Hollow paper tube, preparation method thereof and application of hollow paper tube as hollow cooling section for heating cigarette filter
By incorporating inorganic fibers into the base paper of hollow paper tubes and performing surface treatment, combined with calcium carbonate and adhesives, the problems of insufficient stiffness and resilience of hollow paper tubes are solved, ensuring the appearance quality of cigarettes and making them suitable for industrial production.
Patent Information
- Application Number
- CN202411348705.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-26
AI Technical Summary
The existing hollow paper tubes have insufficient stiffness and poor resilience, making them prone to irreversible deformation and wrinkling during lamination with cellulose acetate filter sections or cigarette rolling, which affects the appearance quality of the cigarettes.
Inorganic fibers, such as basalt fibers or glass fibers, are incorporated into the base paper of hollow paper tubes. The surface of the inorganic fibers is roughened by treatment with sodium hydroxide solution to enhance their bonding force with organic fibers. Combined with calcium carbonate, inorganic adhesives and retention aids, the paper tubes are formed through papermaking and drying, resulting in hollow paper tubes with high stiffness and high resilience.
This method ensures that the hollow paper tube is not easily deformed during the lamination and winding process, maintaining the appearance quality of the cigarette. Moreover, the preparation method is simple, low-cost, and suitable for industrial production.
Smart Images

Figure BDA0005061712350000051 
Figure BDA0005061712350000061
Abstract
Description
Technical Field
[0001] The invention relates to a hollow paper tube, in particular to a hollow paper tube with high stiffness and resilience, and also to a preparation method thereof, and application of the hollow paper tube as a hollow cooling section of a heated cigarette filter, belonging to the technical field of heated cigarettes. Background Art
[0002] As people pay more attention to safety and health, the sales of heated cigarettes in foreign markets are growing. Hollow paper tubes are gradually replacing hollow acetate thin-walled hollow tubes due to their low cost and easy aroma loading, but compared with the latter, hollow paper tubes have some problems in terms of process maturity. For example, the hollow paper tubes are not stiff enough and are easily deformed by slight squeezing; in addition, whether it is when compounding with the acetate filter segment or in the process of cigarette rolling, the rubbing roller will squeeze the paper tube for the firmness of the paper glue. Due to the insufficient resilience of the hollow paper tube, it is easy to cause irreversible deformation, which leads to poor circumference of the filter rod and wrinkles in the process of cigarette rolling, which affects the appearance quality of the cigarette. Summary of the invention
[0003] In view of the technical problems existing in the existing hollow paper tubes, the first object of the present invention is to provide a hollow paper tube with high stiffness and high resilience.
[0004] The second object of the present invention is to provide a method for preparing a hollow paper tube, which method hardly changes the existing processing technology of the hollow paper tube, is simple to operate, has low cost, and can be industrially produced.
[0005] The third object of the present invention is to provide an application of a hollow paper tube, which can replace the existing hollow paper tube for the preparation of heated cigarettes, thereby overcoming the problem that the hollow paper tube is easy to deform and has insufficient resilience and is prone to wrinkles during the composite process of the hollow paper tube and the acetate filter rod or the cigarette rolling process.
[0006] In order to achieve the above technical objectives, the present invention provides a method for preparing a hollow paper tube, which comprises mixing and pulping inorganic fibers and plant fibers to obtain a mixed fiber slurry, soaking the mixed fiber slurry in a sodium hydroxide solution, adding calcium carbonate, an inorganic adhesive and a retention agent, stirring evenly, and then performing net forming, drying and slitting in sequence to obtain base paper, which is spirally formed and rolled into a hollow paper tube.
[0007] The key to the technical solution of the present invention is to add an appropriate amount of inorganic fiber to the base paper of the hollow paper tube. The introduction of inorganic fiber gives the base paper a higher stiffness. However, inorganic fiber has poor compatibility with organic fiber, so the binding performance is poor. The present invention uses alkali solution treatment to not only roughen the surface of inorganic fiber, but also increase the surface hydrogen bond strength of organic fiber through hydrolysis, so that the inorganic fiber and plant fiber are more tightly bound to obtain base paper with better resilience.
[0008] As a preferred solution, the inorganic fiber includes basalt fiber and / or glass fiber. The preferred basalt fiber or glass fiber has a relatively mature industrialization and a low cost. In particular, basalt fiber or glass fiber has good chemical stability, and adding it to the base paper will not affect the smoking quality of the cigarette, and can significantly improve the stiffness of the base paper.
[0009] As a preferred solution, the length of the inorganic fiber is 1 to 8 mm and the diameter is 7 to 15 μm. Selecting inorganic fibers of appropriate size can better blend into organic fibers and improve their dispersibility in organic fibers.
