O-band silicon-based III-V quantum dot narrow linewidth laser and preparation method thereof

By epitaxial growth and optimization of structure on the silicon substrate layer, an O-band silicon-based three-five-group quantum dot narrow linewidth laser with ridge waveguides and gratings is solved, and the monolithic integration problem is solved. The large size of the optical isolator and the material is incompatible. Problem, high-performance, low-cost laser design is achieved.

CN119050812AActive Publication Date: 2024-11-29XIAN INST OF OPTICS & PRECISION MECHANICS CHINESE ACAD OF SCI

Patent Information

Application Number
CN202411168520.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

It is difficult to prepare a high-performance O-band silicon-based three-five-group quantum dot narrow linewidth laser that can be integrated monolithically, and the external coupling chip of the optical isolator occupies a large volume and is incompatible with materials.

Method used

The buffer layer, lower waveguide layer, lower limit layer, InAs quantum dot layer/InGaAs barrier layer, upper limit layer, upper waveguide layer and ohmic contact layer are formed on the silicon substrate layer to form a ridge waveguide and grating, using AlGaAs material Optimize the waveguide and limiting layer, combining the SiO2 passivation layer and metal contact window to achieve monolithic integration.

Benefits of technology

It has realized a high-performance O-band silicon-based quantum dot narrow linewidth laser that can be integrated monolithically, with narrow linewidth, high reflection tolerance, high temperature stability, and low threshold current density, and is suitable for future large-scale silicon photonic integration systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005008499840000011
    Figure HDA0005008499840000011
  • Figure HDA0005008499840000012
    Figure HDA0005008499840000012
Patent Text Reader

Abstract

The invention relates to the technical field of semiconductor lasers, in particular to an O-band silicon-based III-V quantum dot narrow linewidth laser and a preparation method thereof. The O-band silicon-based III-V quantum dot narrow linewidth laser comprises a silicon substrate layer, and a buffer layer, a lower waveguide layer, a lower limiting layer, a quantum dot active layer, an upper limiting layer, an upper waveguide layer, an ohmic contact layer and an electrode layer are sequentially stacked on the silicon substrate layer. The upper waveguide layer and the ohmic contact layer form a ridge waveguide and a grating on at least one side of the ridge waveguide; and the quantum dot active layer comprises an InAs quantum dot layer / InGaAs barrier layer. The O-band silicon-based III-V quantum dot narrow linewidth laser has the advantages of being narrow in linewidth, high in reflection tolerance, high in temperature stability, low in threshold current density and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor lasers, and in particular to an O-band silicon-based III-V quantum dot narrow-linewidth laser and a preparation method thereof. Background Art

[0002] Currently, semiconductor lasers are developing rapidly in the direction of narrow linewidth and integration. By optimizing the laser chip structure design, monolithic integrated narrow linewidth laser output is obtained. At the same time, combined with its small size, light weight, high conversion efficiency, wide spectral range and other advantages, narrow linewidth lasers have a wide range of applications in coherent optical communications, atomic clock pumping and other fields.

[0003] In the prior art, it is easy to realize silicon photonic integration by directly growing quantum dots on silicon-based substrates. By introducing surface sidewall gratings on both sides of the ridge waveguide of the O-band (1260-1360nm) quantum dot laser, a quantum dot laser with narrow line width and excellent temperature stability can be realized, expanding its application in optoelectronic fields such as coherent optical communications. In addition, the backward transmission light generated due to various reasons in the laser optical path will generate noise after returning to the laser, affecting the stability of the laser working state, so it is necessary to insert an optical isolator between the semiconductor laser source and the transmission system to reduce the adverse effects of reflected light on the stability of the light source. However, the isolator usually requires an external coupling chip, which will occupy a large volume of the chip; in addition, the magneto-optical material used in the isolator is generally incompatible with the laser material. In response to the above problems, the III-V quantum dot laser has a very small line width broadening factor, which is 20 times smaller than the traditional quantum well laser. At the same time, it can effectively reduce the adverse effects of reflected light on the power stability of the light source, has excellent reflection tolerance, and can avoid the use of optical isolators, thereby greatly reducing the cost and volume of the laser chip. However, it is currently extremely challenging to prepare high-performance O-band silicon-based III-V quantum dot narrow-linewidth lasers that can be monolithically integrated. Summary of the invention

[0004] The purpose of the present invention is to provide an O-band silicon-based III-V quantum dot narrow linewidth laser to solve the problem in the prior art that it is difficult to prepare a high-performance O-band silicon-based III-V quantum dot narrow linewidth laser that can be monolithically integrated.

