Preparation method of tin-silver-copper-aluminum quaternary alloy and application of tin-silver-copper-aluminum quaternary alloy in negative electrode of secondary battery
Preparation of tin-silver copper-aluminum quadrimer alloy as the negative electrode material of secondary battery through magnetron sputtering method has solved the problems of limited types of materials and complex processes in the prior art, achieved better cycle stability and electrochemical performance, and reduced production costs.
Patent Information
- Application Number
- CN202411174586.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The types of positive and negative electrode materials for existing lithium-ion batteries and sodium-ion batteries are limited, the preparation process is complex, and the negative electrode materials have poor cycling performance during charging and discharging, which poses safety hazards and low Coulomb efficiency.
The magnetron sputtering method is used to prepare tin-silver copper-aluminum quadrature alloy as the negative electrode material of the secondary battery. By setting the flow rate of tin, silver, copper, aluminum targets and argon gas, the magnetron sputtering power parameters, the process is simplified and the cost is reduced. .
It improves the cycle stability and energy density of secondary batteries, extends the battery life, simplifies the battery production process, reduces costs, and improves electrochemical performance.
Smart Images

Figure CN119040829A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of secondary batteries, and in particular relates to a preparation method of a tin-silver-copper-aluminum quaternary alloy and an application thereof in secondary batteries. Background Art
[0002] Secondary batteries, also known as rechargeable batteries, are batteries that can be repeatedly charged and discharged and used multiple times. Compared with non-reusable primary batteries, secondary batteries have the advantages of low cost and less environmental pollution. The main secondary battery technologies currently include lead-acid batteries, nickel-chromium batteries, nickel-metal hydride batteries, lithium-ion batteries, and sodium-ion batteries. Among them, lithium-ion batteries are the most widely used. As a potential energy storage technology to replace lithium-ion batteries, sodium-ion batteries have also received increasing attention in recent years. The core components of lithium-ion batteries and sodium-ion batteries include positive electrodes, negative electrodes, and electrolytes. They achieve electrical energy storage and release through reactions that separate ion transfer and electron transfer at the interfaces of the positive and negative electrodes and the electrolyte. During charging, the reaction occurring at the negative electrode is that lithium / sodium ions are embedded in the negative electrode active material from the electrolyte, and the reaction occurring at the positive electrode is that lithium / sodium ions are released from the positive electrode active material into the electrolyte or the anions are intercalated into the positive electrode active material; during discharging, lithium / sodium ions are released from the negative electrode active material and returned to the electrolyte, and the lithium / sodium ions in the electrolyte are embedded in the positive electrode active material or the anions are released from the positive electrode active material and returned to the electrolyte.
[0003] Lithium ion batteries and sodium ion batteries use oxides, polyanion compounds, organic compounds, etc. as positive electrode active materials, and carbon materials, alloy materials, oxides, sulfides, phosphides, organic compounds, etc. as negative electrode active materials. However, the types of positive and negative electrode materials developed based on lithium ion batteries and sodium ion batteries are very limited, and the research on new positive and negative electrode materials is basically limited to batteries for lithium sheets or sodium sheets. The electrochemical performance of lithium ion batteries and sodium ion batteries based on the developed new positive and negative electrode materials is not very ideal, and the preparation process is also relatively complicated. Research on the preparation of negative electrode materials for sodium ion batteries (patent publication numbers: CN109817960A, CN103647068A, CN103633310A, CN103553129A), this type of invention all provides a method for preparing high-capacity negative electrode materials for sodium ion batteries, but these high-capacity negative electrode materials have the problem of poor cycle performance during the charge and discharge process.
[0004] Lithium-ion batteries and sodium-ion batteries are considered to be powerful ways of large-scale energy storage. The performance of negative electrode materials is a very important performance indicator of lithium-ion batteries and sodium-ion batteries. Taking sodium-ion batteries as an example, the negative electrode materials of sodium-ion batteries are currently mainly hard carbon and alloy negative electrodes. For example, reports such as IONICS, 2020, 26: 5535-5542, Electrochimica Acta, 2020, 361: 137041, and JOURNAL OF INDUSTRIAL AND ENGINEERINGCHEMISTRY, 2020, 91: 317-329 use hard carbon materials as negative electrodes; other reports such as SMALL METHODS, 2020, 4: 2000218, CHEMICAL ENGINEERING JOURNAL, 2020, 388: 124299, and JOURNAL OF ALLOYS AND COMPOUNDS, 2020, 834: 154304 use alloy materials as negative electrodes. However, in addition to the harsh preparation conditions of these materials (especially alloy materials), these two materials each have a major disadvantage when used for sodium ion negative electrode plates: for hard carbon, its voltage platform is close to the deposition potential of metallic sodium, and it is very easy to produce sodium metal dendrites under high current charging conditions, causing serious safety problems. For alloy material negative electrodes, due to their drastic volume deformation, the solid electrolyte interface film on the surface of the metal alloy is continuously broken and generated during the charging and discharging process, so its coulomb efficiency is low, which greatly limits the cycle life of the full battery.
