ZnS / SnS solar cell and preparation method thereof
The existing technology is solved by using nano-scale selenized ZnS/SnS composite materials and ZnS/SnS@Ag8SnS6 films in solar cells, combined with FTO/ZnS/SnS@Ag8SnS6/perovskite absorber layer/spiro-oMeTAD/Ag structures in solar cells, and the existing technology is solved. The problem of insufficient performance of solar cells in the middle has achieved efficient electrical and optical performance improvement.
Patent Information
- Application Number
- CN202411148960.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
AI Technical Summary
The electrical and optical properties of existing SnS/ZnS stacked thin-film solar cells have not yet reached the optimal level and need further improvement.
Nano-scale selenized ZnS/SnS composite materials and ZnS/SnS@Ag8SnS6 films are used as electron transport layers, and FTO/ZnS/SnS@Ag8SnS6/perovskite absorbing layer/spiro-oMeTAD/Ag Solar cell structure to improve electron transmission and optical performance.
The solar cell with high electrical and optical performance has been achieved, with an open circuit voltage of 1.22V, a short circuit current density of 34.75mA/cm2, a filling factor of 74.65%, and a conversion efficiency of 31.65%, which significantly improves the overall performance of the solar cell.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar cell preparation, and in particular to a ZnS / SnS solar cell and a preparation method thereof. Background Art
[0002] The band gap of tin sulfide (SnS) is 1.3-1.5 eV, and the visible light absorption coefficient and theoretical photoelectric conversion efficiency are high. Therefore, SnS is an excellent photoelectric material. The band gap of zinc sulfide (ZnS) is about 3.7 eV. It is rich in elements, has a low-cost and non-toxic preparation method. Therefore, ZnS is suitable as a window layer for solar cells.
[0003] Chinese patent CN103928576B discloses a method for preparing SnS / ZnS laminated thin film solar cells, which includes cleaning FTO conductive glass (FTO conductive glass is fluorine-doped SnO2 transparent conductive glass (SnO2:F), referred to as FTO) and turning on the sputtering power supply of the SnS target to prepare SnS thin film; after the SnS thin film is prepared, ZnS thin film is prepared; a total of 2 to 4 PN junctions are prepared; and after preparing Al thin film, SnS / ZnS laminated thin film solar cells are obtained. However, the electrical and optical properties of the solar cells obtained still need to be further improved.
[0004] Based on this, the present invention designs a ZnS / SnS solar cell and a preparation method thereof to solve the above problems. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a ZnS / SnS solar cell and a method for preparing the same.
[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0007] A method for preparing a ZnS / SnS solar cell comprises the following steps:
[0008] 1. Preparation of Nano-scale Selenized ZnS / SnS Composite Materials
[0009] The ZnS, SnS and selenium powder are mixed and packaged in a quartz tube, the quartz tube is placed in an annealing furnace, the temperature is first increased to 180-200° C. at 25-40° C. / min, maintained for 25-40 min, and then increased to 260-280° C. at 15-20° C. / min, maintained for 5-15 min, to selenize the ZnS / SnS, and then cooled to room temperature and ground to nanometer scale to obtain a nanometer-scale selenized ZnS / SnS composite material;
[0010] 2. Preparation of ZnS / SnS@Ag8SnS6
[0011] Take oleylamine solution, silver acetate, SnCl2 and thiourea; add SnCl2, thiourea and silver acetate dropwise to the oleylamine solution in order, stirring while adding; then add nano-selenide ZnS / SnS composite material, heat to 230-238°C and stir to react for 5-10 minutes, and stand for 1-2 hours; finally cool, wash, centrifuge and dry to obtain ZnS / SnS@Ag8SnS6;
[0012] 3. Prepare solar cells with the structure of FTO / ZnS / SnS@Ag8SnS6 / perovskite light absorbing layer / spiro-oMeTAD / Ag.
[0013] Furthermore, the mass ratio of the ZnS, SnS and selenium powder is 1.2-2:1.3-1.5:0.3-0.6.
[0014] Furthermore, the particle size of the nano-scale selenized ZnS / SnS composite material is 40-60 nm.
[0015] Furthermore, 40 ml of oleylamine solution, 8 mmol silver acetate, 1 mmol SnCl2 and 6 mmol thiourea were taken.
