Lithium-doped amorphous carbon coated graphite composite material as well as preparation method and application thereof

Through the preparation of lithium-doped amorphous carbon-coated graphite composite material, the problems of expansion and low conductivity of the negative electrode material of lithium-ion battery during circulation are solved, the cycle life and rate performance of the battery are improved, and the efficient preparation of the material is achieved and performance improvement.

CN119050316APending Publication Date: 2024-11-29SHENZHEN GOLD MEDAL NEW ENERGY TECH CO LTD +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411232446.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing lithium-ion battery anode materials expand largely during the cycle process and the electron and lithium ions transmission rates are low, resulting in a degradation in rate performance. The material preparation environment is high and the consistency is difficult to control, making it difficult to achieve high life and low cost industrialization.

Method used

The preparation method of lithium-doped amorphous carbon-coated graphite composite material is adopted. Graphite is formed by mixing asphalt coke, nitrogen-containing polymer, lithium fluoride and oxidizing agent evenly, and spray-drying and sintering of liquid coating agent. The core of the material is doped with amorphous carbon shell structure to reduce material defects and improve electrical conductivity.

Benefits of technology

It improves the cycle life and maximum performance of lithium-ion batteries, reduces expansion and irreversible capacity, enhances the first-time efficiency and layer spacing, and achieves efficient preparation and performance improvement of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050316A_ABST
    Figure CN119050316A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium-doped amorphous carbon coated graphite composite material and a preparation method and application thereof, the preparation method comprises the following steps: uniformly mixing pitch coke, a nitrogen-containing polymer, lithium fluoride, an oxidizing agent and pitch to obtain a mixed raw material, and graphitizing the mixed raw material to obtain a graphite precursor material; the preparation method comprises the following steps: adding a graphite precursor and a lithium supplement agent into an organic solution of a liquid coating agent, uniformly dispersing, spray-drying, and sintering a dried product to obtain the required lithium-doped amorphous carbon coated graphite composite material. According to the preparation method of the lithium-doped amorphous carbon coated graphite composite material, a chemical bond connected carbon structure is formed by utilizing the cohesiveness of pitch coke and the action of chemical groups on the surface of an oxidizing agent, lithium fluoride is doped to reduce material defects, the oxidizing agent is added for pore forming to improve isotropy of the material and reduce expansion, and the lithium-doped amorphous carbon coated graphite composite material is prepared. The lithium supplement agent is coated on the shell to supplement loss of lithium ions in the charging and discharging process, the cycle life is prolonged, and the rate and the cycle performance are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of secondary batteries, and in particular to a preparation method of a lithium-doped amorphous carbon-coated graphite composite material, a lithium-doped amorphous carbon-coated graphite composite material and applications thereof. Background Art

[0002] As a green and environmentally friendly new energy, lithium-ion batteries have the advantages of good reliability, high safety, small size and light weight. They have been widely used in digital products, electric vehicles, military products and other fields. With the vigorous development of the new energy industry, the development of lithium-ion batteries is in full swing, but the requirements for the service life, safety and low cost of lithium-ion batteries are also getting higher and higher. At present, lithium-ion batteries are also developing in the direction of long life, high safety, high rate and low cost.

[0003] The negative electrode material is one of the key factors that restrict the energy density and rate charge and discharge performance of lithium-ion batteries. The negative electrode materials used in energy storage batteries are mainly selected from raw materials with high isotropy, artificial graphite materials with low specific surface area and low expansion. However, as the new SEI film expands during the cycle, it consumes lithium ions, causing the cycle performance to decrease during the charge and discharge process.

[0004] Compared with natural graphite negative electrode materials, artificial graphite negative electrode materials have better performance, and artificial graphite negative electrode materials have become the mainstream of power battery negative electrode materials. At present, the raw materials used to prepare artificial graphite lithium-ion battery negative electrode materials are mainly needle coke, petroleum coke, and pitch coke. Pitch coke is the solid residue obtained after high-temperature dry distillation or delayed coking of coal tar. Coal tar has the characteristics of abundant resources, low price, high carbon content, good fluidity, and easy graphitization. It is one of the most important and basic matrix precursors in the production of various carbon materials. The structure and composition of coal tar are very complex. It is composed of a large number of highly condensed carbon rings and heterocyclic compounds. It has the same composition and structure as coal, but there are differences in the degree of ring structure and molecular composition, and its molecular weight distribution range is wide. With the increasing diversity of special requirements in the terminal application segments of lithium-ion batteries, negative electrode materials prepared based on coal tar are gradually gaining attention. Due to its complex molecular structure and composition, coal tar provides a natural possibility for the preparation of negative electrode materials with special properties.

