Cement clinker calcining system and calcining method
By using kaolin calcined components in cement production to activate kaolin and add it to the discharge side of the cement calcined components, the problems of high cement clinker usage and energy consumption are solved, and the effect of reducing carbon emissions and improving the performance of cement products is achieved.
Patent Information
- Application Number
- CN202411139303.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-29
AI Technical Summary
The carbon dioxide emissions caused by clinker calcination during cement production account for more than 60% of the total production process, and the clinker consumption and energy consumption are relatively high, so it needs to be reduced.
Using kaolin calcined components, including preheaters and decomposition furnaces, preheat the raw materials through a multi-stage cyclone, and calcinate activated kaolin in an oxygen-rich or CO reduction atmosphere in the decomposition furnace. After generating activated kaolin, it is added to the cement calcined components. On the discharge side, coordinated cooling and reuse are carried out to adjust the hydration rate and structural activity of cement clinker.
It reduces the use of carbon-containing raw materials in clinker production, reduces carbon emissions, improves the surface area and structural activity of cement clinker, enhances the adhesion and durability of the final cement product, and achieves overall energy-saving and carbon reduction in the calcining system.
Smart Images

Figure CN119043015A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cement preparation, and in particular to a cement clinker calcining system and a calcining method. Background Art
[0002] In the production process of cement materials, the main carbon dioxide emissions come from the decomposition of carbonate minerals during clinker calcination, which can account for more than 60% of the total production process. Therefore, the development of alternative raw materials and production process energy-saving and consumption-reducing technologies to reduce the amount of clinker and energy consumption in cement are the main measures currently taken by the cement industry. Summary of the invention
[0003] In view of this, the present invention provides a cement clinker calcining system and a calcining method to solve the problem of high clinker usage and energy consumption in cement.
[0004] In a first aspect, the present invention provides a cement clinker calcining system, the calcining system comprising:
[0005] Kaolin calcining components, including preheaters and decomposition furnaces;
[0006] The preheater is provided with a multi-stage cyclone; the preheater is provided with a feed inlet and a discharge outlet;
[0007] The decomposition furnace is provided with a fuel addition port and a raw material inlet; the raw material inlet is connected to the discharge port; the decomposition furnace is calcined to generate activated kaolin;
[0008] The calcination temperature in the decomposition furnace is between 700° C. and 850° C., the calcination time is between 0 and 1.5 hours, and the calcination atmosphere in the decomposition furnace is an oxygen-rich atmosphere or a CO reducing atmosphere;
[0009] The cement calcining component is used for calcining to generate cement clinker; the activated kaolin is added to the discharge side of the cement calcining component according to the predetermined proportion of the activated kaolin in the cement clinker.
[0010] Beneficial effects: The embodiment of the present invention can reduce the use of carbon-containing raw materials in clinker production, reduce clinker carbon emissions, and adjust the hydration rate of cement clinker by adding kaolin on the basis of the original cement raw material ratio. It can also realize the calcination activation of kaolin, and at the same time, the calcined kaolin is added to the discharge side of the cement calcination component, for example, it can be the discharge port of the rotary kiln head or the feed port of the grate cooler for coordinated cooling, so as to achieve the overall energy saving and carbon reduction of the calcination system. In addition, the layered aluminosilicate structure in kaolin is dehydrated and decomposed at high temperature, resulting in its structural reorganization. The six-coordinated aluminum ions are transformed into four-coordinated active alumina, and this form of aluminum has higher chemical reactivity. Some silicon-oxygen bonds in the layered structure are broken to form island-shaped active silicon oxide, which also enhances the activity of the material. At the same time, the specific surface area increases, the average pore size and pore volume change, so that the surface area of the material increases, and the internal structure becomes more porous, which is conducive to improving the contact area with other substances and the reaction efficiency. This increases the number of active sites on the surface and structure of cement clinker, significantly improving the performance of the final cement product, such as enhancing its adhesion, improving durability or adjusting other physical and chemical properties.
