Low-temperature high-rate graphite negative electrode material and preparation method thereof
By adding composite fibers and modified microspheres to the graphite negative electrode material to form a special fiber structure, the problem of degradation of graphite negative electrode material under low temperature conditions is solved, and the low-temperature rate performance and service life of lithium-ion batteries are improved.
Patent Information
- Application Number
- CN202411145513.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
AI Technical Summary
The performance of existing graphite negative electrode materials is degraded under low temperature conditions, resulting in lower ion migration rate of lithium-ion batteries, slow ion diffusion and polarization of electrode materials, resulting in lower battery capacity and reduced charge and discharge efficiency.
Using low-temperature and high-magnification graphite negative electrode material, composite fibers and modified microspheres are prepared by adding composite fibers to the active slurry of graphite negative electrode material, and using specific chemical synthesis steps to form a cellulose carbon structure as the core and cyclodextrin Amorphous carbon is a special fiber structure supported by shell and metal-like organic framework to improve the transportation performance of lithium ions under low temperature conditions.
It significantly improves the rate performance and lithium ion diffusion performance of graphite negative electrode materials under low temperature conditions, extends the service life of the material, avoids the problem of performance degradation during recycling, and improves the low-temperature performance of the battery.
Smart Images

Figure BDA0005002087140000131 
Figure BDA0005002087140000141
Abstract
Description
Technical Field
[0001] The present invention relates to the field of graphite negative electrode materials, and in particular to a low-temperature and high-rate graphite negative electrode material and a preparation method thereof. Background Art
[0002] With the growing demand for the application of lithium-ion batteries in energy storage systems, transportation, portable devices and other fields, higher technical requirements are being placed on their performance. At present, the operation of lithium-ion batteries in extremely cold areas such as the north and high altitude plateaus faces severe challenges. This is mainly because in low temperature environments, the ion migration rate of the battery is reduced, and the electrode materials have problems such as slow ion diffusion and polarization, which leads to a decrease in battery capacity, reduced charging and discharging efficiency, and even inability to work normally.
[0003] Graphite material is inexpensive and has excellent cycle stability. It is the most commonly used negative electrode material for commercial lithium-ion batteries. However, under low temperature conditions, the vibration of the graphite lattice is weakened, which restricts the movement of lithium ions in the graphite lattice, thereby slowing down the ion diffusion rate. Secondly, at low temperatures, the transfer resistance of lithium ions at the interface between the graphite electrode and the electrolyte increases, resulting in reduced battery charge and discharge efficiency. Summary of the invention
[0004] The purpose of the present invention is to provide a low-temperature and high-rate graphite negative electrode material and a preparation method thereof, which solves the problem that the performance of existing graphite negative electrode materials is reduced under low temperature conditions, and at the same time improves the rate performance of graphite negative electrode materials under low temperature conditions.
[0005] The purpose of the present invention can be achieved by the following technical scheme: a low-temperature high-rate graphite negative electrode material, comprising a current collector and an active slurry layer, the low-temperature high-rate graphite negative electrode material is prepared by the following steps: coating the active slurry on the surface of the current collector, and then drying at a temperature of 110°C to obtain a low-temperature high-rate graphite negative electrode material;
[0006] The active slurry is prepared by the following steps: weighing the following materials by weight: 30-35 parts of graphite, 1-2 parts of molybdenum disulfide, 0.8-1.2 parts of carbon black, 2-3 parts of composite fiber, 0.5-1 part of styrene-butadiene rubber latex, 1-2 parts of deionized water and 20-25 parts of N-methylpyrrolidone, mixing the active substance, carbon black, composite fiber, styrene-butadiene rubber latex, deionized water and N-methylpyrrolidone to prepare an active slurry;
[0007] The composite fiber is prepared by the following steps:
[0008] Step A1: β-cyclodextrin and N,N-dimethylformamide are mixed, and under nitrogen protection, the stirring rate is 120-150 rpm, and the temperature is 80°C, iodine and triphenylphosphine are added, and the reaction is carried out for 18-24 hours to obtain intermediate a; intermediate a, sodium azide and N,N-dimethylformamide are mixed, and under nitrogen protection, the stirring rate is 120-150 rpm, and the temperature is 80°C, the reaction is carried out for 12-14 hours to obtain intermediate b;
[0009] The ratio of β-cyclodextrin, iodine and triphenylphosphine is 3-3.2 g: 0.8-1 g: 0.5 g, and the ratio of intermediate a, sodium azide and N,N-dimethylformamide is 3-3.2 g: 3-3.2 g: 60-70 mL;
[0010] During the reaction, under the action of triphenylphosphine, the hydroxymethyl group in β-cyclodextrin undergoes a substitution reaction with iodine element, introducing the iodine element to obtain intermediate a. The iodine element in intermediate a then forms an azide group under the action of sodium azide to obtain intermediate b.