[0016] Furthermore, in step 2, after adding SnCl2, the reaction solution is heated to 115-120°C and stirred for reaction for 3-5 minutes, after adding thiourea, the reaction solution is heated to 125-132°C and stirred for reaction for 8-10 minutes, and after adding silver acetate, the reaction solution is heated to 182-225°C and stirred for reaction for 10-15 minutes; then, the nano-selenized ZnS / SnS composite material is added, the temperature is raised to 230-238°C and stirred for reaction for 5-10 minutes.
[0017] Furthermore, step three is as follows:
[0018] FTO conductive glass is cleaned, dried and set aside;
[0019] Preparation of ZnS / SnS@Ag8SnS6 thin film: first, ZnS / SnS@Ag8SnS6 powder is deposited on FTO conductive glass under low sputtering pressure conditions, with a deposition thickness of 80-95nm, and then ZnS / SnS@Ag8SnS6 powder is deposited on FTO conductive glass under high sputtering pressure conditions, with a deposition thickness of 150-200nm; then, annealing is performed at 220-225°C for 3-5min to form a ZnS / SnS@Ag8SnS6 thin film;
[0020] Then, a perovskite light-absorbing layer was prepared on the ZnS / SnS@Ag8SnS6 film;
[0021] Then, spiro-oMeTAD (2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene) was prepared on the perovskite light-absorbing layer to form a hole transport layer;
[0022] Finally, a Ag electrode was prepared on the hole transport layer.
[0023] Furthermore, in step three, the low sputtering gas pressure is 0.5-0.8Pa, and the high sputtering gas pressure is 1.5-2.5Pa.
[0024] Furthermore, in step three, a 100-120 nm thick Ag electrode is formed on the hole transport layer by evaporation.
[0025] In order to better achieve the purpose of the present invention, the present invention also provides a ZnS / SnS solar cell obtained by the above preparation method.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The present invention adopts ZnS / SnS@Ag8SnS6 thin film as an electron transport layer and designs a ZnS / SnS@Ag8SnS6 thin film preparation process to obtain a ZnS / SnS solar cell with high electrical and optical properties. The open circuit voltage (Voc) of the solar cell is 1.22V and the short circuit current density (Jsc) is 34.75mA / cm 2 , the fill factor (FF) is 74.65% and the conversion efficiency PCE is 31.65%. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Embodiment 1
[0030] A method for preparing a ZnS / SnS solar cell comprises the following steps:
[0031] 1. Preparation of Nano-scale Selenized ZnS / SnS Composite Materials
[0032] ZnS, SnS and selenium powder (the mass ratio of ZnS, SnS and selenium powder is 1.2:1.3:0.3) are mixed and packaged in a quartz tube, and the quartz tube is placed in an annealing furnace, first heated to 180°C at 25°C / min, maintained for 25 minutes, and then heated to 260°C at 15°C / min, maintained for 5 minutes to selenize the ZnS / SnS, then cooled to room temperature, and ground to 40 nm to obtain a nano-scale selenized ZnS / SnS composite material;
[0033] 2. Preparation of ZnS / SnS@Ag8SnS6
[0034] Take 40ml of oleylamine solution, 8mmol silver acetate, 1mmol SnCl2 and 6mmol thiourea; add SnCl2, thiourea and silver acetate dropwise to the oleylamine solution in order, stirring while adding; after adding SnCl2, the reaction solution is heated to 115°C and stirred for 3min; after adding thiourea, the reaction solution is heated to 125°C and stirred for 8min; after adding silver acetate, the reaction solution is heated to 182°C and stirred for 10min; then add nano-selenide ZnS / SnS composite material, heat to 230°C and stir for 5min, and let stand for 1h; finally, cool, wash, centrifuge and dry to obtain ZnS / SnS@Ag8SnS6;
[0035] 3. Preparation of solar cells with the structure of FTO / ZnS / SnS@Ag8SnS6 / perovskite light absorbing layer / spiro-oMeTAD / Ag
[0036] FTO conductive glass is cleaned, dried and set aside;
[0037] Preparation of ZnS / SnS@Ag8SnS6 thin film: First, ZnS / SnS@Ag8SnS6 powder was deposited on FTO conductive glass under low sputtering pressure (0.5Pa) with a deposition thickness of 80nm, and then ZnS / SnS@Ag8SnS6 powder was deposited on FTO conductive glass under high sputtering pressure (1.5Pa) with a deposition thickness of 150nm; then annealed at 220℃ for 3min to form ZnS / SnS@Ag8SnS6 thin film;
[0038] Then, a perovskite light-absorbing layer was prepared on the ZnS / SnS@Ag8SnS6 film;
[0039] Then, spiro-oMeTAD is prepared on the perovskite light-absorbing layer to form a hole transport layer;
[0040] Finally, a 100 nm thick Ag electrode was formed on the hole transport layer by evaporation.