[0005] From the published literature reports and published patents, there is no discovery of the use of magnetron sputtering to prepare tin-silver-copper-aluminum quaternary alloy for the negative electrode of secondary batteries. Summary of the invention
[0006] In view of the problems raised in the above background technology, the purpose of the present invention is to overcome the shortcomings of the prior art and to solve the problems of limited materials, high cost, complex preparation process and unsatisfactory electrochemical performance of alloy negative electrodes of existing secondary batteries. The present invention provides a preparation method of a tin-silver-copper-aluminum quaternary alloy and its application in the negative electrode of a secondary battery.
[0007] The present invention uses a magnetron sputtering method to prepare a quaternary alloy using tin, silver, copper and aluminum target materials as raw materials. The preparation process is relatively simple, so the cost is greatly reduced. The present invention solves the shortcomings of the existing lithium-ion batteries, such as limited lithium resource reserves and high costs. In addition, the present invention is simpler in process, safer and more reliable, and has a higher energy density than the existing sodium-ion battery.
[0008] A method for preparing a tin-silver-copper-aluminum quaternary alloy is specifically completed by the following steps:
[0009] 1. Using tin, silver, copper, and aluminum targets as raw materials, set the argon gas flow rate;
[0010] 2. Set the magnetron sputtering power parameters of tin target, silver target, copper target and aluminum target respectively;
[0011] 3. Set the time and substrate speed of magnetron sputtering, turn on the power of magnetron sputtering, start sputtering on the current collector, and end sputtering to obtain a tin-silver-copper-aluminum quaternary alloy.
[0012] A tin-silver-copper-aluminum quaternary alloy is used as a negative electrode active material of a secondary battery.
[0013] Compared with the prior art, the present invention has the following beneficial effects:
[0014] 1. The present invention uses tin, silver, copper and aluminum as raw materials to prepare a quaternary alloy by a magnetron sputtering method, and uses the prepared tin-silver-copper-aluminum quaternary alloy as the negative electrode material of the secondary battery. The capacity decay is small during each charge and discharge process. Therefore, the secondary battery prepared by using the tin-silver-copper-aluminum quaternary alloy prepared by the present invention as the negative electrode of the secondary battery has good cycle stability, and the battery life is increased to a certain extent;
[0015] 2. The new secondary battery negative electrode prepared by the present invention has a larger specific capacity and energy density than the hard carbon negative electrode; and has a stronger cycle stability than other alloy material negative electrodes;
[0016] 3. The preparation of the negative electrode of the secondary battery of the present invention uses a magnetron sputtering method to prepare a quaternary alloy using tin, silver, copper and aluminum as raw materials. The preparation process is relatively simple, so the cost is greatly reduced;
[0017] 4. Compared with existing sodium ion batteries, the electrode materials of the present invention are simple, easily available, environmentally friendly and safe, which makes the production process of the battery simple, low-cost and the electrochemical performance of the battery relatively excellent. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 1 is a schematic diagram of the structure of a secondary battery provided by the present invention, wherein 1 is a negative electrode current collector of the battery, 2 is a negative electrode active material of the battery, 3 is an electrolyte, 4 is a separator, 5 is a positive electrode active material of the battery, and 6 is a positive electrode current collector;
[0019] Figure 2 The Sn prepared in Example 1 66 Ag 9 Cu 16 Al 9 The sodium ion secondary battery assembled with the negative electrode and the Sn prepared in Example 2 54 Ag 16 Cu 18 Al 12Cycling performance curve of sodium ion secondary battery assembled with negative electrode;
[0020] Figure 3 The figure is a cycle performance curve of a sodium ion secondary battery assembled using the tin-silver-copper ternary alloy prepared in Comparative Example 1;
[0021] Figure 4 The figure is a cycle performance curve of a sodium ion secondary battery assembled using the tin-silver-aluminum ternary alloy prepared in Comparative Example 2;
[0022] Figure 5 The figure is a cycle performance curve of a sodium ion secondary battery assembled using the tin-copper-aluminum ternary alloy prepared in Comparative Example 3;
[0023] Figure 6 The figure is a cycle performance curve of a sodium ion secondary battery assembled using the tin-silver binary alloy prepared in Comparative Example 4;
[0024] Figure 7 The figure is a cycle performance curve of a sodium ion secondary battery assembled using the tin-copper binary alloy prepared in Comparative Example 5;
[0025] Figure 8 The figure is a cycle performance curve of a sodium ion secondary battery assembled using the tin-aluminum binary alloy prepared in Comparative Example 6;
[0026] Fig. 9 This is a cycle performance curve of a sodium-ion secondary battery assembled using pure tin as the negative electrode. DETAILED DESCRIPTION
[0027] Specific implementation method 1: This implementation method is a method for preparing a tin-silver-copper-aluminum quaternary alloy, which is specifically completed according to the following steps:
[0028] 1. Using tin, silver, copper, and aluminum targets as raw materials, set the argon gas flow rate;
[0029] 2. Set the magnetron sputtering power parameters of tin target, silver target, copper target and aluminum target respectively;
[0030] 3. Set the time and substrate speed of magnetron sputtering, turn on the power of magnetron sputtering, start sputtering on the current collector, and end sputtering to obtain a tin-silver-copper-aluminum quaternary alloy.