[0005] In order to solve the above problems, the present invention proposes an O-band silicon-based III-V quantum dot narrow linewidth laser, and the technical solution adopted is:

[0006] An O-band silicon-based III-V quantum dot narrow linewidth laser comprises a silicon substrate layer, on which a buffer layer, a lower waveguide layer, a lower confinement layer, a quantum dot active layer, an upper confinement layer, an upper waveguide layer, an ohmic contact layer and an electrode layer are sequentially stacked; the upper waveguide layer and the ohmic contact layer form a ridge waveguide and a grating on at least one side of the ridge waveguide; the quantum dot active layer comprises an InAs quantum dot layer / InGaAs barrier layer.

[0007] Furthermore, the buffer layer includes an AlAs nucleation layer, a GaAs buffer layer and an AlGaAs dislocation filtering layer in order from bottom to top, and the thickness of the GaAs buffer layer is 0.2-2 μm.

[0008] Furthermore, the number of periods of the InAs quantum dot layer / InGaAs barrier layer is 2-15; and the thickness of the InGaAs barrier layer is 2-20 nm.

[0009] Furthermore, the width of the ridge waveguide is 1.5-3 μm, the width of the single-side grating is 0.5-3 μm, the grating is a first-order grating or a high-order grating, the period of the first-order grating is 180-250 nm, and the duty cycle is 0.35-0.75.

[0010] Furthermore, the lower waveguide layer is an n-type AlGaAs waveguide layer with a thickness of 30-800nm; the lower confinement layer is an n-type AlGaAs confinement layer with a thickness of 50-300nm; the upper confinement layer is a p-type AlGaAs confinement layer with a thickness of 3-50nm; the upper waveguide layer is a p-type AlGaAs waveguide layer with a thickness of 200-3000nm; and the ohmic contact layer is a p-type GaAs ohmic contact layer with a thickness of 5-50nm.

[0011] Furthermore, the silicon substrate layer is a Si(001) substrate or a SOI substrate.

[0012] Furthermore, the ridge waveguide is a strip-shaped body located in the middle, and both sides of the ridge waveguide have symmetrical gratings extending along the length direction of the strip-shaped body, and the height of the gratings is consistent with the thickness of the upper waveguide layer.

[0013] Furthermore, both sides of the gratings on both sides away from the ridge waveguide and between adjacent gratings are filled with benzocyclobutene material to form a filling layer, and the thickness of the filling layer is consistent with the thickness of the upper waveguide layer.

[0014] Furthermore, SiO is deposited between the grating, the filling layer and the electrode layer. 2 The passivation layer, the SiO 2A metal contact window is opened on the passivation layer. The width of the metal contact window is the same as the width of the ohmic contact layer, and the ohmic contact layer is exposed to complete the ohmic contact with the electrode layer.

[0015] Beneficial effects: The present invention is an improved invention. The present invention epitaxially grows a buffer layer, a lower waveguide layer, a lower confinement layer, an InAs quantum dot layer / InGaAs barrier layer, an upper confinement layer, an upper waveguide layer, and an ohmic contact layer on a silicon substrate layer to achieve epitaxial growth of III-V quantum dots, and forms an upper waveguide layer and an ohmic contact layer to a ridge waveguide and a grating on at least one side of the ridge waveguide in the structural design of an O-band silicon-based III-V quantum dot narrow linewidth laser, thereby achieving a high-performance O-band silicon-based quantum dot narrow linewidth laser that can be integrated on a single chip, providing an ideal on-chip narrow linewidth light source for future large-scale silicon photonic integrated systems. The O-band silicon-based III-V quantum dot narrow linewidth laser of the present invention has the advantages of narrow linewidth, high reflection tolerance, high temperature stability, low threshold current density, etc., providing an ideal on-chip light source for future on-chip interconnection systems.

[0016] The buffer layer includes an AlAs nucleation layer, a GaAs buffer layer and an AlGaAs dislocation filtering layer from bottom to top. The thickness of the GaAs buffer layer is 0.2-2 μm. The above structural layers effectively prevent the dislocation caused by lattice mismatch from being transferred to the quantum dot gain region, ensuring that high-density and high-quality III-V group quantum dots can be epitaxially grown.

[0017] The period number of the InAs quantum dot layer / InGaAs barrier layer is 2-15, which comprises a combination of multiple quantum dot layers and barrier layers. The thickness of the InGaAs barrier layer is 2-20 nm, which improves the gain bandwidth and quantum efficiency of the laser and reduces the threshold current.

[0018] The width of the ridge waveguide is 1.5-3 μm, the width of the single-side grating is 0.5-3 μm, the grating is a first-order grating or a high-order grating, the period of the first-order grating is 180-250nm, and the duty cycle is 0.35-0.75, ensuring that the performance of the waveguide and the processing effect of the optical signal reach the best state.