[0005] The main measures to improve the cycle of artificial graphite are: reducing expansion, reducing specific surface area and controlling particle size distribution, but it is difficult to achieve significant improvement using current technology. As a way to improve the initial efficiency and cycle performance of materials, lithium supplementation of materials requires high material preparation environment and its consistency is difficult to control, making it difficult to industrialize. Patent CN202310643309.1 discloses a method for preparing negative electrode materials used in energy storage lithium-ion batteries. The preparation process is to select high isotropic asphalt coke for low-temperature graphitization to obtain a graphite precursor material; add metallic lithium and polymer to an organic solvent, filter, and vacuum dry to obtain a lithium supplement agent; add the graphite precursor material, lithium supplement agent and binder to a ball mill and mix evenly, pre-carbonize, secondary granulate, and vapor deposit to obtain a graphite composite material. However, the graphite composite material prepared by this method has problems such as large expansion and low electron and lithium ion transmission rate of the core graphite, thereby reducing its rate performance and causing deviations in its cycle performance under high rate conditions. Summary of the invention

[0006] Based on this, it is necessary to provide a method for preparing a lithium-doped amorphous carbon-coated graphite composite material that can solve the above problems.

[0007] In addition, it is also necessary to provide a lithium-doped amorphous carbon-coated graphite composite material prepared by the preparation method of the above-mentioned lithium-doped amorphous carbon-coated graphite composite material and the application of the above-mentioned lithium-doped amorphous carbon-coated graphite composite material.

[0008] A method for preparing a lithium-doped amorphous carbon-coated graphite composite material comprises the following steps:

[0009] The asphalt coke, nitrogen-containing polymer, lithium fluoride, oxidant and asphalt are uniformly mixed to obtain a mixed raw material, and the mixed raw material is graphitized to obtain a graphite precursor material;

[0010] The liquid coating agent is dissolved in an organic solvent to obtain an organic solution of the liquid coating agent, a graphite precursor and a lithium supplement agent are added to the organic solution of the liquid coating agent, the mixture is evenly dispersed and then spray-dried, and the dried product is then sintered to obtain the desired lithium-doped amorphous carbon-coated graphite composite material, wherein the lithium-doped amorphous carbon-coated graphite composite material includes a core of a graphite material and a shell of a lithium-doped amorphous carbon material coated outside the core.

[0011] In one embodiment, in the operation of uniformly mixing the asphalt coke, the nitrogen-containing polymer, the lithium fluoride, the oxidant and the asphalt to obtain the mixed raw material, the mass ratio of the asphalt coke, the nitrogen-containing polymer, the lithium fluoride, the oxidant and the asphalt is 100:1-5:1-5:1-5:1-5.

[0012] In one embodiment, the nitrogen-containing polymer is selected from at least one of melamine, polyaniline, polypyrrole, polythiophene and polydopamine;

[0013] The oxidant is selected from at least one of peracetic acid, hydrogen peroxide, perbenzoic acid, lauroyl peroxide and peroxyacetic acid.

[0014] In one embodiment, the operation of graphitizing the mixed raw material is: heating the mixed raw material to 200℃-300℃ and maintaining it for 1h-6h, then heating it to 600℃-800℃ and maintaining it for 0.5-2h, and finally heating it to 2200℃-2800℃ and maintaining it for 24-48h.

[0015] In one embodiment, in the operation of adding the graphite precursor and the lithium supplement agent to the organic solution of the liquid coating agent, the concentration of the organic solution of the liquid coating agent is 1wt-10wt%, and the mass ratio of the graphite precursor, the lithium supplement agent and the liquid coating agent is 100:1-5:1-5.

[0016] In one embodiment, the organic solvent is selected from at least one of dimethyl sulfoxide, cyclohexane and N-methylpyrrolidone;

[0017] The liquid coating agent is selected from at least one of phthalates, aliphatic dibasic acid esters, fatty acid esters, benzene polyesters, polyol esters and epoxy hydrocarbons;

[0018] The lithium supplement is a polymer doped with lithium powder, wherein the mass ratio of the polymer to the lithium powder is 10:1-3, and the polymer is selected from at least one of polyalkylene carbonate, polyalkylene oxide, polyalkylsiloxane, polyalkyl acrylate and polyalkyl methacrylate.

[0019] In one embodiment, the lithium supplement agent is prepared by the following operation: dissolving the polymer in a dimethyl carbonate solution to prepare a polymer solution with a concentration of 1wt-10wt%, then adding the lithium powder and dispersing it evenly, and spray drying to obtain the lithium supplement agent.

[0020] In one embodiment, in the operation of sintering the dried product, the sintering temperature is 1000° C.-1300° C., and the sintering time is 1 h-6 h.

[0021] A lithium-doped amorphous carbon-coated graphite composite material is prepared by the above-mentioned method for preparing the lithium-doped amorphous carbon-coated graphite composite material.

[0022] Application of the above-mentioned lithium-doped amorphous carbon-coated graphite composite material in the field of energy storage devices.

[0023] The preparation method of the lithium-doped amorphous carbon-coated graphite composite material of the present invention utilizes the adhesiveness of asphalt coke and the chemical groups on the surface of the oxidant to form a carbon structure connected by chemical bonds, doping lithium fluoride into the asphalt coke to reduce material defects, adding an oxidant to form pores to improve the isotropy of the material and reduce expansion, and sintering the nitrogen-containing polymer and lithium fluoride to achieve nitrogen-lithium doping, thereby improving the electronic and ionic conductivity of the core material, reducing its irreversible capacity and improving the initial efficiency, while coating the outer shell with a lithium supplement to improve the loss of lithium ions during charging and discharging, improve the cycle life, and provide sufficient lithium ions during high-rate charging and discharging, improve high-rate performance, and improve rate and cycle performance.