[0031] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the argon gas flow rate in step 1 is 100 mL / min to 300 mL / min. The other steps are the same as those in specific implementation method 1.
[0032] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that: in step 2, the magnetron sputtering power parameter of the tin target is set to 120W-180W, the magnetron sputtering power parameter of the silver target is set to 15W-40W, the magnetron sputtering power parameter of the copper target is set to 20W-50W, and the magnetron sputtering power parameter of the aluminum target is set to 20W-100W. The other steps are the same as those of specific embodiment 1 or 2.
[0033] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: in step 2, the magnetron sputtering power parameter of the tin target is set to 150 W, the magnetron sputtering power parameter of the silver target is set to 25 W, the magnetron sputtering power parameter of the copper target is set to 30 W, and the magnetron sputtering power parameter of the aluminum target is set to 45 W. The other steps are the same as those of specific embodiments 1 to 3.
[0034] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that: in step 3, the magnetron sputtering time is set to 1800s to 9000s; in step 3, the substrate speed is set to 0r / min to 60r / min; the current collector described in step 3 is a metal conductive material, and the metal conductive material is one of aluminum, copper, tin, zinc, lead, antimony, cadmium, gold, bismuth and germanium, a composite of any one of these metals, or an alloy of any one of these metals. The other steps are the same as specific embodiments 1 to 4.
[0035] Specific implementation method 6: This implementation method is a tin-silver-copper-aluminum quaternary alloy used as the negative electrode of a secondary battery.
[0036] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: the secondary battery comprises a positive electrode, a negative electrode, a separator between the positive electrode and the negative electrode, and an electrolyte; the positive electrode comprises a positive electrode active material and a positive electrode current collector. The other steps are the same as those of specific embodiments 1 to 6.
[0037] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that: the positive electrode active material is lithium nickel cobalt manganese oxide, lithium iron phosphate, lithium cobalt oxide, sodium vanadium phosphate, Prussian blue or layered oxide; the positive electrode current collector is one of carbon-coated aluminum foil, carbon-coated copper foil, carbon-coated iron foil, carbon-coated tin foil, carbon-coated zinc foil, carbon-coated nickel foil, carbon-coated titanium foil, carbon-coated manganese foil, a composite of any one of these metals, or an alloy of any one of these metals. The other steps are the same as specific embodiments 1 to 7.
[0038] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that: the diaphragm is a porous polymer film or an inorganic porous film; the porous polymer film is a porous polypropylene film, a porous polyethylene film or a composite film of porous polypropylene and porous polyethylene; the inorganic porous film is a glass fiber paper or a porous ceramic diaphragm; the electrolyte includes an electrolyte and a solvent, the electrolyte is a lithium salt or sodium salt electrolyte, and the solvent is selected from one or more of esters, sulfones, ethers, nitriles and ionic liquid organic solvents; the concentration of the electrolyte is 0.1 mol / L to 10 mol / L. The other steps are the same as those of specific embodiments 1 to 8.