[0019] The lower waveguide layer is an n-type AlGaAs waveguide layer with a thickness of 30-800nm; the lower confinement layer is an n-type AlGaAs confinement layer with a thickness of 50-300nm; the upper confinement layer is a P-type AlGaAs confinement layer with a thickness of 3-50nm; the upper waveguide layer is a P-type AlGaAs waveguide layer with a thickness of 200-3000nm; the ohmic contact layer is a p-type GaAs ohmic contact layer with a thickness of 5-50nm. The waveguide layer and confinement layer in this structure are both made of AlGaAs material, wherein the lower waveguide layer and the lower confinement layer are both n-type (i.e., the electron concentration is higher), and the upper confinement layer is P-type (i.e., the hole concentration is higher). The above structure realizes the optimization of the laser, thereby improving the efficiency and stability of the laser.

[0020] The ridge waveguide is a strip-shaped body located in the middle, and there are symmetrical gratings extending along the length direction of the strip-shaped body on both sides of the ridge waveguide. The height of the grating is consistent with the thickness of the upper waveguide layer, which can effectively improve the feedback effect of the grating and further improve the filtering effect of the order Bragg grating on the ridge waveguide.

[0021] The two sides of the gratings on both sides away from the ridge waveguide and between adjacent gratings are filled with benzocyclobutene material to form a filling layer. The thickness of the filling layer is consistent with the thickness of the upper waveguide layer, which is used to optimize the performance of the optical waveguide and improve the efficiency and stability of the optical waveguide.

[0022] SiO is deposited between the grating, the filling layer and the electrode layer. 2 The passivation layer, the SiO 2 A metal contact window is provided on the passivation layer. The width of the metal contact window is the same as that of the ohmic contact layer, and the ohmic contact layer is exposed to complete the ohmic contact with the electrode layer. 2 The structure under the passivation layer is not affected by the external environment, and it can also prevent the intrusion of moisture and other impurities, thereby maintaining the long-term stability and reliability of the laser. At the same time, conductive metal connections are formed on the passivation layer. These metal connections can be used to further connect external circuits to realize the input and output of current, thereby controlling the operation of the laser. This design not only ensures the electrical connection of the laser, but also ensures the high performance and reliability of the laser.

[0023] The present invention also proposes a method for preparing an O-band silicon-based III-V quantum dot narrow linewidth laser, and the technical solution adopted is:

[0024] A method for preparing an O-band silicon-based III-V quantum dot narrow linewidth laser comprises the following steps:

[0025] S1, epitaxially growing a buffer layer, a lower waveguide layer, a lower confinement layer, an InAs quantum dot layer / InGaAs barrier layer, an upper confinement layer, an upper waveguide layer and an ohmic contact layer on a silicon substrate layer in sequence;

[0026] S2, using a photolithography method to form a ridge waveguide and gratings on both sides of the ridge waveguide from the upper waveguide layer and the ohmic contact layer;

[0027] S3, filling benzocyclobutene material on both sides of the gratings away from the ridge waveguide and between adjacent gratings to form a filling layer with the same thickness as the upper waveguide layer;

[0028] S4, depositing SiO on the grating and filling layer 2 passivation layer, and the SiO 2 A metal contact window having the same width as that of the ohmic contact layer is opened on the passivation layer, and the ohmic contact layer is arranged in the metal contact window;

[0029] S5, by electron beam evaporation or magnetron sputtering on SiO 2 An electrode layer is prepared on the passivation layer and the ohmic contact layer to obtain the O-band silicon-based III-V quantum dot narrow linewidth laser.

[0030] Beneficial effects: The preparation method of the O-band silicon-based III-V quantum dot narrow linewidth laser epitaxially grows a buffer layer, a lower waveguide layer, a lower confinement layer, an InAs quantum dot layer / InGaAs barrier layer, an upper confinement layer, an upper waveguide layer, and an ohmic contact layer on a silicon substrate layer to achieve epitaxial growth of III-V quantum dots, and in the structural design of the O-band silicon-based III-V quantum dot narrow linewidth laser, the upper waveguide layer and the ohmic contact layer form a ridge waveguide, and etch gratings on both sides of the ridge waveguide, thereby achieving the preparation of a high-performance O-band silicon-based quantum dot narrow linewidth laser that can be integrated on a single chip, providing an ideal on-chip narrow linewidth light source for future large-scale silicon photonic integrated systems. The O-band silicon-based III-V quantum dot narrow linewidth laser prepared by the present invention has the advantages of narrow linewidth, high reflection tolerance, high temperature stability, low threshold current density, etc., and provides an ideal on-chip light source for future on-chip interconnection systems. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic structural diagram of the laser in Example 1 of the O-band silicon-based III-V quantum dot narrow linewidth laser of the present invention;

[0032] Figure 2 It is a top view schematic diagram of the ridge waveguide and grating in Example 1 of the O-band silicon-based III-V quantum dot narrow linewidth laser of the present invention;

