Additive for silicon wafer texturing, reaction liquid, method and application
By adjusting the composition of additives and alkali solution, a single-step velvet making process is realized to form silicon wafers with terraced pyramid microstructure, solving the problem of two-step velvet making in the existing technology that increases costs and processes, simplifying the process flow and reducing the reflectivity.
Patent Information
- Application Number
- CN202411523342.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-10-30
AI Technical Summary
In the prior art, the silicon wafer wool making process prepared by single crystal silicon solar cells requires two steps to achieve low reflectivity, which increases production costs and processes. Some manufacturers need to transform the wool making machine to achieve efficiency improvement.
By adjusting the composition of the additives, an additive composed of polymer, corrosion inhibitor, anionic surfactant and deionized water is used, and combined with alkali solution, a silicon wafer with a terraced pyramid microstructure is achieved in one step.
Without changing the effect of velvet making, conventional velvet making has been realized from two steps to one step, reducing the reflectivity to 5~8%, simplifying the process flow, and reducing production costs and equipment transformation needs.
Smart Images

Figure CN119041032A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicon wafer processing, and relates to an additive, a reaction liquid, a method and an application for silicon wafer texturing. Background Art
[0002] Normally, the first step in preparing a monocrystalline silicon solar cell is to form a pyramid structure on the surface of the silicon wafer. When light is incident on the pyramid structure, part of the light is directly absorbed, part of the light is refracted and then incident again into the silicon wafer to be absorbed, and part of the light is reflected by the surface of the silicon wafer and cannot be used. The purpose of texturing is to form a velvet surface on the surface of the silicon wafer to reduce the reflectivity of the cell. The uneven velvet surface can increase secondary reflection and change the light path and the incident mode.
[0003] At present, the reflectivity of monocrystalline silicon wafers for solar cells is basically around 10.0%. Increasing the absorption of light is critical. For example, CN202210584582.7 discloses the use of alkali and additives to prepare terraced pyramid microstructures on conventionally textured silicon wafers for secondary preparation, and the reflectivity can be reduced to 4-7%. This method requires two steps to achieve the preparation of terraced pyramid microstructures, and cannot be achieved in one step, that is, on the basis of the conventional texturing process, another texturing is performed to obtain a lower reflectivity; similarly, CN202111532361.7 discloses that two-step texturing will improve the uniformity of the pyramid and improve efficiency; CN202010201512.X discloses a method for preparing a porous pyramid structure using two-step texturing, so two-step texturing can reduce the reflectivity and improve terminal efficiency. For battery manufacturers, although two-step texturing can improve efficiency, it requires increased production costs, and some manufacturers also need to modify the texturing machine to achieve it. Summary of the invention
[0004] The purpose of the present invention is to optimize the conventional texturing process. By changing the additives, the conventional texturing process is changed from two-step texturing to one-step texturing without changing the texturing effect, so as to prepare a silicon wafer with a terraced pyramid microstructure. To this end, the present invention provides an additive, a reaction solution, a method and an application for silicon wafer texturing to solve this need in the art.
[0005] On the one hand, the present invention relates to an additive for silicon wafer texturing, wherein the additive is composed of: 0.3-1.0% of a template agent, 0.1-1.0% of a corrosion inhibitor, 0.1-1.0% of a surfactant, and the balance of deionized water, in terms of mass percentage; The template agent is at least one of high molecular polymers with a molecular weight of not less than 10000Da, and the surfactant is at least one of anionic surfactants and alkyl polyether surfactants.
[0006] Furthermore, in the additive for silicon wafer texturing provided by the present invention, the high molecular weight polymer with a molecular weight of not less than 10000 Da is selected from polydimethyldiallylammonium chloride, polyacrylamide, polyethylene glycol, and gum arabic; The corrosion inhibitor is selected from polyaspartic acid, sodium mercaptobenzothiazole, and catechol; The anionic surfactant is selected from sodium dodecylbenzene sulfonate and sodium lignin sulfonate; The alkyl polyether surfactant is selected from alkyl glycoside and polyethylene glycol ether.