[0011] In an optional embodiment, the preheater is provided with three-stage cyclone cylinders, namely, a first cyclone cylinder, a second cyclone cylinder and a third cyclone cylinder;
[0012] The first cyclone is provided with a first air inlet and two first cyclones arranged in parallel at the end of the first air inlet, the first air inlet is provided with a first air inlet and the feed port; the top of the first cyclone is provided with a first exhaust port, and the bottom of the first cyclone is provided with a first discharge port;
[0013] The second cyclone is provided with a second air inlet and a second cyclone connected to the end of the second air inlet; the second air inlet is provided with a second air inlet and a pair of return ports, the top of the second cyclone is provided with a second exhaust port, and the bottom of the second cyclone is provided with a second discharge port;
[0014] A pair of the return ports are respectively connected to the two first discharge ports; the second exhaust port is connected to the first air inlet, and the second discharge port forms the discharge port of the preheater;
[0015] The third cyclone is provided with a third air inlet and a third cyclone; one end of the third air inlet is connected to the smoke exhaust port of the decomposition furnace, and the other end of the third air inlet is connected to the third cyclone; the top of the third cyclone is provided with a third exhaust port, and the bottom of the third cyclone is provided with a third discharge port;
[0016] The third exhaust port is connected to the second air inlet, and the third discharge port discharges waste materials outward.
[0017] In a first embodiment, the calcination temperature in the decomposition furnace is 750° C., the calcination time is 1 hour, and the calcination atmosphere in the decomposition furnace is an oxygen-rich atmosphere.
[0018] In the first embodiment, the activated kaolin is added into the cement calcining assembly at a ratio of 10%.
[0019] In a second embodiment, the area of the second exhaust port of the second cyclone is 1.4 m 2 Up to 1.6m 2 The height of the outer cylinder of the second cyclone is between 1.9m and 2.1m; the decomposition furnace has two fuel addition ports and a single raw material inlet, and the fuel addition port is located on one side of the raw material inlet.
[0020] In a second embodiment, the calcination temperature is between 700° C. and 850° C., the calcination time is 1 hour, and the calcination atmosphere in the decomposition furnace is a CO atmosphere.
[0021] In a second embodiment, the activated kaolin is added to the cement calcining assembly at a ratio of 15%.
[0022] In the third embodiment, a CO reduction tube is added between the second air inlet and the third exhaust port of the third cyclone; the decomposition furnace has three fuel addition ports and three raw material inlets, the fuel addition port is arranged opposite to all the raw material inlets, and along the wind flow direction, the fuel addition port is located upstream of the raw material inlet.
[0023] In the third embodiment, the calcination temperature is 750° C., the calcination time is 1.5 hours, and the calcination atmosphere is a CO atmosphere.
[0024] In a third embodiment, the activated kaolin is added into the cement calcining assembly at a ratio of 20%.
[0025] In a fourth embodiment, the air inlet of the decomposition furnace is connected to an extension pipe, an end of the extension pipe away from the air inlet is connected to an inlet pipe, and the end of the inlet pipe is trumpet-shaped;
[0026] Two raw meal inlets are symmetrically arranged on the inlet pipe, and two fuel addition ports are arranged at one end of the extension pipe close to the inlet pipe. The third raw meal inlet and the third fuel addition port are located on the extension pipe, and the feeding direction of the third raw meal inlet and the feeding direction of the third fuel addition port are both at right angles to the extension direction of the feed pipe; the feed pipe is arranged between the preheater and the decomposition furnace.
[0027] In a fourth embodiment, the calcination temperature is 750° C., the calcination time is 0.5 to 1.5 hours, and the calcination atmosphere is a CO 165 ppm atmosphere.
[0028] In a fourth embodiment, the activated kaolin is added into the cement calcining assembly at a ratio of 5%.
[0029] In a second aspect, the present invention further provides a method for calcining cement clinker, the calcining method comprising:
[0030] The cement raw material and kaolin are dried and ground separately to obtain cement raw meal and kaolin raw meal;
[0031] Adding the cement raw material into a cement calcining assembly for high-temperature calcination to generate cement clinker;
[0032] and passing the kaolin raw material into a kaolin calcining assembly for calcination and activation to generate activated kaolin;
[0033] Adding the activated kaolin to the discharge side of the cement calcining component according to the predetermined proportion of the activated kaolin in the cement clinker;
[0034] The mixture of cement clinker and activated kaolin is cooled by a grate cooler to obtain cement clinker containing kaolin.