[0041] Embodiment 2
[0042] A method for preparing a ZnS / SnS solar cell comprises the following steps:
[0043] 1. Preparation of Nano-scale Selenized ZnS / SnS Composite Materials
[0044] ZnS, SnS and selenium powder (the mass ratio of ZnS, SnS and selenium powder is 2:1.5:0.6) are mixed and encapsulated in a quartz tube, and the quartz tube is placed in an annealing furnace, first heated to 200°C at 40°C / min, maintained for 40 minutes, and then heated to 280°C at 20°C / min, maintained for 15 minutes, to selenize the ZnS / SnS, then cooled to room temperature, and ground to 60nm, to obtain a nano-scale selenized ZnS / SnS composite material;
[0045] 2. Preparation of ZnS / SnS@Ag8SnS6
[0046] Take 40ml of oleylamine solution, 8mmol silver acetate, 1mmol SnCl2 and 6mmol thiourea; add SnCl2, thiourea and silver acetate dropwise to the oleylamine solution in order, stirring while adding; after adding SnCl2, the reaction solution is heated to 120°C and stirred for 5min; after adding thiourea, the reaction solution is heated to 132°C and stirred for 10min; after adding silver acetate, the reaction solution is heated to 225°C and stirred for 15min; then add nano-selenide ZnS / SnS composite material, heat to 238°C and stir for 10min, and let stand for 2h; finally, cool, wash, centrifuge and dry to obtain ZnS / SnS@Ag8SnS6;
[0047] 3. Preparation of solar cells with the structure of FTO / ZnS / SnS@Ag8SnS6 / perovskite light absorbing layer / spiro-oMeTAD / Ag
[0048] FTO conductive glass is cleaned, dried and set aside;
[0049] Preparation of ZnS / SnS@Ag8SnS6 thin film: First, ZnS / SnS@Ag8SnS6 powder was deposited on FTO conductive glass under low sputtering pressure (0.8Pa) with a deposition thickness of 95nm, and then ZnS / SnS@Ag8SnS6 powder was deposited on FTO conductive glass under high sputtering pressure (2.5Pa) with a deposition thickness of 200nm; then annealed at 225℃ for 5min to form ZnS / SnS@Ag8SnS6 thin film;
[0050] Then, a perovskite light-absorbing layer was prepared on the ZnS / SnS@Ag8SnS6 film;
[0051] Then, spiro-oMeTAD is prepared on the perovskite light-absorbing layer to form a hole transport layer;
[0052] Finally, a 120nm thick Ag electrode was formed on the hole transport layer by evaporation.
[0053] Embodiment 3
[0054] A method for preparing a ZnS / SnS solar cell comprises the following steps:
[0055] 1. Preparation of Nano-scale Selenized ZnS / SnS Composite Materials
[0056] ZnS, SnS and selenium powder (the mass ratio of ZnS, SnS and selenium powder is 1.5:1.4:0.5) are mixed and packaged in a quartz tube, and the quartz tube is placed in an annealing furnace, first heated to 191°C at 28°C / min, maintained for 30 minutes, and then heated to 270°C at 17°C / min, maintained for 9 minutes to selenize the ZnS / SnS, then cooled to room temperature, and ground to 50 nm to obtain a nano-scale selenized ZnS / SnS composite material;
[0057] 2. Preparation of ZnS / SnS@Ag8SnS6
[0058] Take 40ml of oleylamine solution, 8mmol silver acetate, 1mmol SnCl2 and 6mmol thiourea; add SnCl2, thiourea and silver acetate dropwise to the oleylamine solution in order, stirring while adding; after adding SnCl2, the reaction solution is heated to 117°C and stirred for 4min; after adding thiourea, the reaction solution is heated to 128°C and stirred for 9min; after adding silver acetate, the reaction solution is heated to 195°C and stirred for 12min; then add nano-selenide ZnS / SnS composite material, heat to 235°C and stir for 7min, and let stand for 1.3h; finally, cool, wash, centrifuge and dry to obtain ZnS / SnS@Ag8SnS6;
[0059] 3. Preparation of solar cells with the structure of FTO / ZnS / SnS@Ag8SnS6 / perovskite light absorbing layer / spiro-oMeTAD / Ag
[0060] FTO conductive glass is cleaned, dried and set aside;
[0061] Preparation of ZnS / SnS@Ag8SnS6 thin film: First, ZnS / SnS@Ag8SnS6 powder was deposited on FTO conductive glass under low sputtering pressure (0.6Pa) with a deposition thickness of 85nm, and then ZnS / SnS@Ag8SnS6 powder was deposited on FTO conductive glass under high sputtering pressure (2Pa) with a deposition thickness of 180nm; then annealed at 223℃ for 4min to form ZnS / SnS@Ag8SnS6 thin film;
[0062] Then, a perovskite light-absorbing layer was prepared on the ZnS / SnS@Ag8SnS6 film;
[0063] Then, spiro-oMeTAD is prepared on the perovskite light-absorbing layer to form a hole transport layer;
[0064] Finally, a 110 nm thick Ag electrode was formed on the hole transport layer by evaporation.
