In-situ measurement method for front edge of carbonized layer of carbonized ablative material

By installing resistive material sheets and insulating films on the carbonized ablation material, the resistance changes of the resistance wire are monitored, and the problem of difficult to measure the front edge position of the carbonized layer is solved, and high-precision in-situ measurement and ablation performance analysis of carbonized ablation materials are realized. Supports lightweight design and online evaluation of thermal protection structures.

CN119043150AActive Publication Date: 2024-11-29HARBIN INST OF TECH

Patent Information

Application Number
CN202411394293.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-11-29
Estimated Expiration
2044-10-08

AI Technical Summary

Technical Problem

During the service of carbonized ablation materials, it is difficult to accurately understand the partitioning conditions inside the material, resulting in the inability to accurately estimate the back temperature of the thermal protection structure, affecting the lightweight design and online evaluation of the thermal protection structure.

Method used

Design an in-situ measurement method for the front edge of the carbonized layer of carbonized ablation material. By etching the thin sheet of resistive material into a circuit, combining with the insulating film to form a flexible resistive sheet, and installing a measuring device on the core material to monitor the resistance wire resistance Changes to reflect the front edge position and backward history of the carbonization layer.

Benefits of technology

It realizes high-precision in-situ measurement of carbonized ablated materials, provides real-time partitioning information of material ablation performance, and supports refined design of thermal protection systems and online temperature forecasting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119043150A_ABST
    Figure CN119043150A_ABST
Patent Text Reader

Abstract

The invention discloses an in-situ measurement method for the front edge of a carbonized layer of a carbonized ablative material. The method comprises the following steps: (1) processing the carbonized ablative material into a core material; (2) etching the resistance material sheet into a designed circuit; (3) an insulating film material is selected, and a blank area is reserved on the side edge; (4) carrying out hot press molding according to an insulating film-circuit-insulating film mode to form a flexible resistor disc; (5) coating back glue on the back of the flexible resistor disc, and connecting a resistance wire lead with a wire; (6) wrapping the flexible resistor disc on the core material to form a measuring device; and (7) installing the measuring device in a test piece, carrying out an ablation test, and reflecting the leading edge position and the retreating process of the carbonization layer by monitoring the change process of the resistance of the resistance wire. According to the invention, in-situ high-precision measurement of the front edge of the carbonized layer of the carbonized ablative material can be provided, internal real-time partition information in the service process of the carbonized ablative material is obtained, and a basis is provided for analyzing the in-situ ablative performance of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an in-situ measurement method for the front edge of a carbonized layer, and in particular to an in-situ measurement method for the front edge of a carbonized layer of a carbonized ablation material. Background Art

[0002] Ablation heat protection has become the main choice for solving the thermal protection problem of hypersonic vehicles due to its strong adaptability, high safety and good reliability. Driven by the goals of lightweight and high efficiency, ablative materials have gradually developed from early high-density carbon phenolic to medium- and low-density AVCOAT, PICA, etc. New lightweight ablative materials represented by PICA have been successfully applied to the thermal protection systems of spacecraft such as Stardust, Mars Science Laboratory and Dragon spacecraft.

[0003] During the service of carbonized ablative materials, as the temperature inside the material gradually increases, one or more components of the original material begin to pyrolyze and produce pyrolysis gas, forming a pyrolysis layer. Subsequently, the pyrolysis gas overflows from the pyrolysis layer, leaving porous carbon residues to form a carbonized layer. As the ablation proceeds, the pyrolysis layer continues to expand into the material, and the interface between the carbonized layer and the pyrolysis layer (i.e., the front of the carbonized layer) then retreats, and the material shows a "carbonized layer-pyrolysis layer-original layer" partition feature. In different service environments, due to different factors such as reentry / entry angles, flight speeds, and atmospheric environments, the thermal loads experienced by the ablative materials vary greatly, and the internal partition characteristics of the materials have obvious differences. The thermal properties of the material are closely related to the partition situation. If the internal partition situation of the material during the ablation process cannot be accurately known, the back temperature of the thermal protection structure cannot be accurately estimated. In order to ensure the safe flight of the aircraft, designers often use a higher safety margin in the design of the thermal protection system, which makes it difficult to achieve a lightweight design of the thermal protection structure.