[0035] In an optional embodiment, the grinding of kaolin comprises:
[0036] When kaolin is ground, the fineness of the ground kaolin powder is controlled to be between 75 μm and 85 μm, and the sieve residue is 4% to 6%.
[0037] In an optional embodiment, the adding of the activated kaolin to the discharge side of the cement calcining assembly comprises:
[0038] The activated kaolin is added into the discharge port of the cement calcining component and the feed port of the active grate cooler. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the related technologies, the drawings required for use in the specific embodiments or the related technical descriptions will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0040] Figure 1 It is a schematic diagram of the structure of the preheater and the decomposition furnace in the embodiment of the present invention;
[0041] Figure 2It is a schematic diagram of the structure of the first cyclone in an embodiment of the present invention;
[0042] Figure 3 Schematic diagram of the structure of the second cyclone in an embodiment of the present invention;
[0043] Figure 4 It is a schematic diagram of the structure of the third cyclone in an embodiment of the present invention;
[0044] Figure 5 This is a schematic diagram of the structure of the decomposition furnace in Example 4.
[0045] Description of reference numerals:
[0046] 1. Preheater;
[0047] 11. first cyclone; 111. first air inlet; 1111. first air inlet; 1112. feed inlet; 112. first cyclone; 1121. first exhaust outlet; 1122. first discharge outlet;
[0048] 12, second cyclone; 121, second air inlet; 1211, second air inlet; 1212, return port; 122, second cyclone; 1221, second exhaust port; 1222, second discharge port;
[0049] 13. third cyclone; 131. third air inlet; 132. third cyclone; 1321. third exhaust port; 1322. third material discharge port;
[0050] 2. Decomposition furnace; 21. Extension pipe; 22. Inlet pipe; 23. Raw material inlet; 24. Fuel addition port. DETAILED DESCRIPTION
[0051] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0052] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0053] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, it can also be the internal communication of two components, it can be a wireless connection, or it can be a wired connection. For ordinary workers in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0054] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0055] In the production process of cement materials, the main carbon dioxide emissions come from the decomposition of carbonate minerals during clinker calcination, which can account for more than 60% of the total production process. Therefore, the development of alternative raw materials and production process energy-saving and consumption-reducing technologies to reduce the amount of clinker and energy consumption in cement are the main measures currently taken by the cement industry.
[0056] In view of this, the present invention provides a cement clinker calcining system and a calcining method to solve the problem of high clinker usage and energy consumption in cement.
[0057] Combine the following Figures 1 to 5 , describing an embodiment of the present invention.
[0058] According to an embodiment of the present invention, on one hand, a cement clinker calcining system is provided, the calcining system comprising a kaolin calcining component and a cement calcining component.
[0059] Specifically, in the embodiment of the present invention, the kaolin calcining assembly includes a preheater 1 and a decomposition furnace 2 .
[0060] Furthermore, the preheater 1 is provided with a multi-stage cyclone, and the preheater 1 is provided with a feed port 1112, a discharge port and a waste port. Raw meal powder is added from the feed port 1112, and the newly added cold raw meal will come into contact with the hot flue gas from the decomposition furnace 2. Through direct heat exchange, the raw meal is gradually heated, and the flue gas is gradually cooled, thereby realizing step-by-step heat recovery. In the multi-stage cyclone system, the raw meal will pass through multiple cyclone separators in sequence. After each stage, the temperature of the raw meal will increase, and the temperature of the flue gas will gradually decrease until it enters the decomposition furnace 2 through the discharge port. The waste port can return the large particles with heavier weight in the raw meal to the grinding system for grinding processing, and the raw meal powder after re-grinding can be added to the preheater 1 again through the feed port 1112.
[0061] Furthermore, the decomposition furnace 2 is provided with a fuel addition port 24 and a raw material inlet 23, and the raw material inlet 23 is connected to the discharge port; the decomposition furnace 2 calcines to generate activated kaolin. The calcination temperature in the decomposition furnace 2 is between 700°C and 850°C, the calcination time is between 0 and 1.5 hours, and the calcination atmosphere in the decomposition furnace 2 is an oxygen-rich atmosphere or a CO reducing atmosphere.