[0024] In combination with the specific embodiments, the lithium-doped amorphous carbon-coated graphite composite material prepared by the preparation method of the lithium-doped amorphous carbon-coated graphite composite material of the present invention has a large interlayer spacing, a high first efficiency and good cycle performance under high rate conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] in:

[0027] Figure 1 The present invention is a flow chart of a method for preparing a lithium-doped amorphous carbon-coated graphite composite material according to one embodiment.

[0028] Figure 2 This is a SEM image of the lithium-doped amorphous carbon-coated graphite composite material prepared in Example 1. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] In the present invention, the descriptions involving "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0031] Combination Figure 1 The present invention discloses a method for preparing a lithium-doped amorphous carbon-coated graphite composite material according to an embodiment of the present invention, comprising the following steps:

[0032] S10, mixing the asphalt coke, the nitrogen-containing polymer, the lithium fluoride, the oxidant and the asphalt uniformly to obtain a mixed raw material, and graphitizing the mixed raw material to obtain a graphite precursor material.

[0033] It should be noted that in S10, the operation of graphitizing the mixed raw material needs to be performed under a protective gas atmosphere, which may be a nitrogen atmosphere, a helium atmosphere, a neon atmosphere, an argon atmosphere, or the like.

[0034] It should be pointed out that the graphite precursor material prepared in S10 is used as a core material, and its specific material is graphite doped with heteroatoms such as N, F, and Li.

[0035] Pitch coke is a low-sulfur, low-ash coke obtained by direct coking of coal tar pitch (medium-temperature pitch or hard pitch) in a coke oven. Pitch coke is one of the main raw materials for artificial graphite negative electrode materials due to its low ash, low sulfur, high mechanical strength and easy graphitization.

[0036] The adhesive property of pitch coke can be used to react with the chemical groups on the surface of the oxidant to form a carbon structure connected by chemical bonds.

[0037] Pitch coke has high isotropy, high residual carbon content, easy graphitization, and easy to form a lamellar structure at high temperature. It has the characteristics of high specific capacity and high first efficiency. Pitch has a low softening point, low residual carbon content, strong fluidity, and is difficult to graphitize at high temperatures. It has a low first efficiency and low specific capacity. Pitch coke and asphalt are of the same origin, that is, they differ in specific capacity, first efficiency and power. Pitch coke can be used directly as a negative electrode material, while asphalt can only be used as a coating agent and its granulating agent.

[0038] By adding oxidants to form pores, the isotropy of the material is improved and the expansion is reduced. At the same time, the oxidants form hydroxyl groups on the surface of the material, dehydrate, carbonize and form a porous structure, improve the isotropy of the material and its porous structure, and improve the liquid retention performance.

[0039] Nitrogen-containing polymers and lithium fluoride are sintered to achieve nitrogen-lithium doping, which improves the electronic and ionic conductivity of the core material.

[0040] Compared with other lithium compounds, lithium fluoride will have residual fluorine atoms during the sintering and doping process. Fluorine atoms have good compatibility with lithium hexafluorophosphate in the electrolyte, reducing interfacial impedance and improving cycle performance.

[0041] Generally speaking, pitch coke can be one of coal-based pitch coke, petroleum pitch coke and mesophase pitch.

[0042] Preferably, in the operation of uniformly mixing the asphalt coke, the nitrogen-containing polymer, the lithium fluoride, the oxidant and the asphalt to obtain the mixed raw material, the mass ratio of the asphalt coke, the nitrogen-containing polymer, the lithium fluoride, the oxidant and the asphalt is 100:1-5:1-5:1-5:1-5.

[0043] Specifically, in the present embodiment, the nitrogen-containing polymer is at least one selected from melamine, polyaniline, polypyrrole, polythiophene and polydopamine.

[0044] Nitrogen-containing polymers such as melamine, polyaniline, polypyrrole, polythiophene and polydopamine are carbonized at high temperatures to form carbonitrides, which can achieve nitrogen doping.

[0045] Nitrogen-containing polymers and lithium fluoride are sintered to achieve nitrogen-lithium doping, thereby improving the electronic and ionic conductivity of the core material, reducing its irreversible capacity and improving the initial efficiency.

[0046] Specifically, in this embodiment, the oxidant is at least one selected from peracetic acid, hydrogen peroxide, perbenzoic acid, lauroyl peroxide and acetic acid peroxide.

[0047] Peroxides are strong oxidants, and the peroxy group (-OO-) in them easily reacts with asphalt coke to form a carbon structure connected by chemical bonds.

[0048] Specifically, in this embodiment, the operation of graphitizing the mixed raw material is: heating the mixed raw material to 200℃-300℃ and maintaining it for 1h-6h, then heating it to 600℃-800℃ and maintaining it for 0.5-2h, and finally heating it to 2200℃-2800℃ and maintaining it for 24-48h.

[0049] Specifically, the mixed raw materials are melted at 200-300°C, pre-carbonized at 600-800°C, and low-temperature graphitized at 2200-2800°C.