[0039] Specific embodiment ten: This embodiment is different from specific embodiments one to nine in that the electrolyte includes lithium hexafluorophosphate, lithium chloride, lithium fluoride, lithium sulfate, lithium carbonate, lithium phosphate, lithium nitrate, lithium difluoro oxalate borate, lithium pyrophosphate, lithium dodecylbenzenesulfonate, lithium dodecyl sulfate, trilithium citrate, lithium metaborate, lithium borate, lithium molybdate, lithium tungstate, lithium bromide, lithium nitrite, lithium iodate, lithium iodide, lithium silicate, lithium ligninsulfonate, lithium oxalate, lithium aluminate, lithium methanesulfonate, lithium acetate, lithium dichromate, lithium hexafluoroarsenate, lithium tetrafluoroborate, lithium perchlorate, lithium trifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium bistrifluoromethanesulfonyl imide, sodium hexafluorophosphate, chloride Sodium, sodium fluoride, sodium sulfate, sodium carbonate, sodium phosphate, sodium nitrate, sodium difluoro oxalate borate, sodium pyrophosphate, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, trisodium citrate, sodium metaborate, sodium borate, sodium molybdate, sodium tungstate, sodium bromide, sodium nitrite, sodium iodate, sodium iodide, sodium silicate, sodium lignin sulfonate, sodium oxalate, sodium aluminate, sodium methane sulfonate, sodium acetate, sodium dichromate, sodium hexafluoroarsenate, sodium tetrafluoroborate, sodium perchlorate, sodium trifluoromethanesulfonimide, sodium trifluoromethanesulfonate and sodium bistrifluoromethanesulfonimide; the solvent includes propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, methyl formate, methyl acetate, N,N-dimethylacetamide, fluoroethylene carbonate, methyl propionate, ethyl propionate, ethyl acetate, γ-butyrolactone, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, dimethoxymethane, 1,2-dimethoxypropane, triethylene glycol dimethyl ether, dimethyl sulfone, dimethyl ether, vinyl sulfite, propylene sulfite, dimethyl sulfite, diethyl sulfite, crown ether (12-crown-4), 1-ethyl-3-methylimidazole-hexafluorophosphate, 1-ethyl-3-methylimidazole-tetrafluoroborate, 1-ethyl-3-methylimidazole-bis(trifluoromethylsulfonyl)imide, 1-propyl-3-methylimidazole-hexafluorophosphate One or more of 1-butyl-1-methylimidazole-bis(trifluoromethanesulfonyl)imide salt, 1-propyl-3-methylimidazole-tetrafluoroborate, 1-propyl-3-methylimidazole-bis(trifluoromethanesulfonyl)imide salt, 1-butyl-1-methylimidazole-hexafluorophosphate, 1-butyl-1-methylimidazole-tetrafluoroborate, 1-butyl-1-methylimidazole-bis(trifluoromethanesulfonyl)imide salt, N-butyl-N-methylpyrrolidine-bis(trifluoromethanesulfonyl)imide salt, 1-butyl-1-methylpyrrolidine-bis(trifluoromethanesulfonyl)imide salt, N-methyl-N-propylpyrrolidine-bis(trifluoromethanesulfonyl)imide salt, N-methyl-N-propylpyrrolidine-bis(trifluoromethanesulfonyl)imide salt, N-methyl-N-propylpiperidine-bis(trifluoromethanesulfonyl)imide salt. Other steps are the same as those in specific embodiments one to nine.
[0040] The following examples are used to verify the beneficial effects of the present invention:
[0041] Embodiment 1: A method for preparing a tin-silver-copper-aluminum quaternary alloy is specifically completed by the following steps:
[0042] 1. Using tin, silver, copper, and aluminum targets as raw materials, set the argon gas flow rate;
[0043] The argon gas flow rate in step 1 is 300 mL / min;
[0044] 2. Set the magnetron sputtering power parameters of tin target, silver target, copper target and aluminum target respectively;
[0045] In step 2, the magnetron sputtering power parameter of the tin target is set to 150 W, the magnetron sputtering power parameter of the silver target is set to 25 W, the magnetron sputtering power parameter of the copper target is set to 30 W, and the magnetron sputtering power parameter of the aluminum target is set to 45 W;
[0046] 3. Set the time and substrate speed of magnetron sputtering, turn on the power of magnetron sputtering, start sputtering on the current collector, and end sputtering to obtain Sn 66 Ag 9 Cu 16 Al 9 Tin-silver-copper-aluminum quaternary alloy;
[0047] In step 3, the magnetron sputtering time is set to 5400 s; in step 3, the substrate speed is set to 60 r / min;
[0048] The current collector described in step three is copper foil.
[0049] Embodiment 2: The difference between this embodiment and embodiment 1 is that in step 2, the magnetron sputtering power parameter of the tin target is set to 140W, the magnetron sputtering power parameter of the silver target is set to 25W, the magnetron sputtering power parameter of the copper target is set to 30W, and the magnetron sputtering power parameter of the aluminum target is set to 45W; in step 3, Sn is obtained. 54 Ag 16 Cu 18 Al 12 The other steps and parameters are the same as those in Example 1.
[0050] Comparative Example 1: The difference between this embodiment and embodiment 1 is that in step 2, the magnetron sputtering power parameter of the tin target is set to 140W, the magnetron sputtering power parameter of the silver target is set to 25W, the magnetron sputtering power parameter of the copper target is set to 30W, and the magnetron sputtering power parameter of the aluminum target is set to 0W; in step 3, a ternary alloy of tin, silver and copper is obtained. The other steps and parameters are the same as those in embodiment 1.
[0051] Comparative Example 2: The difference between this embodiment and embodiment 1 is that in step 2, the magnetron sputtering power parameter of the tin target is set to 140W, the magnetron sputtering power parameter of the silver target is set to 25W, the magnetron sputtering power parameter of the copper target is set to 0W, and the magnetron sputtering power parameter of the aluminum target is set to 45W; in step 3, a ternary alloy of tin, silver, and aluminum is obtained. The other steps and parameters are the same as those in embodiment 1.
[0052] Comparative Example 3: The difference between this embodiment and embodiment 1 is that in step 2, the magnetron sputtering power parameter of the tin target is set to 140W, the magnetron sputtering power parameter of the silver target is set to 0W, the magnetron sputtering power parameter of the copper target is set to 30W, and the magnetron sputtering power parameter of the aluminum target is set to 45W; in step 3, a ternary alloy of tin, copper, and aluminum is obtained. The other steps and parameters are the same as those in embodiment 1.