[0062] Furthermore, the cement calcining assembly may be a rotary kiln, which is used to calcine cement clinker, and the activated kaolin is added to the discharge side of the cement calcining assembly at a predetermined ratio of the activated kaolin in the cement clinker. The predetermined ratio may be, for example, 5%, 10%, 15%, 20%, etc.
[0063] The embodiment of the present invention can reduce the use of carbon-containing raw materials in clinker production, reduce clinker carbon emissions, and adjust the hydration rate of cement clinker by adding kaolin on the basis of the original cement raw material ratio. It is also possible to achieve calcination activation of kaolin, and at the same time, add the calcined kaolin to the discharge side of the cement calcination component, such as the rotary kiln head discharge port or the grate cooler feed port for coordinated cooling, so as to achieve overall energy saving and carbon reduction of the calcination system. In addition, the layered aluminosilicate structure in kaolin is dehydrated and decomposed at high temperature, resulting in its structural reorganization. The six-coordinated aluminum ions are converted into four-coordinated active alumina, and this form of aluminum has higher chemical reactivity. Some silicon-oxygen bonds in the layered structure are broken to form island-shaped active silicon oxide, which also enhances the activity of the material. At the same time, the specific surface area increases, the average pore size and pore volume change, so that the surface area of the material increases, and the internal structure becomes more porous, which is conducive to improving the contact area and reaction efficiency with other substances. This increases the number of active sites on the surface and structure of cement clinker, significantly improving the performance of the final cement product, such as enhancing its adhesion, improving durability or adjusting other physical and chemical properties.
[0064] Furthermore, in an optional embodiment, the preheater 1 is provided with three-stage cyclones, namely a first cyclone 11 , a second cyclone 12 and a third cyclone 13 .
[0065] In the embodiment of the present invention, the first cyclone 11 is provided with a first air inlet 111 and two first cyclones 112 arranged in parallel at the end of the first air inlet 111, and the first air inlet 111 is provided with a first air inlet 1111 and the feed port 1112. The top of the first cyclone 112 is provided with a first exhaust port 1121, and the bottom of the first cyclone 112 is provided with a first discharge port 1122.
[0066] Furthermore, the second cyclone 12 is provided with a second air inlet 121 and a second cyclone 122 connected to the end of the second air inlet 121. The second air inlet 121 is provided with a second air inlet 1211 and a pair of return ports 1212, the top of the second cyclone 122 is provided with a second exhaust port 1221, and the bottom of the second cyclone 122 is provided with a second discharge port 1222.
[0067] Regarding the connection mode of the second cyclone 12, a pair of the return ports 1212 are respectively connected to the two first discharge ports 1122; the second exhaust port 1221 is connected to the first air inlet 1111, and the second discharge port 1222 forms the discharge port of the preheater 1;
[0068] Further, the third cyclone 13 is provided with a third air inlet 131 and a third cyclone 132; one end of the third air inlet 131 is connected to the smoke exhaust port of the decomposition furnace 2, and the other end of the third air inlet 131 is connected to the third cyclone 132. The top of the third cyclone 132 is provided with a third exhaust port 1321, and the bottom of the third cyclone 132 is provided with a third discharge port 1322, and the third discharge port 1322 forms the waste port of the preheater 1.
[0069] As for the connection mode of the third cyclone 13 , the third exhaust port 1321 is connected to the second air inlet 1211 , and the third discharge port 1322 discharges waste materials outward.
[0070] In order to illustrate the present invention and better understand the technical solutions and advantages of the present invention, the present invention will be described in detail below in conjunction with embodiments and drawings, but the present invention is not limited to the following embodiments.
[0071] Embodiment 1:
[0072] In the first embodiment, the calcination temperature in the decomposition furnace 2 is 750° C., the calcination time is 1 hour, and the calcination atmosphere in the decomposition furnace 2 is an oxygen-rich atmosphere. The chemical composition of kaolin is shown in Table 1.