[0011] Step A2: The intermediate b, the modified microspheres and N,N-dimethylformamide were mixed and ultrasonically dispersed for 15 minutes, and copper sulfate and sodium ascorbate were added under nitrogen protection at 50°C, and the reaction was carried out for 24 hours to obtain the precursor 1;
[0012] The dosage ratio of intermediate b, modified microspheres, N,N-dimethylformamide, copper sulfate and sodium ascorbate is 3-3.2g: 0.8-1g: 0.6-0.8g: 0.8-1g;
[0013] During the reaction, under the action of copper sulfate and sodium ascorbate, the azide group in the intermediate b reacts with the alkyne group in the modified microspheres to form a triazole group to obtain the precursor 1;
[0014] Step A3: carboxyl cellulose, mono(6-amino-6-deoxy)-β-cyclodextrin and N,N-dimethylformamide are mixed, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide are added under stirring at a rate of 120-150 rpm and a temperature of 60°C, and the mixture is reacted for 2-3 hours to obtain a precursor 2. Precursor 2, precursor 1, N,N-dimethylformamide and deionized water are mixed and ultrasonically dispersed for 15 minutes, and nickel nitrate hexahydrate is added under stirring at a rate of 150-180 rpm and room temperature, and the mixture is reacted for 1-2 hours. β-cyclodextrin is then added, and the reaction is continued for 3-4 hours. The mixture is heated to 120°C and the reaction is continued for 6-8 hours. The filter cake is filtered to obtain a filter cake, and the filter cake is kept warm for 5 hours under argon protection at a temperature of 700°C to obtain a composite fiber.
[0015] The amount ratio of carboxycellulose, mono(6-amino-6-deoxy)-β-cyclodextrin, 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide is 0.8-1g: 0.8-1g: 0.02g: 0.015g, and the amount ratio of precursor 2, precursor 1, nickel nitrate hexahydrate and β-cyclodextrin is 0.15-0.3g: 0.02-0.025g: 0.2-0.3g: 0.05-0.06g;
[0016] During the reaction, under the action of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide, the carboxyl group in the carboxyl cellulose reacts with the amino group in the mono(6-amino-6-deoxy)-β-cyclodextrin to form an amide bond, thereby obtaining a precursor 2. Since both the precursor 2 and the precursor 1 contain a β-cyclodextrin structure, and the precursor 1 also contains a triazole structure, these structures can be adsorbed with nickel ions and use β-cyclodextrin as a ligand, thereby forming a metal-like organic framework structure on the surface of the precursor 2, which is then kept at 700°C to obtain a composite fiber.
[0017] The modified mesoporous precursor is prepared by the following steps:
[0018] Step B1: Mix silica and anhydrous ethanol and ultrasonically disperse for 30 minutes, stir and add ammonia solution and tetrabutyl titanate at a stirring rate of 120-150 rpm and a temperature of 45°C, react for 24 hours, centrifuge, filter, and obtain core-shell microspheres, mix the core-shell microspheres and deionized water and ultrasonically disperse for 30 minutes, stir and add sodium hydroxide solution at a stirring rate of 80-100 rpm and room temperature, react for 6 hours, centrifuge, filter, dry, and then calcine at a temperature of 800°C to obtain hollow mesoporous microspheres;
[0019] The mass fraction of ammonia solution is 25%, the amount ratio of silicon dioxide, anhydrous ethanol, ammonia solution and tetrabutyl titanate is 0.4-0.5g: 200-240mL: 1.2-1.5mL: 3.8-4mL, the molar concentration of sodium hydroxide solution is 2.5mol / L, and the amount ratio of core-shell microspheres, deionized water and sodium hydroxide solution is 0.4-0.5g: 60-80mL: 4-5mL;
[0020] During the reaction, silicon dioxide is used as a core and tetrabutyl titanate is used as a titanium source. Under the action of an ammonia solution, a titanium oxide shell is formed on the surface of silicon dioxide to obtain core-shell microspheres. Then, under the action of a sodium hydroxide solution, the silicon dioxide core in the core-shell microspheres is corroded, and then calcined to obtain hollow mesoporous microspheres.
[0021] Step B2: Mix sodium tungstate dihydrate and deionized water, stir and add hollow mesoporous microspheres at a stirring rate of 120-150 rpm and room temperature, react for 24 hours, centrifuge, filter, and obtain precursor a; mix precursor a and ethanol solution, stir and add cobalt nitrate hexahydrate at a stirring rate of 120-150 rpm and room temperature, react for 15-20 minutes, centrifuge, filter, and obtain a filter cake; keep the filter cake in vacuum at a temperature of 110° C. for 1.5 hours to obtain composite microspheres;
[0022] The dosage ratio of sodium tungstate dihydrate, deionized water and hollow mesoporous microspheres is 4.5-5g: 20-30mL: 0.2-0.25g, the volume fraction of the ethanol solution is 60%, and the dosage ratio of the precursor a, the ethanol solution and cobalt nitrate hexahydrate is 0.2-0.25g: 0.2-0.3g: 20-30mL;
[0023] During the reaction, due to the hollow mesoporous structure of the hollow mesoporous microspheres, sodium tungstate is immersed in the hollow mesoporous microspheres. At the same time, since sodium tungstate is insoluble in ethanol, after cobalt nitrate enters the hollow mesoporous microspheres, sodium tungstate is converted into tungstic acid, and tungstic acid is dehydrated to form tungsten trioxide, thereby generating tungsten trioxide inside the hollow mesoporous microspheres to obtain composite microspheres.