[0033] In the figure, 1, Si (001) substrate layer, 2, n-type buffer layer, 3, n-type AlGaAs waveguide layer, 4, n-type AlGaAs confinement layer, 5, InAs quantum dot layer / InGaAs barrier layer, 6, p-type AlGaAs confinement layer, 7, p-type AlGaAs waveguide layer, 8, p-type GaAs ohmic contact layer, 9, AlGaAs grating layer, 10, SiO 2 Passivation layer, 11. Metal contact layer, 12. Filling layer. DETAILED DESCRIPTION

[0034] As cited in the background technology, it is extremely challenging to prepare a high-performance O-band silicon-based III-V quantum dot narrow linewidth laser that can be integrated on a single chip in the prior art. Therefore, the present invention provides an O-band silicon-based III-V quantum dot narrow linewidth laser, including a silicon substrate layer for growing quantum dots on the silicon substrate layer; a buffer layer, a lower waveguide layer, a lower confinement layer, a quantum dot active layer, an upper confinement layer, an upper waveguide layer, and an ohmic contact layer are sequentially stacked on the silicon substrate layer, wherein the buffer layer is used to effectively prevent the dislocation caused by the lattice mismatch from being transmitted to the quantum dot gain region, ensuring that high-density and high-quality III-V quantum dots can be epitaxially grown; the upper waveguide layer and the ohmic contact layer form a ridge waveguide and a grating on at least one side of the ridge waveguide, which play a role in filtering and narrowing the linewidth; the quantum dot active layer includes an InAs quantum dot layer / InGaAs barrier layer, which is used to improve the optoelectronic performance of the laser, reduce the linewidth, and reduce emission. The O-band silicon-based III-V quantum dot narrow-linewidth laser prepared by the present invention has the advantages of narrow linewidth, high reflection tolerance, high temperature stability, low threshold current density, etc., and provides an ideal on-chip light source for future on-chip interconnection systems.

[0035] Specific embodiment 1 of the O-band silicon-based III-V quantum dot narrow linewidth laser of the present invention:

[0036] In this embodiment, Figure 1 , Figure 2 As shown, an O-band silicon-based III-V quantum dot narrow linewidth laser comprises a silicon substrate layer, on which a buffer layer, a lower waveguide layer, a lower confinement layer, a quantum dot active layer, an upper confinement layer, an upper waveguide layer, an ohmic contact layer and an electrode layer are sequentially stacked, wherein the upper waveguide layer and the ohmic contact layer form a ridge waveguide and a grating on one side of the ridge waveguide; wherein the silicon substrate layer is a Si(001) substrate layer 1; the electrode layer is a metal contact layer 11; the quantum dot active layer is an InAs quantum dot layer / InGaAs barrier layer 5, the number of periods is 2-15, the thickness of the InGaAs barrier layer is 2-20 nm, and the wavelength is an O-band (1260-1360 nm).

[0037] Specifically, the lower waveguide layer is grown on the upper surface of the buffer layer, and the lower waveguide layer is an n-type waveguide layer, and the n-type waveguide layer is Al x GaAs1-x , where 0<x<1, the thickness of the n-type AlGaAs waveguide layer 3 is 30-800nm, and Si is used as a dopant with a doping concentration of ≥0.5×10 18 cm -2 The lower confinement layer is grown on the upper surface of the n-type AlGaAs waveguide layer 3, the lower confinement layer is the n-type confinement layer, and the n-type confinement layer is Al x GaAs 1-x Wherein, 0<x<1, the thickness of the n-type AlGaAs confinement layer 4 is 50-300nm, Si is used as a dopant, and the doping concentration is ≥0.3×10 18 cm -2 The upper confinement layer is grown on the upper surface of the InAs quantum dot layer / InGaAs barrier layer 5, and the upper confinement layer is a p-type confinement layer, and the p-type confinement layer is Al x GaAs 1-x , where 0<x<1, the thickness of the p-type AlGaAs confinement layer 6 is 3-50nm, and Mg is used as a dopant with a doping concentration of ≥1×10 18 cm -2 The upper waveguide layer is grown on the upper surface of the p-type AlGaAs confinement layer 6, and the upper waveguide layer is a p-type waveguide layer, and the p-type waveguide layer is Al x Ga 1-x As, where 0<x<1, the thickness of the p-type AlGaAs waveguide layer 7 is 200-3000nm, and Mg is used as a dopant with a doping concentration of ≥0.5×10 18 cm -2 The ohmic contact layer is grown on the upper surface of the p-type AlGaAs waveguide layer 7, the ohmic contact layer is a p-type ohmic contact layer, the p-type ohmic contact layer is a p-type GaAs ohmic contact layer 8, the thickness of the p-type GaAs ohmic contact layer 8 is 5-50nm, Mg is used as a dopant, and the doping concentration is ≥3×10 19 cm -2 .