[0050] The conventional graphitization temperature is generally between 3000°C and 4200°C. In the present embodiment, graphitization is achieved at a relatively low temperature, which can increase the interlayer spacing of the material, thereby reducing the expansion of the material and improving the cycle performance.

[0051] Specifically, in this embodiment, the operation of graphitizing the mixed raw material can be performed in a tubular furnace.

[0052] S20, dissolving the liquid coating agent in an organic solvent to obtain an organic solution of the liquid coating agent, adding the graphite precursor and the lithium supplement agent to the organic solution of the liquid coating agent, spray drying after uniform dispersion, and then sintering the dried product to obtain the desired lithium-doped amorphous carbon-coated graphite composite material.

[0053] It should be noted that in S20, the operation of sintering the dried product needs to be performed under a protective gas atmosphere, which may be a nitrogen atmosphere, a helium atmosphere, a neon atmosphere, an argon atmosphere, or the like.

[0054] Specifically, the prepared lithium-doped amorphous carbon-coated graphite composite material includes a core of graphite material and a shell of lithium-doped amorphous carbon material coated outside the core.

[0055] The lithium supplement agent coated in the outer shell reduces the loss of lithium ions during the charge and discharge process, thereby increasing the cycle life, and provides sufficient lithium ions during the high-rate charge and discharge process, thereby improving the high-rate performance, and improving the rate and cycle performance.

[0056] By spray-drying an organic solution of a uniformly dispersed graphite precursor, a lithium supplement and a liquid coating agent, the dispersed system is atomized and then in contact with hot air, the solvent is rapidly vaporized and dried, thereby quickly preparing a powdered product, eliminating traditional evaporation, crushing and other processes.

[0057] Preferably, in the operation of adding the graphite precursor and the lithium supplement agent to the organic solution of the liquid coating agent, the concentration of the organic solution of the liquid coating agent is 1wt-10wt%, and the mass ratio of the graphite precursor, the lithium supplement agent and the liquid coating agent is 100:1-5:1-5.

[0058] Specifically, in this embodiment, the organic solvent is selected from at least one of dimethyl sulfoxide, cyclohexane or N-methylpyrrolidone.

[0059] Specifically, in this embodiment, the liquid coating agent is selected from at least one of phthalic acid esters, aliphatic dibasic acid esters, fatty acid esters, benzene polyesters, polyol esters and epoxy hydrocarbons.

[0060] Preferably, in this embodiment, the lithium supplement is a polymer doped with lithium powder, wherein the mass ratio of the polymer to the lithium powder is 10:1-3, and the polymer is selected from at least one of polyalkylene carbonate, polyalkylene oxide, polyalkylsiloxane, polyalkyl acrylate and polyalkyl methacrylate.

[0061] During the formation process of lithium-ion batteries, SEI growth on the negative electrode surface consumes active lithium, resulting in battery energy loss, which in turn causes problems such as low first-cycle efficiency and poor cycle life. Lithium replenishers actually pre-lithiate electrode materials to improve first-cycle efficiency and life by replenishing lithium loss during the first cycle. Lithium replenishment technology can compensate for active lithium, improve the shortcoming of low first-cycle efficiency of silicon-carbon negative electrodes, give full play to their high capacity advantages, increase battery energy density and extend cycle life.

[0062] The lithium supplement is a polymer doped with lithium powder, which not only protects the lithium powder to a certain extent, but also forms porous carbide during the sintering process.

[0063] Specifically, in this embodiment, the lithium supplement is prepared by the following operation: a polymer is dissolved in a dimethyl carbonate solution to prepare a polymer solution with a concentration of 1wt-10wt%, and then lithium powder is added and dispersed evenly, and the lithium supplement is obtained after spray drying. Spray drying allows the dispersed system to be atomized and contacted with hot air, and the solvent is quickly vaporized to achieve drying, so that a powdered product can be quickly prepared, eliminating traditional evaporation, crushing and other processes.

[0064] Preferably, in the subsequent sintering operation of the dried product, the sintering temperature is 1000° C.-1300° C., and the sintering time is 1 h-6 h.

[0065] The preparation method of the lithium-doped amorphous carbon-coated graphite composite material of the present invention utilizes the adhesiveness of asphalt coke and the chemical groups on the surface of the oxidant to form a carbon structure connected by chemical bonds, doping lithium fluoride into the asphalt coke to reduce material defects, adding an oxidant to form pores to improve the isotropy of the material and reduce expansion, and sintering the nitrogen-containing polymer and lithium fluoride to achieve nitrogen-lithium doping, thereby improving the electronic and ionic conductivity of the core material, reducing its irreversible capacity and improving the initial efficiency, while coating the outer shell with a lithium supplement to improve the loss of lithium ions during charging and discharging, improve the cycle life, and provide sufficient lithium ions during high-rate charging and discharging, improve high-rate performance, and improve rate and cycle performance.

[0066] In combination with the specific embodiments, the lithium-doped amorphous carbon-coated graphite composite material prepared by the preparation method of the lithium-doped amorphous carbon-coated graphite composite material of the present invention has a large interlayer spacing, a high first efficiency and good cycle performance under high rate conditions.