[0024] Step B3: 3-isocyanatepropyltriethoxysilane, m-aminophenylacetylene and tetrahydrofuran were mixed, and the mixture was reacted for 2-3 hours at room temperature at a stirring rate of 120-150 rpm to obtain alkynylsilane. The alkynylsilane and ethanol solution were adjusted to pH 9, and the composite microspheres were added under stirring at a stirring rate of 120-150 rpm and a temperature of 80° C., and the mixture was reacted for 1.5 hours to obtain modified microspheres.
[0025] The dosage ratio of 3-isocyanatepropyltriethoxysilane, m-aminophenylacetylene and tetrahydrofuran is 4.5-4.8 g: 2.3-2.4 g: 30-35 mL, the volume fraction of the ethanol solution is 50%, and the dosage ratio of alkynylsilane, ethanol solution and composite microspheres is 0.24-0.25 g: 10-15 mL: 0.25-0.3 g;
[0026] During the reaction, the isocyanate group in 3-isocyanatepropyltriethoxysilane reacts with the amino group in m-aminophenylacetylene to form a urea group, thereby obtaining an alkynyl silane. The silyl ethoxy group in the alkynyl silane is hydrolyzed to form an active hydroxyl group, which reacts with the hydroxyl group on the surface of the composite microspheres to introduce an alkynyl group, thereby obtaining a modified microsphere.
[0027] Beneficial effects of the invention: The field of graphite negative electrode materials of the invention specifically relates to a low-temperature and high-rate graphite negative electrode material and a preparation method thereof. By adding composite fibers to the active slurry used in the field of graphite negative electrode materials, the problem of reduced performance of existing graphite negative electrode materials under low temperature conditions is solved, and the rate performance of graphite negative electrode materials under low temperature conditions is improved. The composite fibers are prepared by heat preservation, and due to the presence of precursor 1, precursor 2 and β-cyclodextrin, and precursor 2 is based on carboxyl cellulose, so that after heat preservation, a special fiber structure with a cellulose carbon structure as a core and amorphous carbon formed by cyclodextrin as a shell is formed, and a metal-like organic skeleton is used as a support between the shell and the core, and modified microspheres are dotted. Since the special fiber structure formed is a large amount of poly The porous amorphous carbon is used as the matrix, and a large amount of nitrogen elements are introduced as defect sites. The metal organic framework not only provides more active sites, thereby improving the performance of the negative electrode material, but also its supporting effect allows the formation of an interlayer structure in the composite fiber, thereby improving the rapid transport of lithium ions at the electrode-electrolyte interface under low temperature conditions, thereby greatly improving the low-temperature performance of the material, and because modified microspheres are dotted in the amorphous carbon, and due to the hollow mesoporous titanium oxide and tungsten trioxide core structure of the modified microspheres, the modified microspheres have higher lithium ion diffusion performance and lithium ion storage performance, and the structure of the modified microspheres also avoids the problem of performance degradation during cyclic use, thereby allowing the graphite negative electrode material to have a longer service life and greatly improving the rate performance of the negative electrode material. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Embodiment 1 A low-temperature high-rate graphite negative electrode material comprises a current collector and an active slurry layer. The low-temperature high-rate graphite negative electrode material is prepared by the following steps: coating the active slurry on the surface of the current collector, and then drying at a temperature of 110° C. to obtain a low-temperature high-rate graphite negative electrode material;
[0030] The active slurry is prepared by the following steps: weigh the following materials by weight: 30 parts of commercial Guohao graphite, 1 part of commercial Wandao molybdenum disulfide, 0.8 parts of commercial N300 carbon black, 2 parts of composite fiber, 0.5 parts of commercial SN307R styrene-butadiene rubber latex, 1 part of deionized water and 20 parts of N-methylpyrrolidone, mix the active substance, carbon black, composite fiber, styrene-butadiene rubber latex, deionized water and N-methylpyrrolidone to prepare an active slurry;
[0031] The composite fiber is prepared by the following steps:
[0032] Step A1: β-cyclodextrin and N,N-dimethylformamide were mixed, and iodine and triphenylphosphine were added under nitrogen protection, stirring at a rate of 120 rpm and a temperature of 80°C, and the mixture was reacted for 18 hours to obtain intermediate a; intermediate a, sodium azide and N,N-dimethylformamide were mixed, and the mixture was stirred at a rate of 120 rpm and a temperature of 80°C under nitrogen protection, and the mixture was reacted for 12 hours to obtain intermediate b;
[0033] The ratio of β-cyclodextrin, iodine and triphenylphosphine is 3g:0.8g:0.5g, and the ratio of intermediate a, sodium azide and N,N-dimethylformamide is 3g:3g:60mL;
[0034] Step A2: The intermediate b, the modified microspheres and N,N-dimethylformamide were mixed and ultrasonically dispersed for 15 minutes, and copper sulfate and sodium ascorbate were added under nitrogen protection at 50°C, and the reaction was carried out for 24 hours to obtain the precursor 1;
[0035] The amount ratio of intermediate b, modified microspheres, N,N-dimethylformamide, copper sulfate and sodium ascorbate is 3g:0.8g:0.6g:0.8g;
[0036] Step A3: commercially available Lamborghini carboxyl cellulose, mono(6-amino-6-deoxy)-β-cyclodextrin and N,N-dimethylformamide were mixed, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide were added under stirring at a rate of 120 rpm and a temperature of 60°C, and the mixture was reacted for 2 hours to obtain a precursor 2. Precursor 2, precursor 1, N,N-dimethylformamide and deionized water were mixed and ultrasonically dispersed for 15 minutes, and nickel nitrate hexahydrate was added under stirring at a rate of 150 rpm and room temperature, and the mixture was reacted for 1 hour. β-cyclodextrin was then added, and the reaction was continued for 3 hours. The mixture was heated to 120°C and the reaction was continued for 6 hours. The mixture was filtered to obtain a filter cake, and the filter cake was kept warm for 5 hours under argon protection at a temperature of 700°C to obtain a composite fiber.