[0065] Detection of solar cell performance: open circuit voltage (Voc) is 1.22V, short circuit current density (Jsc) is 34.75mA / cm 2 , the fill factor (FF) is 74.65% and the conversion efficiency PCE is 31.65%.
[0066] Comparative Example 1
[0067] A method for preparing a ZnS / SnS solar cell comprises the following steps:
[0068] 1. Preparation of Nano-ZnS / SnS Composite Materials
[0069] ZnS and SnS (the mass ratio of ZnS to SnS is 1.5:1.4) are mixed and packaged in a quartz tube, and the quartz tube is placed in an annealing furnace, first heated to 191°C at 28°C / min, maintained for 30 minutes, then heated to 270°C at 17°C / min, maintained for 9 minutes, then cooled to room temperature, and ground to 50 nm to obtain a nano-scale ZnS / SnS composite material;
[0070] 2. Preparation of ZnS / SnS@Ag8SnS6
[0071] Take 40ml of oleylamine solution, 8mmol silver acetate, 1mmol SnCl2 and 6mmol thiourea; add SnCl2, thiourea and silver acetate dropwise to the oleylamine solution in order, stirring while adding; after adding SnCl2, the reaction solution is heated to 117°C and stirred for 4min; after adding thiourea, the reaction solution is heated to 128°C and stirred for 9min; after adding silver acetate, the reaction solution is heated to 195°C and stirred for 12min; then add nano-scale ZnS / SnS composite material, heat to 235°C and stir for 7min, and let stand for 1.3h; finally, cool, wash, centrifuge and dry to obtain ZnS / SnS@Ag8SnS6;
[0072] 3. Preparation of solar cells with the structure of FTO / ZnS / SnS@Ag8SnS6 / perovskite light absorbing layer / spiro-oMeTAD / Ag
[0073] FTO conductive glass is cleaned, dried and set aside;
[0074] Preparation of ZnS / SnS@Ag8SnS6 thin film: First, ZnS / SnS@Ag8SnS6 powder was deposited on FTO conductive glass under low sputtering pressure (0.6Pa) with a deposition thickness of 85nm, and then ZnS / SnS@Ag8SnS6 powder was deposited on FTO conductive glass under high sputtering pressure (2Pa) with a deposition thickness of 180nm; then annealed at 223℃ for 4min to form ZnS / SnS@Ag8SnS6 thin film;
[0075] Then, a perovskite light-absorbing layer was prepared on the ZnS / SnS@Ag8SnS6 film;
[0076] Then, spiro-oMeTAD is prepared on the perovskite light-absorbing layer to form a hole transport layer;
[0077] Finally, a 110 nm thick Ag electrode was formed on the hole transport layer by evaporation.
[0078] Detection of solar cell performance: open circuit voltage (Voc) is 0.96V, short circuit current density (Jsc) is 30.02mA / cm 2 , the fill factor (FF) is 68.35% and the conversion efficiency PCE is 19.70%.