[0010] As a preferred solution, the inorganic fiber is added in an amount of 0.2 to 0.8 times the mass of the plant fiber. Within the preferred range, as the inorganic fiber addition ratio increases, the stiffness of the base paper increases significantly, but if the inorganic fiber ratio is too high, the flexibility of the base paper will be affected.
[0011] As a preferred solution, the plant fiber is composed of coniferous wood pulp and broadleaf wood pulp in a mass ratio of 3:5 to 5:3. Adding the two in a suitable ratio can improve the flexibility of the base paper.
[0012] As a preferred solution, the beating degree of the mixed beating is 40°SR~60°SR.
[0013] As a preferred solution, the concentration of the sodium hydroxide solution is 0.5-20wt%. The concentration of the sodium hydroxide solution is further preferably 1-10wt%. If the concentration of the sodium hydroxide solution is too high, the organic fiber will be excessively degraded, and if the concentration of the sodium hydroxide solution is too low, the purpose of surface modification of the inorganic fiber cannot be achieved.
[0014] As a preferred solution, the soaking treatment time is 2 to 8 hours. If the soaking time is too long, the organic fiber will be excessively degraded, and if the soaking time is too short, the purpose of surface modification of the inorganic fiber cannot be achieved.
[0015] As a preferred solution, the added amount of calcium carbonate is 1-10% of the total mass of the inorganic fiber and the plant fiber.
[0016] As a preferred solution, the amount of the inorganic adhesive added is 2-6% of the total mass of the inorganic fibers and plant fibers.
[0017] As a preferred solution, the amount of the retention agent added is 0.05-2% of the total mass of the inorganic fiber and the plant fiber.
[0018] As a preferred solution, the inorganic adhesive includes silicates and / or water glasses.
[0019] As a preferred solution, the retention aid includes cationic polyacrylamide.
[0020] The calcium carbonate, inorganic adhesive and retention aid of the present invention are commonly used additives in papermaking. For example, calcium carbonate has a whitening effect; the inorganic adhesive has a bonding effect in the papermaking process; the retention aid helps fillers to be adsorbed in fibers in the papermaking process. All of the above are common materials in the papermaking process.
[0021] As a preferred solution, the drying is carried out using two groups of drying cylinders, wherein the pressure of the rollers in the drying cylinders of the first group of drying cylinders is 80-100 kg / cm, the drying cylinder temperature is 110-130°C, and the drying time is 10-20 min; the pressure of the rollers in the drying cylinders of the second group of drying cylinders is 40-60 kg / cm, the drying cylinder temperature is 80-100°C, and the drying time is 20-30 min.
[0022] As a preferred solution, the hollow paper tube comprises an inner and outer layer; the gram weight of the inner layer of paper is 100-200 g / m 2 , thickness is 0.2~0.3mm, outer paper weight is 40~100g / m 2 , thickness is 0.1~0.2mm.
[0023] The present invention also provides a hollow paper tube obtained by the preparation method. Compared with the conventional hollow paper tube, the hollow paper tube prepared by the present invention has high stiffness and high resilience.
[0024] The present invention also provides an application of a hollow paper tube, which is used as a hollow cooling section of a filter tip for preparing heated cigarettes. The hollow paper tube of the present invention replaces the existing hollow paper tube to prepare heated cigarettes, and during the process of compounding with the acetate filter tip section or rolling the cigarette, it exhibits high stiffness and high resilience, and will not undergo irreversible deformation, thereby ensuring the appearance quality of the cigarette.
[0025] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:
[0026] Compared with the existing hollow paper tubes, the hollow paper tubes of the present invention have higher stiffness and resilience. During the process of compounding with the acetate filter segment or rolling the cigarette, no irreversible deformation or wrinkles will occur, thereby ensuring the appearance quality of the cigarette.
[0027] The hollow paper tube preparation method of the present invention is simple to operate, low in cost, and can be industrially produced. DETAILED DESCRIPTION
[0028] The following specific examples are intended to further illustrate the present invention in detail, rather than to limit the scope of protection of the claims.
[0029] Unless otherwise specified in the following examples, the chemical reagents used are all commercial reagents.
[0030] The basalt fibers and glass fibers in the following examples are commercial products, with a length of 1 to 8 mm and a diameter of 7 to 15 μm.