[0067] The present invention also discloses an embodiment of a lithium-doped amorphous carbon-coated graphite composite material prepared by the above-mentioned method for preparing the lithium-doped amorphous carbon-coated graphite composite material.

[0068] Specifically, the lithium-doped amorphous carbon-coated graphite composite material includes a core of graphite material and a shell of lithium-doped amorphous carbon material coated outside the core.

[0069] The lithium-doped amorphous carbon-coated graphite composite material prepared by the preparation method of the lithium-doped amorphous carbon-coated graphite composite material of the present invention forms a carbon structure connected by chemical bonds by utilizing the adhesiveness of asphalt coke and the chemical groups on the surface of the oxidant, doping lithium fluoride into the asphalt coke to reduce material defects, adding an oxidant to form pores to improve the isotropy of the material and reduce expansion, and nitrogen-containing polymers and lithium fluoride are sintered to achieve nitrogen-lithium doping, thereby improving the electronic and ionic conductivity of the core material, reducing its irreversible capacity and improving the initial efficiency, while coating the outer shell with a lithium supplement to improve the loss of lithium ions during charging and discharging, improve the cycle life, and provide sufficient lithium ions during high-rate charging and discharging, improve high-rate performance, and improve rate and cycle performance.

[0070] In combination with the specific embodiments, the lithium-doped amorphous carbon-coated graphite composite material of the present invention has a large interlayer spacing, a high first efficiency and good cycle performance under high rate conditions.

[0071] The invention also discloses the application of the lithium-doped amorphous carbon-coated graphite composite material in the field of energy storage devices.

[0072] For example, the lithium-doped amorphous carbon-coated graphite composite material can be applied to the field of secondary batteries.

[0073] Specifically, the lithium-doped amorphous carbon-coated graphite composite material can be used as a negative electrode material for lithium-ion secondary batteries.

[0074] In addition, the lithium-doped amorphous carbon-coated graphite composite material can also be used in fields such as supercapacitors.

[0075] The following are specific embodiments.

[0076] Sources of key raw materials:

[0077] Coal-based pitch coke: Manufacturer: Hebei Deri New Material Technology Co., Ltd.; CAS No.: 8042-42-4;

[0078] Petroleum asphalt coke: Manufacturer: PetroChina Jinxi Petrochemical Co., Ltd.; Model: 1#B;

[0079] Asphalt: Manufacturer: Liaoning Xinde New Materials Technology Co., Ltd.; Model: 250#;

[0080] Lithium powder: Manufacturer: Tianjin Zhongneng Lithium Industry Co., Ltd.; Model: passivated lithium powder.

[0081] Example 1

[0082] A method for preparing a lithium-doped amorphous carbon-coated graphite composite material comprises the following steps:

[0083] Weigh 100 g of coal-based pitch coke, 3 g of melamine, 3 g of lithium fluoride, 3 g of peracetic acid and 3 g of asphalt, mix them evenly and transfer them to a tube furnace, heat them to 250 ° C for melting for 3 h under a nitrogen atmosphere, then heat them to 700 ° C for 1 h, and heat them to 2600 ° C for low-temperature graphitization for 36 h to obtain a graphite precursor material;

[0084] 10g of polyalkylene carbonate was dissolved in 200g of dimethyl carbonate to prepare a 5wt% solution, and then 2g of lithium powder was added and dispersed evenly, and spray-dried to obtain a lithium supplement;

[0085] 3g of phthalate is added to 60g of dimethyl sulfoxide organic solvent to prepare a 5wt% solution, then 3g of lithium supplement and 100g of graphite precursor are added and dispersed evenly, spray dried, and then heated to 1150°C and sintered for 3h in a nitrogen atmosphere to obtain the required lithium-doped amorphous carbon-coated graphite composite material. The prepared lithium-doped amorphous carbon-coated graphite composite material includes a shell of lithium-doped amorphous carbon material and a core of graphite material.

[0086] Example 2

[0087] A method for preparing a lithium-doped amorphous carbon-coated graphite composite material comprises the following steps:

[0088] Weigh 100g of coal-based pitch coke, 1g of polyaniline, 1g of lithium fluoride, 1g of peroxybenzoic acid and 1g of asphalt, mix them evenly and transfer them to a tubular furnace, heat them to 200°C for melting for 6h under a nitrogen atmosphere, then heat them to 600°C for 2h, and heat them to 2200°C for low-temperature graphitization for 48h to obtain a graphite precursor material;

[0089] 10g of polyalkylene oxide was dissolved in 1000g of dimethyl carbonate to prepare a 1wt% solution, and then 1g of lithium powder was added and dispersed evenly, and spray-dried to obtain a lithium supplement;

[0090] 1g of aliphatic dibasic acid ester is added to 100g of cyclohexane organic solvent to prepare a 1wt% solution, then 1g of lithium supplement and 100g of graphite precursor are added and dispersed evenly, spray dried, and then heated to 1000°C and sintered for 6h in a nitrogen atmosphere to obtain the required lithium-doped amorphous carbon-coated graphite composite material. The prepared lithium-doped amorphous carbon-coated graphite composite material includes a shell of lithium-doped amorphous carbon material and a core of graphite material.