[0073]
[0074] Table 1 Chemical composition of kaolin
[0075] In the first embodiment, the activated kaolin is added into the cement calcining assembly at a ratio of 10%.
[0076] The addition position is the feeding port of the grate cooler. The 3-day, 7-day and 28-day flexural and compressive strengths of the produced kaolin-containing cement clinker are measured in accordance with GB / T17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)", and the results are shown in Table 2.
[0077]
[0078]
[0079] Table 2 Strength test results of kaolin-containing cement clinker calcined in nutrient-rich atmosphere
[0080] Embodiment 2:
[0081] In the second embodiment, the area of the second exhaust port 1221 of the second cyclone 122 is 1.4 m 2 Up to 1.6m 2 The outer cylinder height of the second cyclone 122 is between 1.9m and 2.1m; the decomposition furnace 2 has two fuel addition ports 24 and a single raw material inlet 23, and the fuel addition port 24 is located on one side of the raw material inlet 23. In the second embodiment, the calcination temperature is between 700°C and 850°C, the calcination time is 1 hour, and the calcination atmosphere in the decomposition furnace 2 is a CO atmosphere. The chemical composition of kaolin is shown in Table 3.
[0082]
[0083] Table 3 Chemical composition of kaolin
[0084] In a second embodiment, the activated kaolin is added to the cement calcining assembly at a ratio of 15%. The addition location is the kiln head discharge port. The 3-day, 7-day and 28-day flexural and compressive strengths of the produced kaolin-containing cement clinker are measured in accordance with GB / T17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)", and the results are shown in Table 4.
[0085]
[0086] Table 4 Strength test results of kaolin-containing cement clinker calcined at different temperatures
[0087] Embodiment 3:
[0088] In the third embodiment, compared with the first two embodiments, the sizes of the cyclones at each level are increased. A CO reduction tube is added between the second air inlet 1211 and the third exhaust port 1321 of the third cyclone 132. The decomposition furnace 2 has three fuel addition ports 24 and three raw material inlets 23. The fuel addition ports 24 are arranged opposite to all the raw material inlets 23, and along the wind flow direction, the fuel addition ports 24 are located upstream of the raw material inlets 23.
[0089] In the third embodiment, the calcination temperature is 750° C., the calcination time is 1.5 hours, and the calcination atmosphere is CO atmosphere. The chemical composition of kaolin is shown in Table 5.
[0090]
[0091] Table 5 Chemical composition of kaolin
[0092] In the third embodiment, the activated kaolin is added to the cement calcining assembly at a ratio of 20%. The addition location is the kiln head discharge port. The 3-day, 7-day and 28-day flexural and compressive strengths of the produced kaolin-containing cement clinker are measured in accordance with GB / T17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)", and the results are shown in Table 6.
[0093]
[0094] Table 6 Strength test results of kaolin-containing cement clinker calcined in reducing atmosphere
[0095] Embodiment 4:
[0096] In the fourth embodiment, the air inlet of the decomposition furnace 2 is connected to an extension pipe 21, and the end of the extension pipe 21 away from the air inlet is connected to an inlet pipe 22, and the end of the inlet pipe 22 is trumpet-shaped. Two raw material inlets 23 are symmetrically arranged on the inlet pipe 22, and two fuel addition ports 24 are arranged at the end of the extension pipe 21 close to the inlet pipe 22, and the third raw material inlet 23 and the third fuel addition port 24 are located on the extension pipe 21, and the feeding direction of the third raw material inlet 23 and the feeding direction of the third fuel addition port 24 are both at right angles to the extension direction of the feed pipe; the feed pipe is arranged between the preheater 1 and the decomposition furnace 2.
[0097] In the fourth embodiment, the calcination temperature is 750° C., the calcination time is 0.5 to 1.5 hours, and the calcination atmosphere is a CO 165 ppm atmosphere. The chemical composition of kaolin is shown in Table 7.
[0098]
[0099] Table 7 Chemical composition of kaolin
[0100] In a fourth embodiment, the activated kaolin is added to the cement calcining assembly at a ratio of 5%. The addition location is the feed port of the grate cooler. The 3-day, 7-day and 28-day flexural and compressive strengths of the produced kaolin-containing cement clinker are measured in accordance with GB / T17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)", and the results are shown in Table 8.