[0031] Example 1
[0032] The mass ratio of basalt fiber and plant fiber (coniferous wood pulp and hardwood pulp, mass ratio of 5:5) is 1:2. After being mixed and beaten (beating degree 50°SR), they are soaked in a 1wt% sodium hydroxide aqueous solution for 2h, and calcium carbonate (5% of fiber mass), silicate inorganic adhesive (2% of fiber mass) and retention agent cationic polyacrylamide (1% of fiber mass) are added in sequence to obtain a composite slurry; after being formed by fourdrinier sheeting, it is dried (two sets of drying cylinders are used for drying, The pressure of the rollers in the first drying cylinder is 100kg / cm, the drying cylinder temperature is 130℃, and the drying time is 20min; the pressure of the rollers in the second drying cylinder is 60kg / cm, the drying cylinder temperature is 100℃, and the drying time is 30min) and after slitting, a hollow paper tube base paper is obtained, and the paper tube paper is spirally formed into a hollow paper tube (the paper tube paper includes an inner paper tube paper and an outer paper tube paper, and the gram weight of the inner paper tube paper is 180g / m 2 , thickness is 0.3mm, outer paper tube paper weight is 40g / m 2 , thickness is 0.1mm).
[0033] The prepared hollow paper tubes were tested in the following aspects:
[0034] 1. Test the hardness of the hollow paper tube according to the method of GB / T22838 "Determination of physical properties of cigarettes and filter rods";
[0035] 2. Since there is no relevant standard for the elasticity measurement of paper tubes, the present invention establishes a relevant paper tube measurement method based on the diameter compression range of 1 to 2 mm during the actual hollow paper tube compounding and cigarette rolling process, as follows:
[0036] (1) Placing the prepared hollow paper tube at the center of the compression test platform;
[0037] (2) Drive the instrument to slowly compress the hollow paper tube, and stop when the compression amount reaches 2 mm in the diameter direction;
[0038] (3) After the compression stops, move in the opposite direction at the same speed until the instrument recovers;
[0039] (4) Measure the diameter D1 of the hollow paper tube before compression and the diameter D2 after compression and rebound, and calculate the rebound rate of the hollow paper tube R = D2 / D1×100%.
[0040] Example 2
[0041] The glass fiber and plant fiber (coniferous wood pulp and hardwood pulp, mass ratio of 3:5) are mixed and beaten (beating degree 60°SR) and then soaked in a 5wt% sodium hydroxide aqueous solution for 4h, and calcium carbonate (10% of fiber mass), water glass inorganic adhesive (4% of fiber mass) and retention agent cationic polyacrylamide (0.5% of fiber mass) are added in sequence to obtain a composite slurry; after forming by fourdrinier sheeting, it is dried (two sets of drying cylinders are used for drying, The pressure of the rollers in the first drying cylinder is 100kg / cm, the drying cylinder temperature is 130℃, and the drying time is 20min; the pressure of the rollers in the second drying cylinder is 60kg / cm, the drying cylinder temperature is 100℃, and the drying time is 30min) and after slitting, a hollow paper tube base paper is obtained, and the paper tube paper is spirally formed into a hollow paper tube (the paper tube paper includes an inner paper tube paper and an outer paper tube paper, and the gram weight of the inner paper tube paper is 180g / m 2 , thickness is 0.3mm, outer paper tube paper weight is 40g / m 2 , thickness is 0.1mm).
[0042] Example 3
[0043] The glass fiber and plant fiber (coniferous wood pulp and hardwood pulp, mass ratio of 3:5) are mixed and beaten (beating degree 55°SR) and then soaked in a 10wt% sodium hydroxide aqueous solution for 8h, and calcium carbonate (10% of fiber mass), water glass inorganic adhesive (5% of fiber mass) and retention agent cationic polyacrylamide (1% of fiber mass) are added in sequence to obtain a composite slurry; after forming by fourdrinier sheeting, the slurry is dried (two sets of drying cylinders are used for drying, The pressure of the rollers in the first drying cylinder is 100kg / cm, the drying cylinder temperature is 130℃, and the drying time is 20min; the pressure of the rollers in the second drying cylinder is 60kg / cm, the drying cylinder temperature is 100℃, and the drying time is 30min) and after slitting, a hollow paper tube base paper is obtained, and the paper tube paper is spirally formed into a hollow paper tube (the paper tube paper includes an inner paper tube paper and an outer paper tube paper, and the gram weight of the inner paper tube paper is 180g / m 2 , thickness is 0.3mm, outer paper tube paper weight is 40g / m 2 , thickness is 0.1mm).
[0044] Comparative Example 1
[0045] The difference from Example 1 is that the hollow paper tube is prepared by a conventional method without adding basalt fiber and soaking in sodium hydroxide aqueous solution.