[0091] Example 3

[0092] A method for preparing a lithium-doped amorphous carbon-coated graphite composite material comprises the following steps:

[0093] Weigh 100 g of petroleum asphalt coke, 5 g of polydopamine, 5 g of lithium fluoride, 5 g of peroxyacetic acid and 5 g of asphalt, mix them evenly and transfer them to a tube furnace, then heat them to 300 ° C to melt for 1 h, then heat them to 800 ° C for 0.5 h under a nitrogen atmosphere, and then heat them to 2800 ° C for low-temperature graphitization for 24 h to obtain a graphite precursor material;

[0094] 10g of polyalkylsiloxane was dissolved in 100g of dimethyl carbonate to prepare a 10wt% solution, and then 3g of lithium powder was added and dispersed evenly, and spray-dried to obtain a lithium supplement;

[0095] 5g of fatty acid ester is added to 50g of N-methylpyrrolidone organic solvent to prepare a 10wt% solution, and then 5g of lithium supplement and 100g of graphite precursor are added and dispersed evenly, spray dried, and then heated to 1300°C and sintered for 1h in a nitrogen atmosphere to obtain the required lithium-doped amorphous carbon-coated graphite composite material. The prepared lithium-doped amorphous carbon-coated graphite composite material includes a shell of lithium-doped amorphous carbon material and a core of graphite material.

[0096] Example 4

[0097] A method for preparing a lithium-doped amorphous carbon-coated graphite composite material comprises the following steps:

[0098] Weigh 100g of coal-based pitch coke, 1g of polythiophene, 5g of lithium fluoride, 1g of lauroyl peroxide and 5g of asphalt, mix them evenly and transfer them to a tube furnace, then heat them to 250°C for melting for 3h under a nitrogen atmosphere, then heat them to 700°C for 1h, and heat them to 2600°C for low-temperature graphitization for 36h to obtain a graphite precursor material;

[0099] 10g of polyalkylene carbonate was dissolved in 200g of dimethyl carbonate to prepare a 5wt% solution, and then 2g of lithium powder was added and dispersed evenly, and spray-dried to obtain a lithium supplement;

[0100] 3g of phthalate is added to 60g of dimethyl sulfoxide organic solvent to prepare a 5wt% solution, then 3g of lithium supplement and 100g of graphite precursor are added and dispersed evenly, spray dried, and then sintered at 1150°C for 3h in a nitrogen atmosphere to obtain the required lithium-doped amorphous carbon-coated graphite composite material. The prepared lithium-doped amorphous carbon-coated graphite composite material includes a shell of lithium-doped amorphous carbon material and a core of graphite material.

[0101] Example 5

[0102] A method for preparing a lithium-doped amorphous carbon-coated graphite composite material comprises the following steps:

[0103] Weigh 100g of coal-based pitch coke, 5g of melamine, 1g of lithium fluoride, 5g of hydrogen peroxide and 1g of asphalt, mix them evenly and transfer them to a tubular furnace, then heat them to 250°C for melting for 3h under a nitrogen atmosphere, then heat them to 700°C for 1h, and heat them to 2600°C for low-temperature graphitization for 36h to obtain a graphite precursor material;

[0104] 10g of polyalkylene carbonate was dissolved in 200g of dimethyl carbonate to prepare a 5wt% solution, and then 2g of lithium powder was added and dispersed evenly, and spray-dried to obtain a lithium supplement;

[0105] 3g of phthalate is added to 60g of dimethyl sulfoxide organic solvent to prepare a 5wt% solution, then 3g of lithium supplement and 100g of graphite precursor are added and dispersed evenly, spray dried, and then sintered at 1150°C for 3h in a nitrogen atmosphere to obtain the required lithium-doped amorphous carbon-coated graphite composite material. The prepared lithium-doped amorphous carbon-coated graphite composite material includes a shell of lithium-doped amorphous carbon material and a core of graphite material.

[0106] Comparative Example 1

[0107] Comparative Example 1 is substantially the same as Example 1, except that no lithium supplementing agent is added.

[0108] The specific preparation process is as follows:

[0109] Weigh 100 g of coal-based pitch coke, 3 g of melamine, 3 g of lithium fluoride, 3 g of peracetic acid and 3 g of asphalt, mix them evenly and transfer them to a tube furnace, heat them to 250 ° C for melting for 3 h under a nitrogen atmosphere, then heat them to 700 ° C for 1 h, and heat them to 2600 ° C for low-temperature graphitization for 36 h to obtain a graphite precursor material;

[0110] 3g of phthalate is added to 60g of dimethyl sulfoxide organic solvent to prepare a 5wt% solution, and then 100g of graphite precursor is added and dispersed evenly, spray dried, and then heated to 1150°C and sintered for 3h in a nitrogen atmosphere to obtain the required amorphous carbon-coated graphite composite material. The prepared amorphous carbon-coated graphite composite material includes a shell of an amorphous carbon material and a core of a graphite material.