[0079] Comparative Example 2
[0080] A method for preparing a ZnS / SnS solar cell comprises the following steps:
[0081] 1. Preparation of Nano-scale Selenized ZnS / SnS Composite Materials
[0082] ZnS, SnS and selenium powder (the mass ratio of ZnS, SnS and selenium powder is 1.5:1.4:0.5) are mixed and packaged in a quartz tube, and the quartz tube is placed in an annealing furnace, first heated to 191°C at 28°C / min, maintained for 30 minutes, and then heated to 270°C at 17°C / min, maintained for 9 minutes to selenize the ZnS / SnS, then cooled to room temperature, and ground to 50 nm to obtain a nano-scale selenized ZnS / SnS composite material;
[0083] 2. Preparation of ZnS / SnS@Ag8SnS6
[0084] Take 40ml of oleylamine solution, 8mmol of silver acetate, 1mmol of SnCl2 and 6mmol of thiourea; add SnCl2, thiourea and silver acetate to the oleylamine solution in sequence, stir while adding, heat to 195℃ and stir for 25min; then add nano-selenide ZnS / SnS composite material, heat to 235℃ and stir for 7min, let stand for 1.3h; finally cool, wash, centrifuge and dry to obtain ZnS / SnS@Ag8SnS6;
[0085] 3. Preparation of solar cells with the structure of FTO / ZnS / SnS@Ag8SnS6 / perovskite light absorbing layer / spiro-oMeTAD / Ag
[0086] FTO conductive glass is cleaned, dried and set aside;
[0087] Preparation of ZnS / SnS@Ag8SnS6 thin film: First, ZnS / SnS@Ag8SnS6 powder was deposited on FTO conductive glass under low sputtering pressure (0.6Pa) with a deposition thickness of 85nm, and then ZnS / SnS@Ag8SnS6 powder was deposited on FTO conductive glass under high sputtering pressure (2Pa) with a deposition thickness of 180nm; then annealed at 223℃ for 4min to form ZnS / SnS@Ag8SnS6 thin film;
[0088] Then, a perovskite light-absorbing layer was prepared on the ZnS / SnS@Ag8SnS6 film;
[0089] Then, spiro-oMeTAD is prepared on the perovskite light-absorbing layer to form a hole transport layer;
[0090] Finally, a 110 nm thick Ag electrode was formed on the hole transport layer by evaporation.
[0091] Detection of solar cell performance: open circuit voltage (Voc) is 1.03V, short circuit current density (Jsc) is 29.32mA / cm 2, the fill factor (FF) is 61.30% and the conversion efficiency PCE is 18.51%.
[0092] Comparative Example 3
[0093] A method for preparing a ZnS / SnS solar cell comprises the following steps:
[0094] 1. Preparation of Nano-scale Selenized ZnS / SnS Composite Materials
[0095] ZnS, SnS and selenium powder (the mass ratio of ZnS, SnS and selenium powder is 1.5:1.4:0.5) are mixed and packaged in a quartz tube, and the quartz tube is placed in an annealing furnace, first heated to 191°C at 28°C / min, maintained for 30 minutes, and then heated to 270°C at 17°C / min, maintained for 9 minutes to selenize the ZnS / SnS, then cooled to room temperature, and ground to 50 nm to obtain a nano-scale selenized ZnS / SnS composite material;
[0096] 2. Preparation of ZnS / SnS@Ag8SnS6
[0097] Take 40ml of oleylamine solution, 8mmol silver acetate, 1mmol SnCl2 and 6mmol thiourea; add SnCl2, thiourea and silver acetate dropwise to the oleylamine solution in order, stirring while adding; after adding SnCl2, the reaction solution is heated to 117°C and stirred for 4min; after adding thiourea, the reaction solution is heated to 128°C and stirred for 9min; after adding silver acetate, the reaction solution is heated to 195°C and stirred for 12min; then add nano-selenide ZnS / SnS composite material, heat to 235°C and stir for 7min, and let stand for 1.3h; finally, cool, wash, centrifuge and dry to obtain ZnS / SnS@Ag8SnS6;
[0098] 3. Preparation of solar cells with the structure of FTO / ZnS / SnS@Ag8SnS6 / perovskite light absorbing layer / spiro-oMeTAD / Ag
[0099] FTO conductive glass is cleaned, dried and set aside;
[0100] Preparation of ZnS / SnS@Ag8SnS6 thin film: ZnS / SnS@Ag8SnS6 powder was deposited on FTO conductive glass at 1.5Pa with a deposition thickness of 265nm; then annealed at 223℃ for 4min to form a ZnS / SnS@Ag8SnS6 thin film;
[0101] Then, a perovskite light-absorbing layer was prepared on the ZnS / SnS@Ag8SnS6 film;
[0102] Then, spiro-oMeTAD is prepared on the perovskite light-absorbing layer to form a hole transport layer;
[0103] Finally, a 110 nm thick Ag electrode was formed on the hole transport layer by evaporation.