[0053] Comparative Example 4: The difference between this embodiment and embodiment 1 is that in step 2, the magnetron sputtering power parameter of the tin target is set to 140W, the magnetron sputtering power parameter of the silver target is set to 25W, the magnetron sputtering power parameter of the copper target is set to 0W, and the magnetron sputtering power parameter of the aluminum target is set to 0W; in step 3, a tin-silver binary alloy is obtained. The other steps and parameters are the same as those in embodiment 1.
[0054] Comparative Example 5: The difference between this embodiment and embodiment 1 is that in step 2, the magnetron sputtering power parameter of the tin target is set to 140W, the magnetron sputtering power parameter of the silver target is set to 0W, the magnetron sputtering power parameter of the copper target is set to 30W, and the magnetron sputtering power parameter of the aluminum target is set to 0W; in step 3, a tin-copper binary alloy is obtained. The other steps and parameters are the same as those in embodiment 1.
[0055] Comparative Example 6: The difference between this embodiment and embodiment 1 is that in step 2, the magnetron sputtering power parameter of the tin target is set to 140W, the magnetron sputtering power parameter of the silver target is set to 0W, the magnetron sputtering power parameter of the copper target is set to 0W, and the magnetron sputtering power parameter of the aluminum target is set to 45W; in step 3, a tin-aluminum binary alloy is obtained. The other steps and parameters are the same as those in embodiment 1.
[0056] Application Example 1: Using the Sn prepared in Example 1 66 Ag 9 Cu 16 Al 9 The sodium ion secondary battery assembled by the tin-silver-copper-aluminum quaternary alloy is specifically completed in the following steps:
[0057] 1) Preparation of battery negative electrode: Sn prepared in Example 1 66 Ag 9 Cu 16 Al 9 The tin-silver-copper-aluminum quaternary alloy is cut into discs with a diameter of 12 mm and compacted to serve as the negative electrode of the battery;
[0058] 2) Preparation of electrolyte: weigh 6.7 g of sodium hexafluorophosphate and add it to 10 mL of a mixed solvent of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate (the volume ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 1:1:1), stir until the sodium hexafluorophosphate is completely dissolved, stir thoroughly and use as electrolyte for standby use;
[0059] 3) Preparation of diaphragm: Cut the glass fiber film into discs with a diameter of 16 mm and use them as diaphragms;
[0060] 4) Prepare the positive electrode of the battery: add 0.8g sodium vanadium phosphate, 0.1g carbon black, and 0.1g polytetrafluoroethylene to 4mL nitrogen methyl pyrrolidone, grind thoroughly to obtain a uniform slurry; then evenly apply the slurry on the surface of the carbon-coated aluminum foil (i.e., the positive electrode current collector) and vacuum dry. Cut the dried electrode sheet into a disc with a diameter of 10mm and use it as the positive electrode of the battery;
[0061] 5) Battery assembly: In an inert gas-protected glove box, the prepared positive electrode, separator, and negative electrode are tightly stacked in sequence, and the electrolyte is dripped to completely soak the separator. Then, the stacked part is encapsulated into a button battery casing to complete the battery assembly and obtain a sodium ion secondary battery.
[0062] At room temperature, the sodium ion secondary battery assembled in Example 1 was subjected to constant current charge and discharge test using Shenzhen Xinweier battery test system. The charge and discharge current was 500 mA / g, and the charge and discharge voltage range was 2 to 3.8 V. The cycle performance curve is shown in FIG. Figure 2 Sn 66 Ag 9 Cu 16 Al 9 Part shown. Figure 2 Sn 66 Ag 9 Cu 16 Al 9 It can be seen that the Sn prepared in Example 1 66 Ag 9 Cu 16 Al 9 After several charge and discharge cycles, the sodium ion secondary battery made of tin-silver-copper-aluminum quaternary alloy has a coulombic efficiency greater than 99%, a charge and discharge capacity of about 600 mAh / g, and a capacity retention rate greater than 90% after about 100 cycles.
[0063] Application Example 2: The difference between this application example and application example 1 is that the Sn prepared in Example 2 is used. 54 Ag 16 Cu 18 Al 12A sodium ion secondary battery assembled with a tin-silver-copper-aluminum quaternary alloy, that is, the Sn prepared in Example 2 54 Ag 16 Cu 18 Al 12 The tin-silver-copper-aluminum quaternary alloy was cut into discs with a diameter of 12 mm and compacted to serve as the negative electrode of the battery. The other steps and parameters were the same as those in Application Example 1.