[0111] Comparative Example 2

[0112] Comparative Example 2 is substantially the same as Example 1, except that lithium fluoride and peracetic acid are not added.

[0113] Weigh 100g of coal-based pitch coke, 3g of melamine and 3g of asphalt, mix them evenly and transfer them to a tubular furnace, heat them to 250°C for melting for 3h under a nitrogen atmosphere, then heat them to 700°C for 1h, and heat them to 2600°C for low-temperature graphitization for 36h to obtain a graphite precursor material;

[0114] 10g of polyalkylene carbonate was dissolved in 200g of dimethyl carbonate to prepare a 5wt% solution, and then 2g of lithium powder was added and dispersed evenly, and spray-dried to obtain a lithium supplement;

[0115] 3g of phthalate is added to 60g of dimethyl sulfoxide organic solvent to prepare a 5wt% solution, then 3g of lithium supplement and 100g of graphite precursor are added and dispersed evenly, spray dried, and then heated to 1150°C and sintered for 3h in a nitrogen atmosphere to obtain the required lithium-doped amorphous carbon-coated graphite composite material. The prepared lithium-doped amorphous carbon-coated graphite composite material includes a shell of lithium-doped amorphous carbon material and a core of graphite material.

[0116] Test Case

[0117] (1) SEM test

[0118] The lithium-doped amorphous carbon-coated graphite composite material prepared in Example 1 was subjected to SEM testing, and the results were as follows: Figure 2 shown.

[0119] Depend on Figure 2 It can be seen that the lithium-doped amorphous carbon-coated graphite composite material prepared in Example 1 presents a secondary particle structure, with a reasonable size distribution and a particle size between 10 μm and 15 μm.

[0120] (2) Physical and chemical performance test and button battery test:

[0121] According to the national standard GB / T-24533-2019 "Graphite Anode Materials for Lithium-ion Batteries", the material's interlayer spacing D002, specific surface area, tap density, degree of graphitization and OI value of its powder material are tested.

[0122] The lithium-doped amorphous carbon-coated graphite composite materials prepared in Examples 1-5, the amorphous carbon-coated graphite composite materials prepared in Comparative Example 1, and the lithium-doped amorphous carbon-coated graphite composite materials prepared in Comparative Example 2 were used as negative electrode carbon materials to prepare negative electrode slurries. The negative electrode slurry formula was negative electrode carbon material: LA133: SBR: SP: H 2 O=95.5:2.5:1:1:150), the negative electrode slurry is coated on the copper foil, dried, rolled and cut to obtain the negative electrode sheet. The lithium sheet is used as the counter electrode and the electrolyte is LiPF 6 / EC+DEC, the volume ratio of electrolyte solvent EC:DEC=1:1, the diaphragm is made of polyethylene PE film, and the button cell is assembled in an argon-filled glove box.

[0123] The prepared button batteries were installed on Wuhan Blue Electric CT2001A battery tester for electrochemical performance testing. The charge and discharge voltage range was controlled at 0.005-2.0 V, and the charge and discharge rate was 0.1C. Finally, they were assembled into button batteries A1, A2, A3 and B1, B2, and their cycle performance (0.5C / 0.5C, 100 weeks) was tested. The test results are shown in Table 1.

[0124] Table 1

[0125]

[0126] From Table 1, it can be seen that the lithium-doped amorphous carbon-coated graphite composite materials prepared in Examples 1-5 have a large interlayer spacing and a high first efficiency. The reason is that the nitrogen-containing polymer and lithium fluoride are sintered to achieve nitrogen-lithium doping to improve the electronic and ionic conductivity of the core material, reduce its irreversible capacity and improve the first efficiency, and the nitrogen-containing polymer promotes the layer expansion of amorphous carbon during the carbonization and volatilization process, so that it can provide sufficient lithium ions during high-rate charge and discharge, thereby improving the cycle performance; at the same time, low-temperature graphitization increases the interlayer spacing of the material.

[0127] 3) Soft pack battery

[0128] The lithium-doped amorphous carbon-coated graphite composite materials prepared in Examples 1-5, the amorphous carbon-coated graphite composite materials prepared in Comparative Example 1, and the lithium-doped amorphous carbon-coated graphite composite materials prepared in Comparative Example 2 were used as negative electrode carbon materials to prepare negative electrode slurries. The negative electrode slurry formula was negative electrode carbon material: LA133: SBR: SP: H 2 O=95.5:2.5:1:1:150, the negative electrode slurry is coated on the copper foil, dried, rolled and cut to obtain the negative electrode sheet. LFP is used as the positive electrode, the solvent is EC / DEC / PC (EC:DEC:PC=1:1:1) as the electrolyte, and the solute is LiPF 6 (1.3mol / L), Celgard 2400 membrane was used as the separator, and 5Ah soft-pack batteries C1, C2, C3, C4, C5 and D1, E1 were prepared respectively.

[0129] Then, the liquid absorption capacity of the negative electrode sheet and the cycle performance (2.0C / 2.0C) of the soft-pack battery were tested. The cycle test method was: 2C / 2C, 2.8-4.2V, 25±3°C, 500 weeks. The test results are shown in Table 2 below.