[0038] In order to effectively improve the feedback effect of the grating and further improve the filtering effect of the high-order Bragg grating on the ridge waveguide, in this embodiment, Figure 1 and Figure 2As shown, the ridge waveguide and the gratings on both sides of the ridge waveguide are etched by a P-type AlGaAs waveguide layer 7 and a p-type GaAs ohmic contact layer 8; the ridge waveguide is a strip-shaped body located in the middle, and both sides of the ridge waveguide have symmetrical gratings extending along the length direction of the strip-shaped body, forming an AlGaAs grating layer 9. The AlGaAs grating layer 9 is processed so that the height of the grating is consistent with the thickness of the upper waveguide layer, that is, the thickness of the AlGaAs grating layer 9 is consistent with the thickness of the P-type AlGaAs waveguide layer 7. Among them, the width of the ridge waveguide is 1.5-3μm, the width of the single-sided grating is 0.5-3μm, the grating is a first-order grating, the period of the first-order grating is 180-250nm, and the duty cycle is 0.35-0.75; or a high-order grating is selected, that is, the grating can be a third-order grating (the grating period is 3 times the period of the first-order grating); the grating can also be a fifth-order grating (the grating period is 5 times the period of the first-order grating).

[0039] In other embodiments, the silicon substrate layer may be a SOI substrate layer.

[0040] In other embodiments, the ridge waveguide is a strip-shaped body located in the middle, and a grating extending along the length direction of the strip-shaped body is provided on the left side of the ridge waveguide to constitute an AlGaAs grating layer 9; in other embodiments, the ridge waveguide is a strip-shaped body located in the middle, and a grating extending along the length direction of the strip-shaped body is provided on the right side of the ridge waveguide to constitute an AlGaAs grating layer 9.

[0041] In other embodiments, the lower waveguide layer is a p-type waveguide layer, and the p-type waveguide layer is Al x Ga 1-x As, where 0<x<1, the thickness of the p-type AlGaAs waveguide layer is 200-3000nm, and Mg is used as a dopant with a doping concentration ≥0.5×10 18 cm -2 ; The lower limiting layer is a p-type limiting layer, and the p-type limiting layer is Al x GaAs 1-x , where 0<x<1, the thickness of the p-type AlGaAs confinement layer is 3-50nm, Mg is used as the dopant, and the doping concentration is ≥1×10 18 cm -2 ; The upper limiting layer is an n-type limiting layer, and the n-type limiting layer is Al x GaAs 1-x , where 0<x<1, the thickness of the n-type AlGaAs confinement layer is 2-4nm, the thickness is 50-300nm, Si is used as a dopant, and the doping concentration is ≥0.3×10 18 cm -2 ; The upper waveguide layer is an n-type waveguide layer, and the n-type waveguide layer is Al x GaAs 1-x, where 0<x<1, the thickness of the n-type AlGaAs waveguide layer is 30-800nm, and Si is used as a dopant with a doping concentration ≥0.5×10 18 cm -2 .

[0042] Specific embodiment 2 of the O-band silicon-based III-V quantum dot narrow linewidth laser of the present invention:

[0043] Based on the above technical concept of the present invention, or based on the above specific embodiment of the present invention, another embodiment is provided below.

[0044] In this embodiment, the buffer layer is an n-type buffer layer 2, and the n-type buffer layer 2 includes an AlAs nucleation layer, a GaAs buffer layer and an AlGaAs dislocation filter layer from bottom to top, wherein the thickness of the GaAs buffer layer is 0.2-2 μm. The specific implementation process is: epitaxially growing an n-type buffer layer 2 on a Si (001) substrate layer 1, and the n-type buffer layer 2 includes a GaAs buffer layer. The epitaxial growth of the GaAs buffer layer specifically includes: first, growing an AlAs nucleation layer with a thickness of 3-12 nm on the Si (001) substrate layer 1, and then growing a GaAs layer with a thickness of 0.2-2 μm as a buffer layer, and subsequently growing multiple AlGaAs layers as dislocation filter layers. The present application introduces structural layers such as a nucleation layer and a dislocation filter layer in the growth of the buffer layer to prevent the dislocation caused by lattice mismatch from being transferred to the quantum dot gain region, thereby ensuring that high-density and high-quality III-V group quantum dots can be epitaxially grown.

[0045] Specific embodiment 3 of the O-band silicon-based III-V quantum dot narrow linewidth laser of the present invention:

[0046] Based on the above technical concept of the present invention, or based on the above specific embodiment of the present invention, another embodiment is provided below.

[0047] In this embodiment, both sides of the gratings on both sides away from the ridge waveguide and between adjacent gratings are filled with benzocyclobutene material to form a filling layer 12. The lower surface of the filling layer 12 is in contact with the upper surface of the p-type AlGaAs confinement layer 6, so that the thickness of the filling layer 12 is consistent with the thickness of the upper waveguide layer, i.e., the P-type AlGaAs waveguide layer 7, which is used to optimize the performance of the optical waveguide and improve the efficiency and stability of the optical waveguide.