[0064] At room temperature, the sodium ion secondary battery assembled in Application Example 2 was subjected to constant current charge and discharge test using Shenzhen Xinweier battery test system. The charge and discharge current was 500 mA / g, and the charge and discharge voltage range was 2 to 3.8 V. The cycle performance curve is shown in FIG. Figure 2 Sn 66 Ag 9 Cu 16 Al 9 Part shown. Figure 2 Sn 66 Ag 9 Cu 16 Al 9 It can be seen from the part that the Sn prepared in Example 2 is used in Example 2. 54 Ag 16 Cu 18 Al 12 After 100 charge and discharge cycles, the charge and discharge capacity of the sodium ion secondary battery assembled by the tin-silver-copper-aluminum quaternary alloy is only about 350 mAh / g, and the capacity retention rate is less than 70%.
[0065] Application Example 3: The difference between this application example and application example 1 is that the sodium ion secondary battery assembled with the tin-silver-copper ternary alloy prepared in reference example 1 is that the tin-silver-copper ternary alloy prepared in reference example 1 is cut into discs with a diameter of 12 mm, which are compacted and used as the negative electrode of the battery for standby use. The other steps and parameters are the same as those in application example 1.
[0066] The sodium ion secondary battery assembled in Example 3 was subjected to constant current charge and discharge test using Shenzhen Xinweier battery test system at room temperature. The charge and discharge current was 500 mA / g, and the charge and discharge voltage range was 2 to 3.8 V. The test results are as follows: Figure 3 As shown: After 100 charge and discharge cycles, the sodium ion secondary battery assembled with the tin-silver-copper ternary alloy prepared in Application Example 3 has a charge and discharge capacity of only about 300 mAh / g, and a capacity retention rate of less than 55%.
[0067] Application Example 4: This application example is different from Application Example 1 in that the sodium ion secondary battery is assembled using the tin-silver-aluminum ternary alloy prepared in Reference Example 2, that is, the tin-silver-aluminum ternary alloy prepared in Reference Example 2 is cut into discs with a diameter of 12 mm, which are compacted and used as the negative electrode of the battery for standby use. The other steps and parameters are the same as those in Application Example 1.
[0068] The sodium ion secondary battery assembled in Example 4 was subjected to constant current charge and discharge tests at room temperature using Shenzhen Xinwell Battery Test System. The charge and discharge current was 500 mA / g, and the charge and discharge voltage range was 2 to 3.8 V. The test results are as follows: Figure 4 As shown: After 100 charge and discharge cycles, the sodium ion secondary battery assembled with the tin-silver-aluminum ternary alloy prepared in Application Example 4 and Control Example 2 has a charge and discharge capacity of only about 230 mAh / g, and a capacity retention rate of less than 40%.
[0069] Application Example 5: This application example is different from Application Example 1 in that the sodium ion secondary battery is assembled using the tin-copper-aluminum ternary alloy prepared in Reference Example 3, that is, the tin-copper-aluminum ternary alloy prepared in Reference Example 3 is cut into discs with a diameter of 12 mm, which are compacted and used as the battery negative electrode for standby use. The other steps and parameters are the same as those in Application Example 1.
[0070] The sodium ion secondary battery assembled in Example 5 was subjected to constant current charge and discharge tests at room temperature using Shenzhen Xinweier Battery Test System. The charge and discharge current was 500 mA / g, and the charge and discharge voltage range was 2 to 3.8 V. The test results are as follows: Figure 5 As shown: After 100 charge and discharge cycles, the sodium ion secondary battery assembled with the tin-copper-aluminum ternary alloy prepared in Application Example 5 and Control Example 3 has a charge and discharge capacity of only about 420 mAh / g, and a capacity retention rate of less than 65%.
[0071] Application Example 6: This application example is different from Application Example 1 in that the sodium ion secondary battery is assembled using the tin-copper-aluminum ternary alloy prepared in Reference Example 4, that is, the tin-silver binary alloy prepared in Reference Example 4 is cut into discs with a diameter of 12 mm, which are compacted and used as the battery negative electrode for standby use. The other steps and parameters are the same as those in Application Example 1.
[0072] The sodium ion secondary battery assembled in Example 6 was subjected to constant current charge and discharge tests at room temperature using Shenzhen Xinwell Battery Test System. The charge and discharge current was 500 mA / g, and the charge and discharge voltage range was 2 to 3.8 V. The test results are shown in FIG. Figure 6 As shown: After 100 charge and discharge cycles, the sodium ion secondary battery assembled with the tin-silver binary alloy prepared in Application Example 6 using Control Example 4 has a charge and discharge capacity of only about 110 mAh / g, and a capacity retention rate of less than 20%.
[0073] Application Example 7: This application example is different from Application Example 1 in that a sodium ion secondary battery is assembled using the tin-copper binary alloy prepared in Reference Example 5, that is, the tin-copper binary alloy prepared in Reference Example 5 is cut into discs with a diameter of 12 mm, which are compacted and used as the negative electrode of the battery for standby use. The other steps and parameters are the same as those in Application Example 1.