[0037] The amount ratio of carboxycellulose, mono(6-amino-6-deoxy)-β-cyclodextrin, 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide is 0.8g:0.8g:0.02g:0.015g, and the amount ratio of precursor 2, precursor 1, nickel nitrate hexahydrate and β-cyclodextrin is 0.15g:0.02g:0.2g:0.06g;
[0038] The modified mesoporous precursor is prepared by the following steps:
[0039] Step B1: Mix commercially available 100 nm silica and anhydrous ethanol and ultrasonically disperse for 30 minutes, stir and add ammonia solution and tetrabutyl titanate at a stirring rate of 120 rpm and a temperature of 45°C, react for 24 hours, centrifuge, filter, and obtain core-shell microspheres, mix the core-shell microspheres and deionized water and ultrasonically disperse for 30 minutes, stir and add sodium hydroxide solution at a stirring rate of 80 rpm and room temperature, react for 6 hours, centrifuge, filter, dry, and then calcine at a temperature of 800°C to obtain hollow mesoporous microspheres;
[0040] The mass fraction of ammonia solution is 25%, the amount ratio of silicon dioxide, anhydrous ethanol, ammonia solution and tetrabutyl titanate is 0.4g:2000mL:1.2mL:3.8mL, the molar concentration of sodium hydroxide solution is 2.5mol / L, and the amount ratio of core-shell microspheres, deionized water and sodium hydroxide solution is 0.4g:60mL:4mL;
[0041] Step B2: Mix sodium tungstate dihydrate and deionized water, stir and add hollow mesoporous microspheres at a stirring rate of 120 rpm and room temperature, react for 24 hours, centrifuge, filter, and obtain precursor a; mix precursor a and ethanol solution, stir and add cobalt nitrate hexahydrate at a stirring rate of 120 rpm and room temperature, react for 15 minutes, centrifuge, filter, and obtain a filter cake; keep the filter cake in vacuum at a temperature of 110° C. for 1.5 hours to obtain composite microspheres;
[0042] The dosage ratio of sodium tungstate dihydrate, deionized water and hollow mesoporous microspheres is 4.5g:20mL:0.2g, the volume fraction of ethanol solution is 60%, and the dosage ratio of precursor a, ethanol solution and cobalt nitrate hexahydrate is 0.2g:0.2g:20mL;
[0043] Step B3: 3-isocyanatepropyltriethoxysilane, m-aminophenylacetylene and tetrahydrofuran were mixed, and the mixture was reacted for 2 h at a stirring rate of 120 rpm and room temperature to obtain alkynylsilane. The alkynylsilane and ethanol solution were adjusted to pH 9, and the composite microspheres were added under stirring at a stirring rate of 120 rpm and a temperature of 80° C., and the mixture was reacted for 1.5 h to obtain modified microspheres.
[0044] The amount ratio of 3-isocyanatepropyltriethoxysilane, m-aminophenylacetylene and tetrahydrofuran is 4.5g:2.3g:30mL, the volume fraction of the ethanol solution is 50%, and the amount ratio of alkynylsilane, ethanol solution and composite microspheres is 0.24g:10mL:0.25g.
