Fluid management layer for absorbent article and absorbent article containing same

By using a combination of non-swelling wicking, elastic and hardened fibers in the fluid management layer of disposable absorbent products, the fiber structure is optimized, and the trade-off between collection speed and back seepage is solved, achieving rapid collection and reduction back seepage The effect of the absorbent product improves the performance and comfort.

CN119053310APending Publication Date: 2024-11-29PROCTER & GAMBLE CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280095176.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-04-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

There is a trade-off between the acquisition speed and back seepage of existing disposable absorbent products. The faster the acquisition speed, the more back seepage tends to increase, and when the absorbed fiber is exposed to liquid, it may cause the pore size to shrink and block the fluid management layer, affecting the Collection time and back seepage.

Method used

Using a combination of non-swelling wicking fibers, elastomer and hardened fibers, determined by material composition and fiber specificity, including 10% to 60% non-swelling wicking fibers, 15% to 70% elastomer and 25% to 70% % hardened fibers and optimize the fiber structure by radius relative shape factor and line density to form a fluid management layer with high capillary force.

Benefits of technology

The balance of rapid fluid acquisition and reduced return seepage is achieved, providing comfortable absorption performance and protection, while avoiding channel blockage caused by absorbing fiber swelling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053310A_ABST
    Figure CN119053310A_ABST
Patent Text Reader

Abstract

The present invention relates to a nonwoven sheet, as determined by material composition analysis, about 10% to about 60% of non-swellable wicking fibers, about 15% to about 70% of elastic fibers, and about 25% to about 70% of hardened fibers by weight of the fluid nonwoven, and wherein the non-swellable wicking fibers, the elastic fibers, and the hardened fibers, as determined by a radius-to-form factor test, are non-swellable and non-swellable wicking fibers, as determined by a radius-to-form factor test. The non-swellable wicking fiber has a radius relative form factor in the range of from about 25% to about 100%, and the non-swellable wicking fiber has a linear density of from 0.8 dtex to 3.3 dtex as determined by a fiber dtex test; the present invention relates to a non-woven sheet, and to an absorbent article comprising a liquid permeable topsheet, a liquid impermeable backsheet, an absorbent core disposed between the topsheet and the backsheet, and a fluid management layer disposed between the topsheet and the absorbent core, the fluid management layer comprising the non-woven sheet disclosed herein.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates generally to fluid management layers for disposable absorbent articles and, in particular, to fluid management layers that are nonwovens having improved performance properties. Background Art

[0002] Disposable absorbent articles such as feminine hygiene products, taped diapers, pant diapers, and incontinence products are designed to absorb fluids from the wearer's body. Users of such disposable absorbent articles have several concerns. Leakage of products such as catamenial pads, diapers, sanitary towels, and incontinence pads is an important concern. The comfort of the product and the wearer's body's feeling of the product are also a concern. In order to provide better comfort, current disposable absorbent articles are typically provided with a top sheet that is flexible, feels soft, and is non-irritating to the wearer's skin.

[0003] With regard to comfort, some consumers may desire a product that has sufficient thickness and stiffness to provide a desired amount of protection, while also being flexible.Bulky materials can be used to provide a cushiony feeling to the article.

[0004] Disposable absorbent articles are generally designed to include a liquid-permeable top sheet, a liquid-impermeable back sheet, and an absorbent core disposed between the top sheet and the back sheet. In order to avoid preventing liquid from being transferred from the top sheet to the absorbent core and to minimize the amount of body fluid retained on the top sheet, absorbent articles have been designed by introducing a fluid management layer between the top sheet and the absorbent core. One desired function of the fluid management layer is to quickly collect liquid or other body exudates and transfer them to the absorbent core in an effective manner. Another desired function is to reduce the amount of fluid in the top sheet to avoid a wet feeling. In order to reduce the amount of liquid in the top sheet, the fluid management layer is required to have good wicking properties to distribute the liquid along the planar direction of the fluid management layer, thereby reducing the liquid concentration at the loading point, and to have high capillary forces to draw liquid from the top sheet. Small pore sizes in the planar direction or z-direction contribute to both wicking properties and capillary forces. Although the small-sized holes in the fluid management layer enhance the wicking properties and capillary forces, they also bring high flow resistance to liquid penetrating the fluid management layer, which results in a slow acquisition speed. Therefore, there is usually a trade-off between acquisition speed and re-infiltration. That is, the faster the acquisition speed, the higher the re-infiltration tends to increase, and vice versa.