[0004] Therefore, by obtaining the internal partition characteristics of the material during the ablation process through in-situ measurement, we can better analyze the in-situ ablation performance of the material and the back wall temperature of the material under typical thermal loads, which is of great value for realizing the lightweight design of thermal protection structures and the online evaluation of the status of thermal protection structures. Summary of the invention

[0005] The present invention provides an in-situ measurement method for the front of a carbonized layer of a carbonized ablation material, aiming at the zoning characteristics of "carbonized layer-pyrolysis layer-original layer" formed by pyrolysis of the material during its service.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] An in-situ measurement method of the front edge of a carbonized layer of a carbonized ablation material comprises the following steps:

[0008] Step (1) processing the carbonized ablation material into a cylindrical core material;

[0009] Step (2) using laser etching to etch the resistor material sheet into a designed circuit;

[0010] Step (3) selecting an insulating film material, wherein the insulating material width exceeds the circuit width, leaving a certain degree of blank area on the side;

[0011] Step (4) using a hot pressing method to hot press the two insulating films and the circuit in a "insulating film-circuit-insulating film" manner to form a flexible resistor;

[0012] Step (5) applying adhesive to the back of the flexible resistor and connecting the resistor wire to the conductor;

[0013] Step (6) wrapping the flexible resistor on the core material and bonding it to the blank area of ​​the insulating film through the adhesive to form a final measuring device;

[0014] Step (7) installs the measuring device in the test piece, performs an ablation test, and reflects the front position and retreat process of the carbonized layer by monitoring the change process of the resistance of the resistance wire.

[0015] Compared with the prior art, the present invention has the following advantages:

[0016] The present invention can provide in-situ high-precision measurement of the front edge of the carbonized layer of the carbonized ablation material, obtain real-time internal partitioning information of the carbonized ablation material during service, provide a basis for analyzing the in-situ ablation performance of the material, and further realize online accurate prediction of the back wall temperature and surface heat load of the material, providing support for the refined design of the thermal protection system in subsequent flight missions. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 Schematic diagram of in-situ measurement of the carbonization layer front.

[0018] Figure 2 This is the circuit diagram of the measuring device.

[0019] Figure 3 This is a diagram of the processed core material.

[0020] Figure 4 This is the design diagram of the resistance wire circuit.

[0021] Figure 5 Figure 2 is a diagram of the measuring device.

[0022] Figure 6 This is the measurement result diagram.

[0023] Figure 7 This is the error diagram of the measurement results. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is further described below in conjunction with the accompanying drawings, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.

[0025] Since the carbonized layer is conductive, based on this property, the present invention designs an in-situ measurement method for the front edge of the carbonized layer of the carbonized ablation material. The basic principle of the measurement method is as follows: Figure 1 As shown in the figure, the measuring device consists of three parts: core material, insulating material and resistance wire. Two resistance wires are evenly and equidistantly wound on the insulating material. A core material made of ablative material is embedded inside the insulating material to ensure that the sensor and the ablative material are ablated synchronously. During the ablation process, a carbonized layer is formed inside the material to connect the two resistance wires. As the ablation proceeds, the front edge of the carbonized layer retreats, and the effective circuit of the connected circuit becomes shorter. By monitoring the change process of the resistance of the resistance wire, the front position and retreat process of the carbonized layer are reflected.

[0026] The circuit diagram of the measuring device is as follows Figure 2 As shown, the total resistance of the entire circuit can be expressed as:

[0027] R(t)=R lead +R char +ρgL(t) (1)

[0028] Where R lead Represents the resistance of the voltmeter, wire, etc., R char represents the resistance of the carbonized layer between the two wires, ρ represents the resistance per unit length of the resistance wire, in Ω / mm, L(t) represents the remaining effective circuit length, which is a function of time t, and g represents the proportional coefficient of the total length of the two resistance wires to the initial length of the sensor, where:

[0029] g=nl / L0 (2)

[0030] Where n represents the total number of turns of the resistance wire, l represents the length of each turn of the resistance wire, and L0 represents the initial length of the sensor.