[0007] Furthermore, in the additive for silicon wafer texturing provided by the present invention, the resistivity of the deionized water is greater than 18 MΩ.
[0008] On the other hand, the present invention relates to a reaction solution for texturing silicon wafers, which is obtained by mixing an alkaline solution with a concentration of 1 to 3 wt % and the additive according to any one of claims 1 to 3.
[0009] Furthermore, in the reaction solution for silicon wafer texturing provided by the present invention, the volume ratio of the alkaline solution to the additive is 100:0.1-5.
[0010] Furthermore, in the reaction solution for texturing of silicon wafers provided by the present invention, the alkali in the alkali solution is sodium hydroxide and / or potassium hydroxide.
[0011] On the other hand, the present invention relates to a method for texturing a silicon wafer, comprising: pre-cleaning the silicon wafer and then texturing it after cleaning; the texturing comprises: placing the silicon wafer in the reaction solution described in any one of claims 4 to 6 for reaction, the reaction temperature is 60 to 90°C, and the reaction time is 60s to 420s.
[0012] On the other hand, the present invention relates to a silicon wafer with a terraced pyramid microstructure, which is produced by adopting the silicon wafer texturing method.
[0013] Furthermore, in the silicon wafer with the terraced pyramid microstructure provided by the present invention, the reflectivity of the silicon wafer with the terraced pyramid microstructure is 5-8%.
[0014] On the other hand, the present invention relates to the use of the additive or the reaction solution in silicon wafer texturing.
[0015] Compared with the prior art, the technical solution provided by the present invention has at least the following beneficial effects or advantages: The present invention finds that when texturing silicon wafers, since the adhesion of adsorbents and corrosion inhibitors to silicon wafers in pure water is lower than that of water, the additives in the reaction tank are easily detached, and conventional texturing cannot interrupt the reaction process, resulting in the need to use at least two reaction tanks to achieve the ultimate texturing purpose. Although two-step texturing can improve efficiency, it requires increased production costs, and some manufacturers also need to modify the texturing machines to achieve this. The present invention changes the additives, and without changing the texturing effect, changes conventional texturing from two-step texturing to one-step texturing, thereby preparing a silicon wafer with a terraced pyramid microstructure. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 This is the surface pyramid morphology of the silicon wafer produced in the first reaction tank in Example 1.
[0018] Figure 2 This is the surface pyramid morphology of the silicon wafer produced in the second reaction tank in Example 1.
[0019] Figure 3 This is the surface pyramid morphology of the silicon wafer prepared in Example 2. DETAILED DESCRIPTION
[0020] The technical scheme of the present invention is described below in conjunction with the embodiments, but the present invention is not limited to the following embodiments. The experimental methods and detection methods described in each embodiment are conventional methods unless otherwise specified; the reagents and materials can be purchased on the market unless otherwise specified. The % in the following embodiments, unless otherwise specified, are all mass percentages. The ratios in the following embodiments, unless otherwise specified, are all mass ratios.
[0021] Example 1 This embodiment provides a conventional texturing process.
[0022] For example, the specific process of conventional texturing process is as follows: Step 1: Place the single crystal silicon wafer in a cleaning solution for cleaning; the cleaning solution contains 32% sodium hydroxide, 1.3% hydrogen peroxide, and the balance is water; the cleaning temperature is 65°C and the cleaning time is 2 minutes.
[0023] Step 2: Use a texturing liquid to texturize the cleaned silicon wafer to form a pyramid structure. The texturing liquid is a mixture of 0.22wt% sodium hydroxide solution and an additive (Xi'an Blue Bridge New Energy Technology Co., Ltd., model LQ61-1) at a volume ratio of 400:1. The texturing temperature is 80°C and the texturing time is 200s. The silicon wafer with a pyramid structure formed on the surface is obtained through a conventional texturing process.