[0101]
[0102] Table 8 Strength test results of cement clinker containing kaolin calcined at different times
[0103] In a second aspect, the present invention further provides a method for calcining cement clinker, the calcining method comprising the following steps:
[0104] S1, drying the cement raw material and kaolin respectively and then grinding them to obtain cement raw material and kaolin raw material;
[0105] S2, adding the cement raw material into a cement calcining assembly for high temperature calcination to generate cement clinker;
[0106] S3, passing the kaolin raw material into a kaolin calcining assembly for calcination and activation to generate activated kaolin;
[0107] S4, adding the activated kaolin to the cement clinker at a predetermined proportion to the discharge side of the cement calcining assembly;
[0108] S5. Cooling the mixture of cement clinker and activated kaolin using a grate cooler to obtain cement clinker containing kaolin.
[0109] Further, in an optional embodiment, the grinding of kaolin comprises:
[0110] When kaolin is ground, the fineness of the ground kaolin powder is controlled to be between 75 μm and 85 μm, and the sieve residue is 4% to 6%.
[0111] Further, in an optional embodiment, the adding of the activated kaolin to the discharge side of the cement calcining assembly comprises:
[0112] The activated kaolin is added into the discharge port of the cement calcining component and the feed port of the active grate cooler.
[0113] Although the embodiments of the present invention have been described in conjunction with the accompanying drawings, those skilled in the art may make various modifications and variations without departing from the spirit and scope of the present invention, and such modifications and variations are all within the scope defined by the appended claims.
Claims
1. A cement clinker calcining system, characterized in that: include: A kaolin calcining assembly comprises a preheater (1) and a decomposition furnace (2); The preheater (1) is provided with a multi-stage cyclone; the preheater (1) is provided with a feed inlet (1112) and a discharge outlet; The decomposition furnace (2) is provided with a fuel addition port (24) and a raw material inlet (23); the raw material inlet (23) is connected to the discharge port; the decomposition furnace (2) is calcined to generate activated kaolin; The calcination temperature in the decomposition furnace (2) is between 700° C. and 850° C., the calcination time is between 0 and 1.5 hours, and the calcination atmosphere in the decomposition furnace (2) is an oxygen-rich atmosphere or a CO reducing atmosphere; Cement calcining component, used for calcining to produce cement clinker; The activated kaolin is added to the discharge side of the cement calcining component at a predetermined ratio of the activated kaolin in the cement clinker.
2. The calcining system according to claim 1, characterized in that: The preheater (1) is provided with three-stage cyclone cylinders, namely a first cyclone cylinder (11), a second cyclone cylinder (12) and a third cyclone cylinder (13); The first cyclone cylinder (11) is provided with a first air inlet cylinder (111) and two first cyclones (112) arranged in parallel at the end of the first air inlet cylinder (111); the first air inlet cylinder (111) is provided with a first air inlet (1111) and the feed port (1112); the top of the first cyclone (112) is provided with a first exhaust port (1121), and the bottom of the first cyclone (112) is provided with a first discharge port (1122); The second cyclone cylinder (12) is provided with a second air inlet cylinder (121) and a second cyclone (122) connected to the end of the second air inlet cylinder (121); the second air inlet cylinder (121) is provided with a second air inlet (1211) and a pair of return ports (1212); the top of the second cyclone (122) is provided with a second exhaust port (1221); the bottom of the second cyclone (122) is provided with a second discharge port (1222); A pair of the return ports (1212) are respectively connected to the two first discharge ports (1122); the second exhaust port (1221) is connected to the first air inlet (1111), and the second discharge port (1222) forms the discharge port of the preheater (1); The third cyclone cylinder (13) is provided with a third air inlet cylinder (131) and a third cyclone (132); one end of the third air inlet cylinder (131) is connected to the smoke exhaust port of the decomposition furnace (2), and the other end of the third air inlet cylinder (131) is connected to the third cyclone (132); the top of the third cyclone (132) is provided with a third exhaust port (1321), and the bottom of the third cyclone (132) is provided with a third discharge port (1322); The third exhaust port (1321) is connected to the second air inlet (1211), and the third discharge port (1322) discharges waste materials to the outside.