[0045] Embodiment 2 A low-temperature high-rate graphite negative electrode material comprises a current collector and an active slurry layer. The low-temperature high-rate graphite negative electrode material is prepared by the following steps: coating the active slurry on the surface of the current collector, and then drying at a temperature of 110° C. to obtain a low-temperature high-rate graphite negative electrode material;
[0046] The active slurry is prepared by the following steps: weigh the following materials by weight: 30 parts of commercial Guohao graphite, 1 part of commercial Wandao molybdenum disulfide, 0.8 parts of commercial N300 carbon black, 3 parts of composite fiber, 0.5 parts of commercial SN307R styrene-butadiene rubber latex, 1 part of deionized water and 25 parts of N-methylpyrrolidone, and mix the active substance, carbon black, composite fiber, styrene-butadiene rubber latex, deionized water and N-methylpyrrolidone to prepare an active slurry;
[0047] The composite fiber is prepared by the following steps:
[0048] Step A1: β-cyclodextrin and N,N-dimethylformamide were mixed, and iodine and triphenylphosphine were added under nitrogen protection, stirring at a rate of 150 rpm and a temperature of 80°C, and the mixture was reacted for 24 hours to obtain intermediate a; intermediate a, sodium azide and N,N-dimethylformamide were mixed, and the mixture was stirred at a rate of 120 rpm and a temperature of 80°C under nitrogen protection, and the mixture was reacted for 14 hours to obtain intermediate b;
[0049] The ratio of β-cyclodextrin, iodine and triphenylphosphine is 3.2 g: 0.8 g: 0.5 g, and the ratio of intermediate a, sodium azide and N,N-dimethylformamide is 3.2 g: 3.2 g: 60 mL;
[0050] Step A2: The intermediate b, the modified microspheres and N,N-dimethylformamide were mixed and ultrasonically dispersed for 15 minutes, and copper sulfate and sodium ascorbate were added under nitrogen protection at 50°C, and the reaction was carried out for 24 hours to obtain the precursor 1;
[0051] The amount ratio of intermediate b, modified microspheres, N,N-dimethylformamide, copper sulfate and sodium ascorbate is 3.2g:0.8g:0.8g:0.8g;
[0052] Step A3: commercially available Lamborghini carboxyl cellulose, mono(6-amino-6-deoxy)-β-cyclodextrin and N,N-dimethylformamide were mixed, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide were added under stirring at a rate of 120 rpm and a temperature of 60°C, and the mixture was reacted for 3 hours to obtain a precursor 2. Precursor 2, precursor 1, N,N-dimethylformamide and deionized water were mixed and ultrasonically dispersed for 15 minutes, and nickel nitrate hexahydrate was added under stirring at a rate of 150 rpm and room temperature, and the mixture was reacted for 2 hours. β-cyclodextrin was then added, and the reaction was continued for 3 hours. The mixture was heated to 120°C and the reaction was continued for 8 hours. The mixture was filtered to obtain a filter cake, and the filter cake was kept warm for 5 hours under argon protection at a temperature of 700°C to obtain a composite fiber.
[0053] The amount ratio of carboxycellulose, mono(6-amino-6-deoxy)-β-cyclodextrin, 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide is 0.8g:1g:0.02g:0.015g, and the amount ratio of precursor 2, precursor 1, nickel nitrate hexahydrate and β-cyclodextrin is 0.15g:0.02g:0.2g:0.06g;
[0054] The modified mesoporous precursor is prepared by the following steps:
[0055] Step B1: Mix commercially available 100 nm silica and anhydrous ethanol and ultrasonically disperse for 30 minutes, stir and add ammonia solution and tetrabutyl titanate at a stirring rate of 150 rpm and a temperature of 45°C, react for 24 hours, centrifuge, filter, and obtain core-shell microspheres, mix the core-shell microspheres and deionized water and ultrasonically disperse for 30 minutes, stir and add sodium hydroxide solution at a stirring rate of 80 rpm and room temperature, react for 6 hours, centrifuge, filter, dry, and then calcine at a temperature of 800°C to obtain hollow mesoporous microspheres;
[0056] The mass fraction of ammonia solution is 25%, the amount ratio of silicon dioxide, anhydrous ethanol, ammonia solution and tetrabutyl titanate is 0.5g:200mL:1.5mL:3.8mL, the molar concentration of sodium hydroxide solution is 2.5mol / L, and the amount ratio of core-shell microspheres, deionized water and sodium hydroxide solution is 0.5g:80mL:4mL;
[0057] Step B2: Mix sodium tungstate dihydrate and deionized water, stir and add hollow mesoporous microspheres at a stirring rate of 120 rpm and room temperature, react for 24 hours, centrifuge, filter, and obtain precursor a; mix precursor a and ethanol solution, stir and add cobalt nitrate hexahydrate at a stirring rate of 150 rpm and room temperature, react for 15 minutes, centrifuge, filter, and obtain a filter cake; keep the filter cake in vacuum at a temperature of 110° C. for 1.5 hours to obtain composite microspheres;
[0058] The dosage ratio of sodium tungstate dihydrate, deionized water and hollow mesoporous microspheres is 5g:20mL:0.25g, the volume fraction of ethanol solution is 60%, and the dosage ratio of precursor a, ethanol solution and cobalt nitrate hexahydrate is 0.25g:0.3g:20mL;
[0059] Step B3: 3-isocyanatepropyltriethoxysilane, m-aminophenylacetylene and tetrahydrofuran were mixed, and the mixture was reacted for 3 hours at a stirring rate of 120 rpm and room temperature to obtain alkynylsilane. The alkynylsilane and ethanol solution were adjusted to pH 9, and the composite microspheres were added under stirring at a stirring rate of 120 rpm and a temperature of 80° C., and the mixture was reacted for 1.5 hours to obtain modified microspheres.
[0060] The amount ratio of 3-isocyanatepropyltriethoxysilane, m-aminophenylacetylene and tetrahydrofuran is 4.5g:2.4g:30mL, the volume fraction of the ethanol solution is 50%, and the amount ratio of alkynylsilane, ethanol solution and composite microspheres is 0.25g:15mL:0.25g.