[0024] like Figure 1 As shown, the surface of the formed pyramid is smooth and flat without any microstructure formation, and the reflectivity is 11.0% at this time.
[0025] Step 3: Place the single silicon wafer processed in step 2 into a cleaning solution for cleaning at a temperature of 65° C. for 2 minutes.
[0026] Step 4: Add 0.22 wt % sodium hydroxide solution and a microstructure reflectivity reducing additive into deionized water. The sodium hydroxide solution and the additive (microstructure reflectivity reducing additive, Xi'an Blue Bridge New Energy Technology Co., Ltd., model LQ61-2) are mixed in a volume ratio of 200:1 to form a reaction solution, which is stirred evenly after dissolution.
[0027] Step 5: Place the single crystal silicon wafer obtained in step 3 in the reaction solution of step 4 to prepare the microstructure at a temperature of 78° C. for 120 seconds to obtain the following: Figure 2 The single crystal silicon wafer shown has a terraced pyramid single silicon velvet surface.
[0028] Conventional low-reflectivity silicon wafer texturing production needs to be divided into two steps. The silicon wafer enters the first reaction tank to react for 200~400 seconds. After the reaction, the silicon wafer is placed in the second reaction tank to react for 50~150 seconds. There are many processes and a long time.
[0029] Example 2 This embodiment provides a one-step texturing process using specific additives.
[0030] Step 1: Place the single crystal silicon wafer in a cleaning solution for cleaning; the cleaning solution contains 32% sodium hydroxide, 1.3% hydrogen peroxide, and the balance is water; the cleaning temperature is 65°C and the cleaning time is 2 minutes.
[0031] Step 2: prepare an additive consisting of 0.3% polydimethyldiallylammonium chloride, 0.1% polyaspartic acid, 0.1% sodium dodecylbenzene sulfonate, and the remainder deionized water.
[0032] Step 3: Use the reaction liquid to texturize the cleaned silicon wafer to form a pyramid structure. The texturizing temperature is 60° C. and the texturizing time is 60 s. The volume ratio of the reaction liquid to the additive is 100:0.1.
[0033] Example 3 This embodiment provides a one-step texturing process using specific additives.
[0034] Step 1: Place the single crystal silicon wafer in a cleaning solution for cleaning; the cleaning solution contains 32% sodium hydroxide, 1.3% hydrogen peroxide, and the balance is water; the cleaning temperature is 65°C and the cleaning time is 2 minutes.
[0035] Step 2, prepare an additive consisting of 0.3% polydimethyldiallylammonium chloride, 0.2% polyacrylamide, 0.1% polyaspartic acid, 0.2% sodium mercaptobenzothiazole, 0.1% sodium dodecylbenzene sulfonate, 0.3% sodium lignin sulfonate, and the remainder deionized water.
[0036] Step 3: Use the reaction liquid to texturize the cleaned silicon wafer to form a pyramid structure. The texturizing temperature is 70° C. and the texturizing time is 300 s. The volume ratio of the reaction liquid to the additive is 100:1, which is a solution of 1% sodium hydroxide + 1% potassium hydroxide.
[0037] Example 4 This embodiment provides a one-step texturing process using specific additives.
[0038] Step 1: Place the single crystal silicon wafer in a cleaning solution for cleaning; the cleaning solution contains 32% sodium hydroxide, 1.3% hydrogen peroxide, and the balance is water; the cleaning temperature is 65°C and the cleaning time is 2 minutes.
[0039] Step 2, prepare an additive consisting of 0.5% polyethylene glycol (molecular weight: 12000), 0.5% gum arabic (molecular weight: 220000), 0.5% sodium mercaptobenzothiazole, 0.5% catechol, 0.3% sodium dodecylbenzene sulfonate, 0.7% alkyl glycoside, and the balance deionized water.