[0048] SiO is deposited between the gratings on both sides of the ridge waveguide and the upper contact surface of the filling layer 12 and the lower contact surface of the metal contact layer 11. 2 Passivation layer 10, SiO 2A metal contact window is provided on the passivation layer 10. The width of the metal contact window is the same as the width of the p-type GaAs ohmic contact layer 9. The p-type GaAs ohmic contact layer 9 is arranged in the metal contact window so that the p-type GaAs ohmic contact layer 9 is exposed, and the metal contact layer 11 is in contact with the p-type GaAs ohmic contact layer 9. The above structure is used to protect SiO 2 The structure below the passivation layer 10 is not affected by the external environment, and can also prevent the intrusion of moisture and other impurities, thereby maintaining the long-term stability and reliability of the laser. At the same time, conductive metal connections are formed on the passivation layer, which can be used to further connect to external circuits to achieve current input and output, thereby controlling the operation of the laser. This design not only ensures the electrical connection of the laser, but also ensures the high performance and reliability of the laser.

[0049] Specific Example 1 of the method for preparing an O-band silicon-based III-V group quantum dot narrow linewidth laser of the present invention:

[0050] The method for preparing an O-band silicon-based III-V group quantum dot narrow linewidth laser comprises the following steps:

[0051] First, a buffer layer, a lower waveguide layer, a lower confinement layer, an InAs quantum dot layer / InGaAs barrier layer, an upper confinement layer, an upper waveguide layer and an ohmic contact layer are epitaxially grown in sequence on a silicon substrate layer;

[0052] Specifically, a buffer layer is first epitaxially grown on a silicon substrate layer, that is, an n-type buffer layer 2 is epitaxially grown on a Si (001) substrate layer 1, wherein the n-type buffer layer 2 includes a GaAs buffer layer, and the epitaxial growth of the GaAs buffer layer specifically includes: first, a 3-12 nm AlAs nucleation layer is grown on the Si (001) substrate layer 1, then a GaAs layer with a thickness of 0.2-2 μm is grown as a buffer layer, and then multiple AlGaAs layers are grown as dislocation filtering layers. Then, an n-type AlGaAs waveguide layer, an n-type AlGaAs restriction layer, an InAs quantum dot layer / InGaAs barrier layer, a p-type AlGaAs restriction layer, a p-type AlGaAs waveguide layer, and a p-type GaAs ohmic contact layer are sequentially grown on the AlGaAs layer; wherein the number of periods of the InAs quantum dot layer / InGaAs barrier layer is 2-15, the thickness of the InGaAs barrier layer is 2-20 nm, and the wavelength is an O band (1260-1360 nm).

[0053] Specifically, the lower waveguide layer is an n-type waveguide layer, and the n-type waveguide layer is Al x GaAs 1-x , where 0<x<1, the thickness of the n-type AlGaAs waveguide layer 3 is 30-800nm, and Si is used as a dopant with a doping concentration of ≥0.5×10 18 cm -2The lower confinement layer is grown on the upper surface of the n-type AlGaAs waveguide layer 3, the lower confinement layer is the n-type confinement layer, and the n-type confinement layer is Al x GaAs 1-x Wherein, 0<x<1, the thickness of the n-type AlGaAs confinement layer 4 is 50-300nm, Si is used as a dopant, and the doping concentration is ≥0.3×10 18 cm -2 The upper confinement layer is grown on the upper surface of the InAs quantum dot layer / InGaAs barrier layer 5, and the upper confinement layer is a p-type confinement layer, and the p-type confinement layer is Al x GaAs 1-x , where 0<x<1, the thickness of the p-type AlGaAs confinement layer 6 is 3-50nm, and Mg is used as a dopant with a doping concentration of ≥1×10 18 cm -2 The upper waveguide layer is grown on the upper surface of the p-type AlGaAs confinement layer 6, and the upper waveguide layer is a p-type waveguide layer, and the p-type waveguide layer is Al x Ga 1-x As, where 0<x<1, the thickness of the p-type AlGaAs waveguide layer 7 is 200-3000nm, and Mg is used as a dopant with a doping concentration of ≥0.5×10 18 cm -2 The ohmic contact layer is grown on the upper surface of the p-type AlGaAs waveguide layer 7, the ohmic contact layer is a p-type ohmic contact layer, the p-type ohmic contact layer is a p-type GaAs ohmic contact layer 8, the thickness of the p-type GaAs ohmic contact layer 8 is 5-50nm, Mg is used as a dopant, and the doping concentration is ≥3×10 19 cm -2 .