[0005] US2020 / 0315872A discloses a fluid management layer comprising 10 to 60 wt% absorbent fibers, 15 to 70 wt% elastic fibers, and 25 to 70 wt% stiffening fibers. However, when exposed to liquid, the absorbent fibers tend to swell, which may result in smaller pore sizes and block some channels in the fluid management layer, and ultimately have a negative impact on acquisition time and / or rewet.

[0006] Therefore, there is a need to create absorbent articles with improved fluid acquisition and rewet.

[0007] Therefore, there is a need to create an absorbent article that takes into account possible trade-offs so that it is both comfortable and maintains performance. Summary of the invention

[0008] The present invention relates to a nonwoven sheet, as determined by material composition analysis, comprising from about 10% to about 60% non-swelling wicking fibers by weight of the fluid management layer, from about 15% to about 70% elastic fibers by weight of the fluid management layer, and from about 25% to about 70% stiffening fibers by weight of the fluid management layer, and wherein the non-swelling wicking fibers have a radius relative shape factor in the range of from about 25% to about 100% as determined by a radius relative shape factor test, and the non-swelling wicking fibers have a linear density of 0.8 dtex to 3.3 dtex as determined by a fiber dtex test.

[0009] The present invention relates to a nonwoven sheet, as determined by material composition analysis, comprising at least about 10% to about 60% non-swelling wicking fibers by weight of a fluid management layer, and about 15% to about 70% elastic fibers and about 25% to about 70% stiffening fibers by weight of the fluid management layer, and wherein the non-swelling wicking fibers have a radius relative shape factor in the range of about 25% to about 100% as determined by a radius relative shape factor test, and the non-swelling wicking fibers have a linear density of 0.8 dtex to 3.3 dtex as determined by a fiber dtex test.

[0010] The present invention also relates to an absorbent article, which includes a liquid-permeable top sheet, a liquid-impermeable back sheet, an absorbent core arranged between the top sheet and the back sheet, and a fluid management layer arranged between the top sheet and the absorbent core, the liquid management layer including a nonwoven fabric, wherein as determined by material composition analysis, the nonwoven fabric includes about 10% to about 60% of non-swelling wicking fibers by weight of the fluid management layer, about 15% to about 70% of elastic fibers by weight of the fluid management layer, and about 25% to about 70% of stiffening fibers by weight of the fluid management layer, and wherein as determined by a radius relative shape factor test, the non-swelling wicking fibers have a radius relative shape factor in the range of about 25% to about 100%, and as determined by a fiber dtex test, the non-swelling wicking fibers have a linear density of 0.8 dtex to 3.3 dtex.

[0011] The present invention also relates to an absorbent article, which includes a liquid-permeable top sheet, a liquid-impermeable back sheet, an absorbent core arranged between the top sheet and the back sheet, and a fluid management layer arranged between the top sheet and the absorbent core, the liquid management layer including a nonwoven fabric, wherein as determined by material composition analysis, the nonwoven fabric includes about 10% to about 60% of non-swelling wicking fibers by weight of the fluid management layer, and about 15% to about 70% of elastic fibers and about 25% to about 70% of stiffening fibers by weight of the fluid management layer, and wherein as determined by a radius relative shape factor test, the non-swelling wicking fibers have a radius relative shape factor in the range of about 25% to about 100%, and as determined by a fiber dtex test, the non-swelling wicking fibers have a linear density of 0.8 dtex to 3.3 dtex.

[0012] For ease of discussion, absorbent articles will be discussed with reference to the reference numerals mentioned in these drawings. However, unless otherwise expressly indicated, the drawings and detailed description should not be considered to limit the scope of the claims, and the invention disclosed herein is also applicable to various absorbent article forms. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In the accompanying drawings, similar reference numerals or other designations in all views denote similar components. Some of these figures may have been simplified by omitting selected elements in order to more clearly show other elements. The accompanying drawings are not drawn to scale.

[0014] Figure 1 is a schematic diagram of a front view of a fluid management layer according to the present invention.

[0015] Figure 2 is a schematic diagram of a process that can be used to construct a fluid management layer according to the present invention.

[0016] Figure 3Ais a schematic diagram of a disposable absorbent article according to the present invention.

[0017] Figure 3B yes Figure 3A A schematic diagram of the absorbent system of a disposable absorbent article is shown.

[0018] Figure 4 is a SEM image showing a cross section of a fluid management layer according to the present invention.