[0074] The sodium ion secondary battery assembled in Example 7 was subjected to constant current charge and discharge test at room temperature using Shenzhen Xinweier battery test system. The charge and discharge current was 500 mA / g, and the charge and discharge voltage range was 2 to 3.8 V. The test results are as follows: Figure 7 As shown: After 100 charge and discharge cycles, the sodium ion secondary battery assembled with the tin-copper binary alloy prepared in Application Example 7 using Control Example 5 has a charge and discharge capacity of only about 340 mAh / g, and a capacity retention rate of less than 50%.
[0075] Application Example 8: This application example is different from Application Example 1 in that the sodium ion secondary battery is assembled using the tin-aluminum binary alloy prepared in Reference Example 6, that is, the tin-aluminum binary alloy prepared in Reference Example 6 is cut into discs with a diameter of 12 mm, which are compacted and used as the negative electrode of the battery for standby use. The other steps and parameters are the same as those in Application Example 1.
[0076] The sodium ion secondary battery assembled in Example 8 was subjected to constant current charge and discharge tests at room temperature using Shenzhen Xinwell Battery Test System. The charge and discharge current was 500 mA / g, and the charge and discharge voltage range was 2 to 3.8 V. The test results are as follows: Figure 8 As shown: After 100 charge and discharge cycles, the sodium ion secondary battery assembled with the tin-aluminum binary alloy prepared in Application Example 8 using Control Example 6 has a charge and discharge capacity of only about 240 mAh / g, and a capacity retention rate of less than 35%.
[0077] Application Example 9: This application example is different from Application Example 1 in that a sodium ion secondary battery is assembled using pure tin as the negative electrode, that is, pure tin is cut into discs with a diameter of 12 mm, which are compacted and used as the negative electrode of the battery. Other steps and parameters are the same as those in Application Example 1.
[0078] The sodium ion secondary battery assembled in Example 9 was subjected to constant current charge and discharge tests at room temperature using Shenzhen Xinwell Battery Test System. The charge and discharge current was 500 mA / g, and the charge and discharge voltage range was 2 to 3.8 V. The test results are as follows: Fig. 9 As shown: In Application Example 9, the sodium ion secondary battery assembled using pure tin as the negative electrode has a charge and discharge capacity of less than 10 mAh / g after 32 charge and discharge cycles, and a capacity retention rate of less than 1% after 100 cycles.
Claims
1. A method for preparing a tin-silver-copper-aluminum quaternary alloy, characterized in that The preparation method is specifically completed according to the following steps:
1. Using tin, silver, copper, and aluminum targets as raw materials, set the argon gas flow rate; 2. Set the magnetron sputtering power parameters of tin target, silver target, copper target and aluminum target respectively; 3. Set the time and substrate speed of magnetron sputtering, turn on the power of magnetron sputtering, start sputtering on the current collector, and end sputtering to obtain a tin-silver-copper-aluminum quaternary alloy.
2. The method for preparing a tin-silver-copper-aluminum quaternary alloy according to claim 1, characterized in that The argon gas flow rate in step 1 is 100 mL / min to 300 mL / min.
3. The method for preparing a tin-silver-copper-aluminum quaternary alloy according to claim 1, characterized in that In step 2, the magnetron sputtering power parameter of the tin target is set to 120W-180W, the magnetron sputtering power parameter of the silver target is set to 15W-40W, the magnetron sputtering power parameter of the copper target is set to 20W-50W, and the magnetron sputtering power parameter of the aluminum target is set to 20W-100W.
4. The method for preparing a tin-silver-copper-aluminum quaternary alloy according to claim 3, characterized in that In step 2, the magnetron sputtering power parameter of the tin target is set to 150W, the magnetron sputtering power parameter of the silver target is set to 25W, the magnetron sputtering power parameter of the copper target is set to 30W, and the magnetron sputtering power parameter of the aluminum target is set to 45W.
5. The method for preparing a tin-silver-copper-aluminum quaternary alloy according to claim 1, characterized in that In step three, the magnetron sputtering time is set to 1800s to 9000s; in step three, the substrate rotation speed is set to 0r / min to 60r / min; the current collector described in step three is a metal conductive material, and the metal conductive material is one of aluminum, copper, tin, zinc, lead, antimony, cadmium, gold, bismuth and germanium, a composite of any one of these metals, or an alloy of any one of them.
6. Application of a tin-silver-copper-aluminum quaternary alloy prepared by the preparation method according to claim 1, characterized in that A tin-silver-copper-aluminum quaternary alloy is used as the negative electrode of a secondary battery.
7. The use of a tin-silver-copper-aluminum quaternary alloy according to claim 6, characterized in that The secondary battery comprises a positive electrode, a negative electrode, a separator between the positive electrode and the negative electrode, and an electrolyte; the positive electrode comprises a positive electrode active material and a positive electrode current collector.