[0054] Secondly, the upper waveguide layer and the ohmic contact layer are formed into a ridge waveguide by using a photolithography method, and gratings are etched on both sides of the ridge waveguide;

[0055] Specifically, a photolithography method is adopted to photolithography and etch the p-type AlGaAs waveguide layer 7 and the p-type GaAs ohmic contact layer 8 to form a ridge waveguide and gratings on both sides of the ridge waveguide; the ridge waveguide is a strip-shaped body located in the middle, and the two sides of the ridge waveguide have symmetrical gratings extending along the length direction of the strip-shaped body, forming an AlGaAs grating layer 9, and the AlGaAs grating layer 9 is processed so that the height of the grating is consistent with the thickness of the upper waveguide layer, that is, the thickness of the AlGaAs grating layer 9 is consistent with the thickness of the P-type AlGaAs waveguide layer 7. Among them, the width of the ridge waveguide is 1.5-3μm, the width of the single-side grating is 0.5-3μm, the grating is a first-order grating, the period of the first-order grating is 180-250nm, and the duty cycle is 0.35-0.75; or a high-order grating is selected.

[0056] Next, benzocyclobutene material is filled on both sides of the gratings away from the ridge waveguide and between adjacent gratings to form a filling layer with the same thickness as the upper waveguide layer;

[0057] Specifically, benzocyclobutene material (BCB) is filled on both sides of the gratings away from the ridge waveguide and between adjacent gratings to form a filling layer 12 with the same thickness as the upper waveguide layer. The lower surface of the filling layer 12 is in contact with the upper surface of the p-type AlGaAs confinement layer 6, so that the thickness of the filling layer 12 is consistent with the thickness of the upper waveguide layer, i.e., the P-type AlGaAs waveguide layer 7.

[0058] Then, SiO is deposited on the grating and filling layers. 2 passivation layer, and the SiO 2 A metal contact window having the same width as that of the ohmic contact layer is opened on the passivation layer, and the ohmic contact layer is arranged in the metal contact window;

[0059] Specifically, SiO2 is deposited on the grating and filling layers on both sides of the ridge waveguide. 2 Passivation layer 10, SiO 2 A metal contact window is opened on the passivation layer 10, and the width of the metal contact window is the same as the width of the p-type GaAs ohmic contact layer 8. The p-type GaAs ohmic contact layer 8 is arranged in the metal contact window so that the p-type GaAs ohmic contact layer 8 is exposed, thereby completing the contact between the p-type GaAs ohmic contact layer 8 and the metal contact layer 11.

[0060] Finally, the SiO 2 An electrode layer is prepared on the passivation layer and the ohmic contact layer to obtain the O-band silicon-based III-V quantum dot narrow linewidth laser.

[0061] Specifically, in SiO 2 The metal contact layer 11 is prepared on the passivation layer 10 and the p-type GaAs ohmic contact layer 8 by electron beam evaporation or magnetron sputtering, and ohmic contact is achieved by high temperature annealing, wherein the high temperature annealing temperature is 300-500° C. and the time is 2-10 min.

[0062] Through the above description of the specific embodiment of the O-band silicon-based III-V quantum dot narrow linewidth laser of the present invention, it can be seen that the O-band silicon-based III-V quantum dot narrow linewidth laser of the present invention includes a silicon substrate layer for growing quantum dots on the silicon substrate layer; a buffer layer, a lower waveguide layer, a lower confinement layer, an InAs quantum dot layer / InGaAs barrier layer, an upper confinement layer, an upper waveguide layer and an ohmic contact layer are sequentially stacked on the silicon substrate layer, wherein the buffer layer is used to effectively prevent the dislocation caused by lattice mismatch from being transferred to the quantum dot gain region, thereby ensuring that high-density and high-quality III-V quantum dots can be epitaxially grown; the upper waveguide layer and the ohmic contact layer form a ridge waveguide and a grating on at least one side of the ridge waveguide, which play a role in filtering and narrowing the linewidth; the quantum dot active layer includes an InAs quantum dot layer / InGaAs barrier layer, which is used to improve the optoelectronic performance of the laser, reduce the linewidth, and reduce the reflection. The O-band silicon-based III-V quantum dot narrow linewidth laser of the present invention has the advantages of narrow linewidth, high reflection tolerance, high temperature stability, low threshold current density, etc., and provides an ideal on-chip light source for future on-chip interconnection systems.

[0063] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. The patent protection scope of the present invention shall be based on the claims. All equivalent structural changes made using the contents of the description and drawings of the present invention should also be included in the protection scope of the present invention.

Claims

1. An O-band silicon-based III-V quantum dot narrow linewidth laser, characterized in that: The invention comprises a silicon substrate layer, on which a buffer layer, a lower waveguide layer, a lower confinement layer, a quantum dot active layer, an upper confinement layer, an upper waveguide layer, an ohmic contact layer and an electrode layer are sequentially stacked; the upper waveguide layer and the ohmic contact layer are etched into a ridge waveguide and a grating on at least one side of the ridge waveguide; The quantum dot active layer includes an InAs quantum dot layer / InGaAs barrier layer.