3. The calcining system according to claim 2, characterized in that: The calcination temperature in the decomposition furnace (2) is 750° C., the calcination time is 1 hour, and the calcination atmosphere in the decomposition furnace (2) is an oxygen-rich atmosphere.
4. The calcining system according to claim 3, characterized in that: The activated kaolin was added into the cement calcining assembly at a ratio of 10%.
5. The calcining system according to claim 2, characterized in that: The area of the second exhaust port (1221) of the second cyclone (122) is 1.4 m 2 Up to 1.6m 2 The outer cylinder height of the second cyclone (122) is between 1.9m and 2.1m; the decomposition furnace (2) has two fuel addition ports (24) and a single raw material inlet (23), and the fuel addition port (24) is located on one side of the raw material inlet (23).
6. The calcining system according to claim 5, characterized in that: The calcination temperature is between 700° C. and 850° C., the calcination time is 1 hour, and the calcination atmosphere in the decomposition furnace (2) is a CO atmosphere.
7. The calcining system according to claim 6, characterized in that: The activated kaolin was added into the cement calcining assembly at a ratio of 15%.
8. The calcining system according to claim 2, characterized in that: A CO reduction tube is added between the second air inlet (1211) and the third exhaust port (1321) of the third cyclone (132); the decomposition furnace (2) has three fuel addition ports (24) and three raw material inlets (23); the fuel addition ports (24) are arranged opposite to all the raw material inlets (23), and along the wind flow direction, the fuel addition ports (24) are located upstream of the raw material inlets (23).
9. The calcining system according to claim 8, characterized in that: The calcination temperature was 750° C., the calcination time was 1.5 hours, and the calcination atmosphere was a CO atmosphere.
10. The calcining system according to claim 9, characterized in that: The activated kaolin was added into the cement calcining assembly at a ratio of 20%.
11. The calcining system according to claim 2, characterized in that: The air inlet of the decomposition furnace (2) is connected to an extension pipe (21), and one end of the extension pipe (21) away from the air inlet is connected to an inlet pipe (22), and the end of the inlet pipe (22) is trumpet-shaped; Two raw meal inlets (23) are symmetrically arranged on the inlet pipe (22); two fuel addition ports (24) are arranged on the extension pipe (21) at one end close to the inlet pipe (22); the third raw meal inlet (23) and the third fuel addition port (24) are located on the extension pipe (21); and the feeding direction of the third raw meal inlet (23) and the feeding direction of the third fuel addition port (24) are both at right angles to the extension direction of the feed pipe; the feed pipe is arranged between the preheater (1) and the decomposition furnace (2).
12. The calcining system according to claim 11, characterized in that: The calcination temperature is 750° C., the calcination time is 0.5 to 1.5 hours, and the calcination atmosphere is a CO 165 ppm atmosphere.
13. The calcining system according to claim 12, characterized in that: The activated kaolin was added into the cement calcining assembly at a ratio of 5%.
14. A method for calcining cement clinker, characterized in that: include: The cement raw material and kaolin are dried and ground separately to obtain cement raw meal and kaolin raw meal; Adding the cement raw material into a cement calcining assembly for calcining to generate cement clinker; and passing the kaolin raw material into a kaolin calcining assembly for calcination and activation to generate activated kaolin; Adding the activated kaolin to the discharge side of the cement calcining component according to the predetermined proportion of the activated kaolin in the cement clinker; The mixture of cement clinker and activated kaolin is cooled by a grate cooler to obtain cement clinker containing kaolin.
15. The calcination method according to claim 14, characterized in that: The method of grinding kaolin comprises: When kaolin is ground, the fineness of the ground kaolin powder is controlled to be between 75 μm and 85 μm, and the sieve residue is 4% to 6%.
16. The calcining system according to claim 14 or 15, characterized in that: The step of adding the activated kaolin to the discharge side of the cement calcining assembly comprises: The activated kaolin is added into the discharge port of the cement calcining component and the feed port of the active grate cooler.