[0061] Embodiment 3 A low-temperature high-rate graphite negative electrode material comprises a current collector and an active slurry layer. The low-temperature high-rate graphite negative electrode material is prepared by the following steps: coating the active slurry on the surface of the current collector, and then drying at a temperature of 110° C. to obtain a low-temperature high-rate graphite negative electrode material;
[0062] The active slurry is prepared by the following steps: weigh the following materials by weight: 35 parts of commercial Guohao graphite, 2 parts of commercial Wandao molybdenum disulfide, 1.2 parts of commercial N300 carbon black, 3 parts of composite fiber, 1 part of commercial SN307R styrene-butadiene rubber latex, 1-2 parts of deionized water and 25 parts of N-methylpyrrolidone, and mix the active substance, carbon black, composite fiber, styrene-butadiene rubber latex, deionized water and N-methylpyrrolidone to prepare an active slurry;
[0063] The composite fiber is prepared by the following steps:
[0064] Step A1: β-cyclodextrin and N,N-dimethylformamide were mixed, and iodine and triphenylphosphine were added under nitrogen protection, stirring at a rate of 150 rpm and a temperature of 80°C, and the mixture was reacted for 24 hours to obtain intermediate a; intermediate a, sodium azide and N,N-dimethylformamide were mixed, and the mixture was stirred at a rate of 150 rpm and a temperature of 80°C under nitrogen protection, and the mixture was reacted for 14 hours to obtain intermediate b;
[0065] The ratio of β-cyclodextrin, iodine and triphenylphosphine is 3.2 g: 1 g: 0.5 g, and the ratio of intermediate a, sodium azide and N,N-dimethylformamide is 3.2 g: 3.2 g: 70 mL;
[0066] Step A2: The intermediate b, the modified microspheres and N,N-dimethylformamide were mixed and ultrasonically dispersed for 15 minutes, and copper sulfate and sodium ascorbate were added under nitrogen protection at 50°C, and the reaction was carried out for 24 hours to obtain the precursor 1;
[0067] The dosage ratio of intermediate b, modified microspheres, N,N-dimethylformamide, copper sulfate and sodium ascorbate is 3.2g:1g:0.8g:1g;
[0068] Step A3: commercially available Lamborghini carboxyl cellulose, mono(6-amino-6-deoxy)-β-cyclodextrin and N,N-dimethylformamide were mixed, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide were added under stirring at a rate of 150 rpm and a temperature of 60°C, and the mixture was reacted for 3 hours to obtain a precursor 2. Precursor 2, precursor 1, N,N-dimethylformamide and deionized water were mixed and ultrasonically dispersed for 15 minutes, and nickel nitrate hexahydrate was added under stirring at a rate of 180 rpm and room temperature, and the mixture was reacted for 2 hours. β-cyclodextrin was then added, and the reaction was continued for 4 hours. The mixture was heated to 120°C and the reaction was continued for 8 hours. The mixture was filtered to obtain a filter cake, and the filter cake was kept warm for 5 hours under argon protection at a temperature of 700°C to obtain a composite fiber.
[0069] The amount ratio of carboxycellulose, mono(6-amino-6-deoxy)-β-cyclodextrin, 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide is 1g:1g:0.02g:0.015g, and the amount ratio of precursor 2, precursor 1, nickel nitrate hexahydrate and β-cyclodextrin is 0.3g:0.025g:0.3g:0.06g;
[0070] The modified mesoporous precursor is prepared by the following steps:
[0071] Step B1: Mix commercially available 100 nm silica and anhydrous ethanol and ultrasonically disperse for 30 minutes, stir and add ammonia solution and tetrabutyl titanate at a stirring rate of 150 rpm and a temperature of 45°C, react for 24 hours, centrifuge, filter, and obtain core-shell microspheres, mix the core-shell microspheres and deionized water and ultrasonically disperse for 30 minutes, stir and add sodium hydroxide solution at a stirring rate of 100 rpm and room temperature, react for 6 hours, centrifuge, filter, dry, and then calcine at a temperature of 800°C to obtain hollow mesoporous microspheres;
[0072] The mass fraction of ammonia solution is 25%, the amount ratio of silicon dioxide, anhydrous ethanol, ammonia solution and tetrabutyl titanate is 0.5g:240mL:1.5mL:4mL, the molar concentration of sodium hydroxide solution is 2.5mol / L, and the amount ratio of core-shell microspheres, deionized water and sodium hydroxide solution is 0.5g:80mL:5mL;
[0073] Step B2: Mix sodium tungstate dihydrate and deionized water, stir and add hollow mesoporous microspheres at a stirring rate of 150 rpm and room temperature, react for 24 hours, centrifuge, filter, and obtain precursor a; mix precursor a and ethanol solution, stir and add cobalt nitrate hexahydrate at a stirring rate of 150 rpm and room temperature, react for 20 minutes, centrifuge, filter, and obtain a filter cake; keep the filter cake in vacuum at a temperature of 110° C. for 1.5 hours to obtain composite microspheres;
[0074] The dosage ratio of sodium tungstate dihydrate, deionized water and hollow mesoporous microspheres is 5g:30mL:0.25g, the volume fraction of ethanol solution is 60%, and the dosage ratio of precursor a, ethanol solution and cobalt nitrate hexahydrate is 0.25g:0.3g:30mL;
[0075] Step B3: 3-isocyanatepropyltriethoxysilane, m-aminophenylacetylene and tetrahydrofuran were mixed, and the mixture was reacted for 3 hours at a stirring rate of 150 rpm and room temperature to obtain alkynylsilane. The alkynylsilane and ethanol solution were adjusted to pH 9, and the composite microspheres were added under stirring at a stirring rate of 150 rpm and a temperature of 80° C., and the mixture was reacted for 1.5 hours to obtain modified microspheres.