8. The use of a tin-silver-copper-aluminum quaternary alloy according to claim 7, characterized in that The positive electrode active material is lithium nickel cobalt manganese oxide, lithium iron phosphate, lithium cobalt oxide, sodium vanadium phosphate, Prussian blue or layered oxide; the positive electrode current collector is one of carbon-coated aluminum foil, carbon-coated copper foil, carbon-coated iron foil, carbon-coated tin foil, carbon-coated zinc foil, carbon-coated nickel foil, carbon-coated titanium foil, carbon-coated manganese foil, a composite of any one of these metals, or an alloy of any one of these metals.
9. The use of a tin-silver-copper-aluminum quaternary alloy according to claim 7, characterized in that The diaphragm is a porous polymer film or an inorganic porous film; the porous polymer film is a porous polypropylene film, a porous polyethylene film or a composite film of porous polypropylene and porous polyethylene; the inorganic porous film is a glass fiber paper or a porous ceramic diaphragm; the electrolyte includes an electrolyte and a solvent, the electrolyte is a lithium salt or sodium salt electrolyte, and the solvent is selected from one or more of esters, sulfones, ethers, nitriles and ionic liquid organic solvents; the concentration of the electrolyte is 0.1 mol / L to 10 mol / L.
10. The use of a tin-silver-copper-aluminum quaternary alloy according to claim 9, characterized in that The electrolyte includes lithium hexafluorophosphate, lithium chloride, lithium fluoride, lithium sulfate, lithium carbonate, lithium phosphate, lithium nitrate, lithium difluoro oxalate borate, lithium pyrophosphate, lithium dodecylbenzene sulfonate, lithium dodecyl sulfate, trilithium citrate, lithium metaborate, lithium borate, lithium molybdate, lithium tungstate, lithium bromide, lithium nitrite, lithium iodate, lithium iodide, lithium silicate, lithium lignin sulfonate, lithium oxalate, lithium aluminate, lithium methane sulfonate, lithium acetate, lithium dichromate, lithium hexafluoroarsenate, lithium tetrafluoroborate, lithium perchlorate, lithium trifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium bistrifluoromethanesulfonyl imide, sodium hexafluorophosphate, sodium chloride, sodium fluoride, sodium sulfate, sodium carbonate, sodium phosphate, sodium nitrate, One or more of sodium difluorooxalatoborate, sodium pyrophosphate, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, trisodium citrate, sodium metaborate, sodium borate, sodium molybdate, sodium tungstate, sodium bromide, sodium nitrite, sodium iodate, sodium iodide, sodium silicate, sodium lignin sulfonate, sodium oxalate, sodium aluminate, sodium methane sulfonate, sodium acetate, sodium dichromate, sodium hexafluoroarsenate, sodium tetrafluoroborate, sodium perchlorate, sodium trifluoromethanesulfonimide, sodium trifluoromethanesulfonate and sodium bistrifluoromethanesulfonimide; the solvent includes propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, methyl formate, methyl acetate, N,N-dimethylacetamide, fluorocarbonic acid Ethylene ester, methyl propionate, ethyl propionate, ethyl acetate, γ-butyrolactone, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, dimethoxymethane, 1,2-dimethoxypropane, triethylene glycol dimethyl ether, dimethyl sulfone, dimethyl ether, vinyl sulfite, propylene sulfite, dimethyl sulfite, diethyl sulfite, crown ether (12-crown-4), 1-ethyl-3-methylimidazole-hexafluorophosphate, 1-ethyl-3-methylimidazole-tetrafluoroborate, 1-ethyl-3-methylimidazole-bis(trifluoromethylsulfonyl)imide salt, 1-propyl-3-methylimidazole-hexafluorophosphate, 1-propyl- One or more of 3-methylimidazole-tetrafluoroborate, 1-propyl-3-methylimidazole-bis(trifluoromethylsulfonyl)imide, 1-butyl-1-methylimidazole-hexafluorophosphate, 1-butyl-1-methylimidazole-tetrafluoroborate, 1-butyl-1-methylimidazole-bis(trifluoromethylsulfonyl)imide, N-butyl-N-methylpyrrolidine-bis(trifluoromethylsulfonyl)imide, 1-butyl-1-methylpyrrolidine-bis(trifluoromethylsulfonyl)imide, N-methyl-N-propylpyrrolidine-bis(trifluoromethylsulfonyl)imide, N-methyl, propylpiperidinium-bis(trifluoromethylsulfonyl)imide and N-butyl-N-methylpiperidinium bis(trifluoromethanesulfonyl)imide.
Citation Information
Patent Citations
Sodium ion battery cathode material sodium bismuth disulfide nanoparticles and preparation method
CN103553129A
Sodium-ion battery anode material sodium lithium titanate and preparation method thereof
CN103633310A
Method for preparing negative electrode material of sodium ion battery
CN103647068A
Sodium ion battery negative electrode material, sodium ion battery and preparation method of sodium ion battery
CN109817960A
Aluminum foil belt of compound metal and preparation method and uses