2. The O-band silicon-based III-V quantum dot narrow linewidth laser according to claim 1, characterized in that: The buffer layer comprises an AlAs nucleation layer, a GaAs buffer layer and an AlGaAs dislocation filtering layer in order from bottom to top, and the thickness of the GaAs buffer layer is 0.2-2 μm.

3. The O-band silicon-based III-V quantum dot narrow linewidth laser according to claim 1, characterized in that: The period number of the InAs quantum dot layer / InGaAs barrier layer is 2-15; the thickness of the InGaAs barrier layer is 2-20 nm.

4. The O-band silicon-based III-V quantum dot narrow linewidth laser according to claim 1, characterized in that: The width of the ridge waveguide is 1.5-3 μm, the width of the grating on one side is 0.5-3 μm, the grating is a first-order grating or a high-order grating, the period of the first-order grating is 180-250 nm, and the duty cycle is 0.35-0.

75.

5. The O-band silicon-based III-V quantum dot narrow linewidth laser according to claim 1, characterized in that: The lower waveguide layer is an n-type AlGaAs waveguide layer with a thickness of 30-800nm; the lower confinement layer is an n-type AlGaAs confinement layer with a thickness of 50-300nm; the upper confinement layer is a p-type AlGaAs confinement layer with a thickness of 3-50nm; the upper waveguide layer is a p-type AlGaAs waveguide layer with a thickness of 200-3000nm; and the ohmic contact layer is a p-type GaAs ohmic contact layer with a thickness of 5-50nm.

6. The O-band silicon-based III-V quantum dot narrow linewidth laser according to claim 1, characterized in that: The silicon substrate layer is a Si (001) substrate or a SOI substrate.

7. The O-band silicon-based III-V quantum dot narrow linewidth laser according to claim 4, characterized in that: The ridge waveguide is a strip-shaped body located in the middle, and gratings are symmetrically provided on both sides of the ridge waveguide and extend along the length direction of the strip-shaped body, and the height of the gratings is consistent with the thickness of the upper waveguide layer.

8. The O-band silicon-based III-V quantum dot narrow linewidth laser according to claim 7, characterized in that: Both sides of the gratings on both sides away from the ridge waveguide and between adjacent gratings are filled with benzocyclobutene material to form a filling layer, and the thickness of the filling layer is consistent with the thickness of the upper waveguide layer.

9. The O-band silicon-based III-V quantum dot narrow linewidth laser according to claim 8, characterized in that: A SiO2 passivation layer is deposited between the grating, the filling layer and the electrode layer. A metal contact window is opened on the SiO2 passivation layer. The width of the metal contact window is the same as that of the ohmic contact layer, and the ohmic contact layer is exposed to complete the ohmic contact with the electrode layer.

10. A method for preparing an O-band silicon-based III-V quantum dot narrow linewidth laser, characterized in that: Used for preparing the O-band silicon-based III-V quantum dot narrow linewidth laser as claimed in any one of claims 1 to 9, The following steps are involved: S1, epitaxially growing a buffer layer, a lower waveguide layer, a lower confinement layer, an InAs quantum dot layer / InGaAs barrier layer, an upper confinement layer, an upper waveguide layer and an ohmic contact layer on a silicon substrate layer in sequence; S2, using a photolithography method to form a ridge waveguide from the upper waveguide layer and the ohmic contact layer, and etching gratings on both sides of the ridge waveguide; S3, filling benzocyclobutene material on both sides of the gratings away from the ridge waveguide and between adjacent gratings to form a filling layer with the same thickness as the upper waveguide layer; S4, depositing a SiO2 passivation layer on the grating and the filling layer, and opening a metal contact window on the SiO2 passivation layer with a width equal to that of the ohmic contact layer, wherein the ohmic contact layer is disposed in the metal contact window; S5, preparing an electrode layer on the SiO2 passivation layer and the ohmic contact layer by electron beam evaporation or magnetron sputtering to obtain the O-band silicon-based III-V quantum dot narrow linewidth laser.

Citation Information

Patent Citations

  • Multi-quantum-well semiconductor laser and preparation method thereof

    CN102801108A

  • Short wavelength AlGaInP red light semiconductor laser

    CN105390937A

  • Nano-patterned-substrate lateral-epitaxy silicon-based-quantum-dot laser material and preparation method therefor

    CN106480498A

  • Preparation method of epitaxial material of silicon-based nanometer laser array with electrically-injected long wavelength

    CN108418095A

  • Silicon-based substrate, substrate base plate and manufacturing method thereof, and photoelectric device

    CN111146320A

Cited By

  • Preparation method of addressable silicon-based integrated nano laser and laser

    CN120601247A

  • Quantum dot DFB laser based on substrate buried grating and preparation method

    CN121076580A

  • Semiconductor laser with light field guide layer and preparation method thereof

    CN121602229A