third temperature at a first cooling rate, and the auxiliary gas volume flow rate is reduced again to a seventh volume flow rate; When the CVD furnace is cooled to the fourth temperature, the introduction of hydrogen is stopped to allow the CVD to cool to room temperature.
8. The method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron according to claim 3, It is characterized in that The titanium source is one or more combinations of butyl titanate, titanium tetrachloride, titanium trichloride, titanium dichloride, titanium chloride and / or titanium powder.
9. The method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron according to claim 3, It is characterized in that The aluminum source is one or more combinations of aluminum powder, aluminum ingot, aluminum trichloride and / or aluminum pentachloride.
10. The method for preparing a wear-resistant insulating composite coating on the surface of electromagnetic pure iron according to claim 3, It is characterized in that One or more combinations of the nitrogen, argon and / or hydrogen.