[0031] The voltage measured by the voltmeter is:

[0032] V(t)=IR(t) (3)

[0033] Where I is the constant excitation current. Substituting equation (1) into equation (3) can obtain the position of the front of the carbonization layer:

[0034] L(t)=[V(t) / IR lead -R char ] / (ρg) (4)

[0035] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0036] Step (1) processes the carbonized ablation material into a cylindrical thin-diameter core material to ensure that the measuring device and the ablation material are ablated synchronously.

[0037] Step (2) uses laser etching to etch the resistor material sheet into a designed circuit, wherein: the resistor material is a metal or alloy material, and the resistor material needs to meet the characteristics of high resistivity and high melting point, including but not limited to nickel, nickel-chromium alloy, iron-chromium-aluminum alloy, platinum-tungsten alloy, etc., and the distance between two resistor wires in the designed circuit is not greater than 0.10 mm.

[0038] Step (3) selects an insulating film material, wherein the width of the insulating material exceeds the width of the circuit, leaving a certain degree of blank area on the side, wherein: the insulating material needs to meet the characteristics of high temperature resistance and being thin enough, with an operating temperature range of 300-500°C and a thickness range of 0.01-0.10mm.

[0039] Step (4) adopts a hot pressing method to hot press the two insulating films and the circuit in the manner of "insulating film-circuit-insulating film" to form a flexible resistor sheet, wherein: the overall thickness of the flexible resistor sheet after hot pressing does not exceed 0.30 mm.

[0040] Step (5) Apply adhesive to the back of the flexible resistor and connect the resistor wire to the conductor.

[0041] Step (6) wraps the flexible resistor on the core material and adheres it to the blank area of ​​the insulating film through the adhesive to form a final measuring device.

[0042] Step (7) installs the measuring device in the test piece, performs an ablation test, and reflects the front position and retreat process of the carbonized layer by monitoring the change process of the resistance of the resistance wire.

[0043] Example:

[0044] This embodiment takes the measurement of the carbonization layer front of a light phenolic impregnated carbon ablation material as an example, and specifically includes the following steps:

[0045] (1) Figure 3 As shown, the lightweight phenolic impregnated carbon fiber ablation material is processed into a cylindrical core material with a diameter of 3.00 mm and a length of 30.00 mm.

[0046] (2) The resistor material is iron-chromium-aluminum. The iron-chromium-aluminum resistor sheet with a thickness of 0.10 mm is etched into the following Figure 4 The circuit is shown. After etching, the width of a single resistance wire is 0.01mm, the resistance per unit length of the resistance wire is ρ1.50Ω / mm, and the distance between the two resistance wires is 0.10mm. After measurement, the resistance of the carbonized layer with a length of 0.10mm is Rchar 0.04Ω.

[0047] (3) The insulating film material is polyimide, and the size of the polyimide is as follows: Figure 4 As shown, the effective length is 30.00mm, the width is 17.00mm, the thickness is 0.05mm, and a 3.00mm blank area is left on the side.

[0048] (4) The polyimide film and the resistance wire are hot-pressed into a "polyimide film-resistance wire-polyimide film" pattern by a hot pressing method to form a flexible resistance sheet.

[0049] (5) Apply 3M468 glue on the back of the flexible resistor, and connect the resistor wire lead and the copper wire at the tail of the flexible resistor through 704 silicone rubber. The length of the copper wire is 1500.00mm, and the wire resistance R lead After applying the adhesive, the thickness of the entire flexible resistor is 0.26±0.05mm.

[0050] (6) Wrap the flexible resistor on the core material and connect it to the blank area at 3.00 mm through the adhesive to make a Figure 5 The measuring device shown.