[0040] Step 3: Use the reaction liquid to texturize the cleaned silicon wafer to form a pyramid structure. The texturizing temperature is 90° C. and the texturizing time is 420 s. The volume ratio of the reaction liquid to the additive is 100:5.
[0041] The parameters of the silicon wafers prepared in various embodiments are shown in Table 1.
[0042] Table 1: Parameters of silicon wafers obtained in various embodiments
[0043] As can be seen from Table 1, the present invention better realizes the texturing of silicon wafers in one reaction tank reaction. Under the premise of not changing the texturing effect, the conventional texturing is changed from two-step texturing to one-step texturing, and a silicon wafer with a terraced pyramid microstructure is prepared.
[0044] As described above, the basic principle, main features and advantages of the present invention are well described. The above embodiments and descriptions are only descriptions of the preferred implementation modes of the present invention, and the present invention is not limited by the above embodiments. Without departing from the spirit and scope of the present invention, various changes and improvements made by ordinary technicians in this field to the technical solution of the present invention should fall within the protection scope determined by the present invention.
Claims
1. An additive for silicon wafer texturing, It is characterized in that In terms of mass percentage, the additive is composed of: 0.3-1.0% of a template, 0.1-1.0% of a corrosion inhibitor, 0.1-1.0% of a surfactant, and the balance of deionized water; The template agent is at least one of high molecular polymers with a molecular weight of not less than 10000Da, and the surfactant is at least one of anionic surfactants and alkyl polyether surfactants.
2. The additive for silicon wafer texturing according to claim 1, It is characterized in that The high molecular weight polymer with a molecular weight of not less than 10000Da is selected from polydimethyldiallyl ammonium chloride, polyacrylamide, polyethylene glycol, and gum arabic; The corrosion inhibitor is selected from polyaspartic acid, sodium mercaptobenzothiazole, and catechol; The anionic surfactant is selected from sodium dodecylbenzene sulfonate and sodium lignin sulfonate; The alkyl polyether surfactant is selected from alkyl glycoside and polyethylene glycol ether.
3. The additive for silicon wafer texturing according to claim 1, It is characterized in that The resistivity of the deionized water is greater than 18 MΩ.
4. A reaction solution for texturing silicon wafers, It is characterized in that The invention is obtained by mixing an alkaline solution with a concentration of 1-3 wt% and the additive according to any one of claims 1-3.
5. The reaction solution for silicon wafer texturing according to claim 4, It is characterized in that The volume ratio of the alkaline solution to the additive is 100:0.1-5.
6. The reaction solution for silicon wafer texturing according to claim 4, It is characterized in that The alkali in the alkali solution is sodium hydroxide and / or potassium hydroxide.
7. A method for texturing a silicon wafer, include: The silicon wafer is pre-cleaned and then texturized after cleaning, wherein the texturizing comprises: placing the silicon wafer in the reaction solution of any one of claims 4 to 6 for reaction, the reaction temperature is 60 to 90° C., and the reaction time is 60s to 420s.
8. A silicon wafer with a terraced pyramid microstructure, It is characterized in that The method for texturing a silicon wafer as claimed in claim 7 is used to prepare the silicon wafer.
9. The silicon wafer having a terraced pyramid microstructure according to claim 8, It is characterized in that The reflectivity of the silicon wafer with the terraced pyramid microstructure is 5-8%.
10. Use of the additive according to any one of claims 1 to 3, or the reaction solution according to any one of claims 4 to 6 in silicon wafer texturing.
Citation Information
Patent Citations
Texturing additive for inverted pyramid textured monocrystalline silicon wafer and application thereof
CN107955974A
Additive for diamond wire polycrystalline silicon chip acidic texturing liquid and application of additive
CN108193280A
Environment-friendly monocrystalline silicon texturing additive and preparation process thereof, monocrystalline silicon texturing liquid and texturing method
CN111647951A
Monocrystalline silicon etching and texturing additive and application thereof
CN112813502A
Texturing additive, texturing liquid and preparation method and application of texturing additive and texturing liquid