[0104] Detection of solar cell performance: open circuit voltage (Voc) is 0.91V, short circuit current density (Jsc) is 21.28mA / cm 2 , the fill factor (FF) is 69.47% and the conversion efficiency PCE is 13.45%.
[0105] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a ZnS / SnS solar cell, It is characterized in that The following steps are involved:
1. Preparation of Nano-scale Selenized ZnS / SnS Composite Materials The ZnS, SnS and selenium powder are mixed and packaged in a quartz tube, the quartz tube is placed in an annealing furnace, the temperature is first increased to 180-200° C. at 25-40° C. / min, maintained for 25-40 min, and then increased to 260-280° C. at 15-20° C. / min, maintained for 5-15 min, to selenize the ZnS / SnS, and then cooled to room temperature and ground to nanometer scale to obtain a nanometer-scale selenized ZnS / SnS composite material; 2. ZnS / SnS@Ag 8 S N 6 Preparation Take oleylamine solution, silver acetate, SnCl 2 and thiourea; SnCl 2 , thiourea, and silver acetate are sequentially added dropwise to the oleylamine solution while stirring; then the nano-selenized ZnS / SnS composite material is added, the temperature is raised to 230-238°C, stirred for reaction for 5-10 minutes, and allowed to stand for 1-2 hours; finally, the ZnS / SnS@Ag is obtained after cooling, washing, centrifugation, and drying. 8 S N 6 ; 3. Preparation structure is FTO / ZnS / SnS@Ag 8 S N 6 / perovskite absorber / spiro-oMeTAD / Ag solar cells.
2. The ZnS / SnS solar cell according to claim 1, It is characterized in that The mass ratio of the ZnS, SnS and selenium powder is 1.2-2:1.3-1.5:0.3-0.
6.
3. The ZnS / SnS solar cell according to claim 2, It is characterized in that The particle size of the nano-scale selenized ZnS / SnS composite material is 40-60 nm.
4. The ZnS / SnS solar cell according to claim 3, It is characterized in that Take 40ml of oleylamine solution, 8mmol silver acetate, 1mmol SnCl 2 and 6mmol thiourea.
5. The ZnS / SnS solar cell according to claim 4, It is characterized in that In step 2, add SnCl 2 The reaction solution is heated to 115-120° C. and stirred for reaction for 3-5 minutes. After thiourea is added, the reaction solution is heated to 125-132° C. and stirred for reaction for 8-10 minutes. After silver acetate is added, the reaction solution is heated to 182-225° C. and stirred for reaction for 10-15 minutes. Then, the nano-selenized ZnS / SnS composite material is added, the temperature is raised to 230-238° C. and stirred for reaction for 5-10 minutes.
6. The ZnS / SnS solar cell according to claim 5, It is characterized in that Step three is as follows: FTO conductive glass is cleaned, dried and set aside; ZnS / SnS@Ag 8 S N 6 Thin film preparation: ZnS / SnS@Ag was firstly prepared under low sputtering pressure. 8 S N 6 The powder is deposited on FTO conductive glass with a thickness of 80-95 nm, and then ZnS / SnS@Ag is deposited under high sputtering pressure. 8 S N 6 The powder is deposited on FTO conductive glass with a deposition thickness of 150-200 nm; then annealed at 220-225°C for 3-5 min to form ZnS / SnS@Ag 8 S N 6 film; Then in ZnS / SnS@Ag 8 S N 6 Preparing a perovskite light-absorbing layer on the film; Then, spiro-oMeTAD is prepared on the perovskite light-absorbing layer to form a hole transport layer; Finally, a Ag electrode was prepared on the hole transport layer.
7. The ZnS / SnS solar cell according to claim 6, It is characterized in that In step three, the low sputtering gas pressure is 0.5-0.8 Pa, and the high sputtering gas pressure is 1.5-2.5 Pa.
8. The ZnS / SnS solar cell according to claim 7, It is characterized in that In step three, a 100-120 nm thick Ag electrode is formed on the hole transport layer by evaporation.
9. A ZnS / SnS solar cell prepared according to the method of claim 8.