[0051] (7) Install the measuring device in the specimen and use oxyacetylene heating equipment to heat the specimen at 1.0 MW / 2 、1.5MW / 2 and 2.0MW / 2 The ablation test was carried out under heat flow. The measured carbonization layer front retreat process is as follows Figure 5 As shown in the figure, the measurement error is obtained by comparing the front position of the carbonized layer measured by the slice after the test. Figure 6 As shown, it can be seen that the overall accuracy of the carbonization layer front measurement method of the present invention is high, and the maximum error does not exceed 4.32%.

Claims

1. An in-situ measurement method for the front of the carbonized layer of carbonized ablation materials, Features The method comprises the following steps: Step (1) processing the carbonized ablation material into a cylindrical core material; Step (2) using laser etching to etch the resistor material sheet into a designed circuit; Step (3) selecting an insulating film material, wherein the insulating material width exceeds the circuit width, leaving a certain degree of blank area on the side; Step (4) using a hot pressing method to hot press the two insulating films and the circuit in a "insulating film-circuit-insulating film" manner to form a flexible resistor; Step (5) applying adhesive to the back of the flexible resistor and connecting the resistor wire to the conductor; Step (6) wrapping the flexible resistor on the core material and bonding it to the blank area of ​​the insulating film through the adhesive to form a final measuring device; Step (7) installs the measuring device in the test piece, performs an ablation test, and reflects the front position and retreat process of the carbonized layer by monitoring the change process of the resistance of the resistance wire.

2. The in-situ measurement method of the front edge of the carbonized layer of the carbonized ablation material according to claim 1, Features The resistor material is a metal or alloy material.

3. The in-situ measurement method of the front edge of the carbonized layer of the carbonized ablation material according to claim 2, Features The resistance material is one of nickel, nickel-chromium alloy, iron-chromium-aluminum alloy and platinum-tungsten alloy.

4. The in-situ measurement method of the front edge of the carbonized layer of the carbonized ablation material according to claim 1, Features The distance between the two resistance wires in the circuit is no greater than 0.10 mm.

5. The in-situ measurement method of the front edge of the carbonized layer of the carbonized ablation material according to claim 1, Features The use temperature range of the insulating material is 300-500° C., and the thickness range is 0.01-0.10 mm.

6. The in-situ measurement method of the front edge of the carbonized layer of the carbonized ablation material according to claim 1, Features The overall thickness of the flexible resistor sheet does not exceed 0.30 mm.

7. The in-situ measurement method of the front edge of the carbonized layer of the carbonized ablation material according to claim 1, Features The calculation formula of the front position of the carbonization layer is as follows: L(t)=[V(t) / I-R lead -R char ] / (ρg) Where R lead Represents the voltage meter and the wire-related resistance, R char represents the resistance of the carbonized layer between the two wires, ρ represents the resistance per unit length of the resistance wire, L(t) represents the remaining effective circuit length, g represents the proportional coefficient of the total length of the two resistance wires to the initial length of the sensor, and V(t) represents the voltage measured by the voltmeter.

8. The in-situ measurement method of the front edge of the carbonized layer of the carbonized ablation material according to claim 7, Features g = nl / L 0 , where n represents the total number of turns of the resistance wire, l represents the length of each turn of the resistance wire, L 0 Indicates the initial length of the sensor.

9. The in-situ measurement method of the front edge of the carbonized layer of the carbonized ablation material according to claim 7, Features V(t)=IR(t), R(t)=R lead +R char +ρgL(t), I is the constant excitation current.

Citation Information

Patent Citations

  • Damage-sensing composite structures

    CN102753961A

  • Device and method for preparing in-situ formed biochar with high specific surface area

    CN112058222A

  • Damage-sensing composite structures

    US20110089958A1

  • Analysis to enable stress relief in the material under test

    WO2019108694A1

Cited By

  • Carbonized ablative material surface heat flow identification method, device, equipment, medium and product

    CN119741986A

  • Sensor for in-situ measurement of material surface ablation and carbonization layer front edge retreating amount

    CN122361297A