[0046] Comparative Example 2
[0047] The difference from Example 1 is that the prepared paper tube only has basalt fiber added thereto, and is not soaked in a sodium hydroxide aqueous solution.
[0048] Comparative Example 3
[0049] The difference from Example 1 is that during the preparation process of the paper tube, after mixing and pulping, the paper tube is immersed in a 60 wt % sodium hydroxide aqueous solution for 2 hours.
[0050] Comparative Example 4
[0051] The difference from Example 1 is that the mass ratio of basalt fiber: plant fiber (coniferous wood pulp and hardwood wood pulp, mass ratio of 5:5) is 3:1.
[0052] Table 1 Comparison of stiffness of paper tubes prepared in Example and Comparative Example
[0053] Hardness test value / % Example 1 93 Example 2 95 Example 3 98 Comparative Example 1 81 Comparative Example 2 87 Comparative Example 3 51 Comparative Example 4 80
[0054] Table 2 Comparison of paper tube resilience prepared in Example and Comparative Example
[0055]
[0056]
Claims
1. A method for preparing a hollow paper tube, characterized in that: The inorganic fiber and the plant fiber are mixed and pulped to obtain a mixed fiber slurry, which is soaked in a sodium hydroxide solution, and then calcium carbonate, an inorganic adhesive and a retention aid are added and stirred evenly, followed by screen forming, drying and slitting to obtain base paper, which is spirally formed and rolled into a hollow paper tube.
2. The method for preparing a hollow paper tube according to claim 1, characterized in that: The inorganic fibers include basalt fibers and / or glass fibers.
3. The method for preparing a hollow paper tube according to claim 2, characterized in that: The inorganic fiber has a length of 1 to 8 mm and a diameter of 7 to 15 μm.
4. A method for preparing a hollow paper tube according to claim 2 or 3, characterized in that: The mixing ratio of the inorganic fiber is 0.2 to 0.8 times the mass of the plant fiber.
5. The method for preparing a hollow paper tube according to claim 4, characterized in that: The plant fiber is composed of coniferous wood pulp and broadleaf wood pulp in a mass ratio of 3:5 to 5:
3.
6. The method for preparing a hollow paper tube according to claim 1, characterized in that: The beating degree of the mixed beating is 40°SR~60°SR.
7. The method for preparing a hollow paper tube according to claim 1, characterized in that: The concentration of the sodium hydroxide solution is 0.5-20 wt %.
8. The method for preparing a hollow paper tube according to claim 1 or 7, characterized in that: The soaking treatment time is 2 to 8 hours.
9. The method for preparing a hollow paper tube according to claim 1, characterized in that: The amount of calcium carbonate added is 1 to 10% of the total mass of the inorganic fiber and the plant fiber; The amount of the inorganic adhesive added is 2-6% of the total mass of the inorganic fiber and the plant fiber; The addition amount of the retention aid is 0.05-2% of the total mass of the inorganic fiber and the plant fiber.
10. The method for preparing a hollow paper tube according to claim 1, characterized in that: The inorganic adhesive includes silicates and / or water glasses; The retention aid includes cationic polyacrylamide.
11. The method for preparing a hollow paper tube according to claim 1, characterized in that: The drying is carried out using two groups of drying cylinders, wherein the pressure of the rollers in the drying cylinders of the first group of drying cylinders is 80-100 kg / cm, the drying cylinder temperature is 110-130°C, and the drying time is 10-20 min; the pressure of the rollers in the drying cylinders of the second group of drying cylinders is 40-60 kg / cm, the drying cylinder temperature is 80-100°C, and the drying time is 20-30 min.
12. The method for preparing a hollow paper tube according to claim 1, characterized in that: The hollow paper tube includes two layers, inner and outer; the gram weight of the inner layer of paper is 100-200g / m 2 , thickness is 0.2~0.3mm, outer paper weight is 40~100g / m 2 , thickness is 0.1~0.2mm.
13. A hollow paper tube, characterized in that: The method is obtained by the preparation method according to any one of claims 1 to 12.
14. The use of a hollow paper tube according to claim 13, characterized in that: The hollow cooling section as a filter tip is used in the preparation of heated cigarettes.
Citation Information
Patent Citations
Sepiolite antibacterial cigarette filter tip paper and preparation method
CN107713007A
Paper tube with functions of reducing smoke temperatures and releasing aroma and application of paper tube
CN107960680A
Glass fiber toughening composite aerogel and preparation method thereof
CN109463796A
Preparation method of basalt fiber paper
CN110219201A
Aroma-enhancing and moisture-retaining hollow pipe for heating cigarettes and preparation method thereof