[0076] The amount ratio of 3-isocyanatepropyltriethoxysilane, m-aminophenylacetylene and tetrahydrofuran is 4.8g:2.4g:35mL, the volume fraction of the ethanol solution is 50%, and the amount ratio of alkynylsilane, ethanol solution and composite microspheres is 0.25g:15mL:0.3g.
[0077] Comparative Example 1 Compared with Example 3, this comparative example removes β-cyclodextrin in step A3 of the composite fiber preparation process of Example 3, and the other steps are the same.
[0078] Comparative Example 2 Compared with Example 3, this comparative example is different in that the precursor 1 in the composite fiber preparation process of Example 3 is replaced by the modified microspheres of Example 3, and the other steps are the same.
[0079] Comparative Example 3 Compared with Example 3, this comparative example replaces the composite microspheres in the preparation process of the modified microspheres in Example 3 with the hollow mesoporous microspheres in Example 3, and the other steps are the same.
[0080] Comparative Example 4 Compared with Example 3, this comparative example replaces the composite fiber in the active slurry preparation process of Example 3 with the commercially available Moyu fiber conductive additive, and the other steps are the same.
[0081] Take the low-temperature and high-rate graphite negative electrode materials prepared in Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4, and use the low-temperature and high-rate graphite negative electrode materials as the negative electrode materials of CR2032 button batteries to prepare CR2032 button batteries, and use a battery tester to test the initial specific capacity at 0.2C and 2C, 25°C and the retention rate after 100 cycles. The initial specific capacity at 2C, -10°C and 0°C is tested, and the test results are as shown in Table 1:
[0082] Table 1 Test results
[0083]
[0084]
[0085] It can be seen from the test results in the table shown that Example 1, Example 2 and Example 3 are compared with Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4. Comparative Example 1 removes β-cyclodextrin in step A3 of the composite fiber preparation process of Example 3, resulting in the inability to form a metal-like organic structure, thereby affecting its low temperature performance, rate performance and cycle performance. Comparative Example 2 replaces the precursor 1 in the composite fiber preparation process of Example 3 with the modified microspheres of Example 3. Due to the lack of azide groups, the doping active sites are reduced, thereby affecting its lithium storage performance, thereby causing its performance to decrease. Comparative Example 3 replaces the composite microspheres in the preparation process of the modified microspheres of Example 3 with the hollow mesoporous microspheres of Example 3. Due to the lack of tungsten trioxide cores, its low temperature performance is reduced. Comparative Example 4 replaces the composite fiber in the active slurry preparation process of Example 3 with the commercially available Moyu fiber conductive additive, indicating that the composite fiber has excellent performance compared with common fiber conductive additives on the market.
[0086] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0087] The above contents are merely examples and explanations of the concept of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a low-temperature and high-rate graphite negative electrode material, characterized in that: The low-temperature high-rate graphite negative electrode material comprises a current collector and an active slurry layer, and is prepared by the following steps: coating the active slurry on the surface of the current collector, and then drying the slurry at a temperature of 110°C to obtain a low-temperature high-rate graphite negative electrode material; The active slurry is prepared by the following steps: weighing the following materials in parts by weight: 30-35 parts of graphite, 1-2 parts of molybdenum disulfide, 0.8-1.2 parts of carbon black, 2-3 parts of composite fiber, 0.5-1 part of styrene-butadiene rubber latex, 1-2 parts of deionized water and 20-25 parts of N-methylpyrrolidone, mixing the active substance, carbon black, composite fiber, styrene-butadiene rubber latex, deionized water and N-methylpyrrolidone to prepare the active slurry.
2. The method for preparing a low-temperature and high-rate graphite negative electrode material according to claim 1, characterized in that: The composite fiber is prepared by the following steps: Step A1: β-cyclodextrin and N,N-dimethylformamide are mixed, and under nitrogen protection, the stirring rate is 120-150 rpm, and the temperature is 80°C, iodine and triphenylphosphine are added, and the reaction is carried out for 18-24 hours to obtain intermediate a; intermediate a, sodium azide and N,N-dimethylformamide are mixed, and under nitrogen protection, the stirring rate is 120-150 rpm, and the temperature is 80°C, the reaction is carried out for 12-14 hours to obtain intermediate b; Step A2: The intermediate b, the modified microspheres and N,N-dimethylformamide were mixed and ultrasonically dispersed for 15 minutes, and copper sulfate and sodium ascorbate were added under nitrogen protection at 50°C, and the reaction was carried out for 24 hours to obtain the precursor 1; Step A3: Carboxyl cellulose, mono(6-amino-6-deoxy)-β-cyclodextrin and N,N-dimethylformamide are mixed, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide are added under stirring at a rate of 120-150 rpm and a temperature of 60°C, and the reaction is carried out for 2-3 hours to obtain a precursor 2. Precursor 2, precursor 1, N,N-dimethylformamide and deionized water are mixed and ultrasonically dispersed for 15 minutes, and nickel nitrate hexahydrate is added under stirring at a rate of 150-180 rpm and room temperature, and the reaction is carried out for 1-2 hours. β-cyclodextrin is then added, and the reaction is continued for 3-4 hours. The temperature is then raised to 120°C, and the reaction is continued for 6-8 hours. The filter cake is filtered to obtain a filter cake, and the filter cake is kept warm at 700°C under argon protection for 5 hours to obtain a composite fiber.