[0130] Table 2

[0131]

[0132] From Table 2, it can be seen that the liquid absorption and retention capacity of the negative electrode using the lithium-doped amorphous carbon-coated graphite composite materials prepared in Examples 1-5 as the negative electrode carbon material is significantly better than that of the comparative example. The reason for this is that the lithium-doped amorphous carbon-coated graphite composite materials prepared in Examples 1-5 have a high specific surface area, which improves the liquid absorption capacity of the material and improves the cycle performance; at the same time, the lithium-doped amorphous carbon-coated graphite composite materials prepared in Examples 1-5 have a large interlayer spacing, which reduces the expansion of the material and improves the cycle performance.

[0133] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a lithium-doped amorphous carbon-coated graphite composite material, It is characterized in that The steps include: The asphalt coke, nitrogen-containing polymer, lithium fluoride, oxidant and asphalt are uniformly mixed to obtain a mixed raw material, and the mixed raw material is graphitized to obtain a graphite precursor material; The liquid coating agent is dissolved in an organic solvent to obtain an organic solution of the liquid coating agent, a graphite precursor and a lithium supplement agent are added to the organic solution of the liquid coating agent, the mixture is evenly dispersed and then spray-dried, and the dried product is then sintered to obtain the desired lithium-doped amorphous carbon-coated graphite composite material, wherein the lithium-doped amorphous carbon-coated graphite composite material includes a core of a graphite material and a shell of a lithium-doped amorphous carbon material coated outside the core.

2. The method for preparing the lithium-doped amorphous carbon-coated graphite composite material according to claim 1, It is characterized in that In the operation of uniformly mixing the asphalt coke, the nitrogen-containing polymer, the lithium fluoride, the oxidant and the asphalt to obtain the mixed raw material, the mass ratio of the asphalt coke, the nitrogen-containing polymer, the lithium fluoride, the oxidant and the asphalt is 100:1-5:1-5:1-5:1-5.

3. The method for preparing the lithium-doped amorphous carbon-coated graphite composite material according to claim 2, It is characterized in that The nitrogen-containing polymer is selected from at least one of melamine, polyaniline, polypyrrole, polythiophene and polydopamine; The oxidant is selected from at least one of peracetic acid, hydrogen peroxide, perbenzoic acid, lauroyl peroxide and peroxyacetic acid.

4. The method for preparing the lithium-doped amorphous carbon-coated graphite composite material according to claim 2, It is characterized in that The operation of graphitizing the mixed raw material is as follows: heating the mixed raw material to 200°C-300°C and maintaining it for 1h-6h, then heating it to 600°C-800°C and maintaining it for 0.5-2h, and finally heating it to 2200°C-2800°C and maintaining it for 24-48h.

5. The method for preparing the lithium-doped amorphous carbon-coated graphite composite material according to any one of claims 1 to 4, It is characterized in that In the operation of adding the graphite precursor and the lithium supplement agent to the organic solution of the liquid coating agent, the concentration of the organic solution of the liquid coating agent is 1wt-10wt%, and the mass ratio of the graphite precursor, the lithium supplement agent and the liquid coating agent is 100:1-5:1-5.

6. The method for preparing the lithium-doped amorphous carbon-coated graphite composite material according to claim 5, It is characterized in that The organic solvent is selected from at least one of dimethyl sulfoxide, cyclohexane and N-methylpyrrolidone; The liquid coating agent is selected from at least one of phthalates, aliphatic dibasic acid esters, fatty acid esters, benzene polyesters, polyol esters and epoxy hydrocarbons; The lithium supplement is a polymer doped with lithium powder, wherein the mass ratio of the polymer to the lithium powder is 10:1-3, and the polymer is selected from at least one of polyalkylene carbonate, polyalkylene oxide, polyalkylsiloxane, polyalkyl acrylate and polyalkyl methacrylate.

7. The method for preparing the lithium-doped amorphous carbon-coated graphite composite material according to claim 6, It is characterized in that The lithium supplement agent is prepared by the following operation: dissolving the polymer in a dimethyl carbonate solution to prepare a polymer solution with a concentration of 1wt-10wt%, then adding the lithium powder and dispersing it evenly, and spray drying to obtain the lithium supplement agent.

8. The method for preparing the lithium-doped amorphous carbon-coated graphite composite material according to claim 5, It is characterized in that In the subsequent operation of sintering the dried product, the sintering temperature is 1000° C.-1300° C., and the sintering time is 1 h-6 h.

9. A lithium-doped amorphous carbon-coated graphite composite material, It is characterized in that The lithium-doped amorphous carbon-coated graphite composite material is prepared by the preparation method of the lithium-doped amorphous carbon-coated graphite composite material according to any one of claims 1 to 8.

10. Use of the lithium-doped amorphous carbon-coated graphite composite material according to claim 9 in the field of energy storage devices.

Citation Information

Cited By

  • Graphite composite material and preparation method and application thereof

    CN120545338A

  • Fluorine-doped modified artificial graphite as well as preparation method and application thereof

    CN121292428A

  • A fluorine-doped modified artificial graphite, its preparation method and application

    CN121292428B