3. The method for preparing a low-temperature and high-rate graphite negative electrode material according to claim 2, characterized in that: In step A1: the usage ratio of β-cyclodextrin, elemental iodine and triphenylphosphine is 3-3.2 g: 0.8-1 g: 0.5 g, and the usage ratio of intermediate a, sodium azide and N,N-dimethylformamide is 3-3.2 g: 3-3.2 g: 60-70 mL.
4. The method for preparing a low-temperature and high-rate graphite negative electrode material according to claim 2, characterized in that: In step A2: the usage ratio of intermediate b, modified microspheres, N,N-dimethylformamide, copper sulfate and sodium ascorbate is 3-3.2 g: 0.8-1 g: 0.6-0.8 g: 0.8-1 g.
5. The method for preparing a low-temperature and high-rate graphite negative electrode material according to claim 2, characterized in that: In step A3: the amount ratio of carboxycellulose, mono (6-amino-6-deoxy) -β-cyclodextrin, 1-ethyl- (3-dimethylaminopropyl) carbodiimide and N-hydroxysuccinimide is 0.8-1g: 0.8-1g: 0.02g: 0.015g, and the amount ratio of precursor 2, precursor 1, nickel nitrate hexahydrate and β-cyclodextrin is 0.15-0.3g: 0.02-0.025g: 0.2-0.3g: 0.05-0.06g.
6. The method for preparing a low-temperature and high-rate graphite negative electrode material according to claim 2, characterized in that: The modified mesoporous precursor is prepared by the following steps: Step B1: Mix silica and anhydrous ethanol and ultrasonically disperse for 30 minutes, stir and add ammonia solution and tetrabutyl titanate at a stirring rate of 120-150 rpm and a temperature of 45°C, react for 24 hours, centrifuge, filter, and obtain core-shell microspheres, mix the core-shell microspheres and deionized water and ultrasonically disperse for 30 minutes, stir and add sodium hydroxide solution at a stirring rate of 80-100 rpm and room temperature, react for 6 hours, centrifuge, filter, dry, and then calcine at a temperature of 800°C to obtain hollow mesoporous microspheres; Step B2: Mix sodium tungstate dihydrate and deionized water, stir and add hollow mesoporous microspheres at a stirring rate of 120-150 rpm and room temperature, react for 24 hours, centrifuge, filter, and obtain precursor a; mix precursor a and ethanol solution, stir and add cobalt nitrate hexahydrate at a stirring rate of 120-150 rpm and room temperature, react for 15-20 minutes, centrifuge, filter, and obtain a filter cake; keep the filter cake in vacuum at a temperature of 110° C. for 1.5 hours to obtain composite microspheres; Step B3: Mix 3-isocyanatepropyltriethoxysilane, m-aminophenylacetylene and tetrahydrofuran, and react for 2-3 hours at a stirring rate of 120-150 rpm and room temperature to obtain alkynyl silane. Adjust the pH value of alkynyl silane and ethanol solution to 9, stir at a stirring rate of 120-150 rpm and a temperature of 80°C, add composite microspheres, and react for 1.5 hours to obtain modified microspheres.
7. The method for preparing a low-temperature and high-rate graphite negative electrode material according to claim 6, characterized in that: In step B1: the mass fraction of the ammonia solution is 25%, the amount ratio of silicon dioxide, anhydrous ethanol, ammonia solution and tetrabutyl titanate is 0.4-0.5g: 200-240mL: 1.2-1.5mL: 3.8-4mL, the molar concentration of the sodium hydroxide solution is 2.5mol / L, and the amount ratio of the core-shell microspheres, deionized water and sodium hydroxide solution is 0.4-0.5g: 60-80mL: 4-5mL.
8. The method for preparing a low-temperature and high-rate graphite negative electrode material according to claim 6, characterized in that: In step B2: the dosage ratio of sodium tungstate dihydrate, deionized water and hollow mesoporous microspheres is 4.5-5g:20-30mL:0.2-0.25g, the volume fraction of the ethanol solution is 60%, and the dosage ratio of the precursor a, the ethanol solution and cobalt nitrate hexahydrate is 0.2-0.25g:0.2-0.3g:20-30mL.
9. The method for preparing a low-temperature and high-rate graphite negative electrode material according to claim 6, characterized in that: In step B3: the amount ratio of 3-isocyanatepropyltriethoxysilane, m-aminophenylacetylene and tetrahydrofuran is 4.5-4.8g:2.3-2.4g:30-35mL, the volume fraction of the ethanol solution is 50%, and the amount ratio of alkynylsilane, ethanol solution and composite microspheres is 0.24-0.25g:10-15mL:0.25-0.3g.
10. A low-temperature and high-rate graphite negative electrode material, characterized in that: Prepared according to any one of claims 1 to 9.
Citation Information
Cited By
Low-temperature high-rate graphite negative electrode material and preparation method thereof
CN120834153A