[0019] Figure 5 is a SEM image showing a cross section of a fluid management layer according to the present invention

[0020] Figure 6 is a schematic diagram of a fiber to illustrate the measurement results of the radius of the fiber relative to the shape factor.

[0021] Fig. 7A is a perspective view of the strikethrough plate used for acquisition time measurements.

[0022] Figure 7B yes Fig. 7A A plan view of a vapor permeable panel.

[0023] Figure 7C yes Figure 7B A plan view of the cross section of the breathable plate taken along the 7C-7C direction.

[0024] Fig.7D yes Figure 7B A plan view of a portion of a breathable panel.

[0025] Fig. 7E yes Figure 7B A plan view of the cross section of the breathable plate in the 7E-7E direction. DETAILED DESCRIPTION

[0026] As used herein, the following terms shall have the meanings specified below:

[0027] "Absorbent article" refers to a wearable device that absorbs and contains liquids, and more specifically, refers to a device that is placed close to or adjacent to the wearer's body to absorb and contain the various exudates discharged from the body. Absorbent articles may include diapers, training pants, adult incontinence underwear (e.g., liners, pads, and briefs) and / or feminine hygiene products.

[0028] As used herein, the term "integrated" is used to describe fibers of a nonwoven material that have been interwoven, entangled, and / or pushed / pulled in the positive and / or negative Z direction (thickness direction of the nonwoven material). Some exemplary methods for integrating fibers of a nonwoven web include hydroentanglement and needle punching. Hydroentanglement uses multiple high-pressure water jets to entangle fibers. Needle punching involves using needles to push and / or pull fibers to entangle them with other fibers in the nonwoven.

[0029] As used herein, the term "combed" is used to describe the structural features of the fluid management layer described herein. Nonwovens utilize fibers that are cut into specific lengths, which are otherwise referred to as "short length fibers." Short length fibers can be any suitable length. For example, short length fibers can have a length of up to 120 mm or can have a length as short as 10 mm. However, if a particular group of fibers is short length fibers (e.g., viscose fibers), the length of each of the viscose fibers in the nonwoven is primarily the same, i.e., short length. It is noteworthy that in the case of including additional short fiber length fiber types such as polypropylene fibers, the length of each of the polypropylene fibers in the nonwoven is also primarily the same.

[0030] In contrast, continuous filaments, such as by a spunbond process or a meltblown process, do not produce short length fibers. Instead, these filaments have an indefinite length and are not cut into specific lengths as described for their staple length counterparts.

[0031] The "longitudinal" direction is a direction extending parallel to the largest linear dimension of the article (generally the longitudinal axis), and includes directions within 45° of the longitudinal direction. As used herein, the "length" of an article or component thereof generally refers to the size / distance of the largest linear dimension, or generally refers to the size / distance of the longitudinal axis of the article or component thereof.

[0032] The "lateral" or "transverse" direction is orthogonal to the longitudinal direction, i.e., in the same principal plane of the article and the longitudinal axis, and transversely parallel to the transverse axis. As used herein, the "width" of an article or part thereof refers to the size / distance of the dimension orthogonal to the longitudinal direction of the article or part thereof, i.e., orthogonal to the length of the article or part thereof, and typically it refers to the distance / size of the dimension parallel to the transverse axis of the article or part.

[0033] The "Z-direction" is orthogonal to both the longitudinal and lateral directions.

[0034] As used herein, "machine direction" or "MD" refers to the direction parallel to the flow of a nonwoven through a nonwoven making machine and / or absorbent article product manufacturing equipment.

[0035] As used herein, "cross direction" or "CD" refers to the direction parallel to the width of a nonwoven making machine and / or absorbent article product manufacturing equipment and perpendicular to the machine direction.

[0036] The nonwoven sheets as disclosed herein can be used in a variety of disposable absorbent articles, but are particularly useful in diapers, feminine hygiene products, and incontinence products such as sanitary napkins and incontinence pads. The nonwovens of the present disclosure can be particularly effectively used as fluid management layers in the above-mentioned absorbent articles. In addition, the nonwovens of the present disclosure provide increased thickness even at lower basis weights and have good fluid handling properties in both acquisition speed and rewet mitigation.

[0037] The fluid management layer of the present disclosure may be disposed between the topsheet and the absorbent core.

[0038] The fluid management layer of the present disclosure may include one or more nonwoven webs or nonwoven layers (hereinafter collectively referred to as "nonwoven webs"). The one or more nonwoven webs may be carded nonwoven webs.

[0039] The fiber of nonwoven web can be integrated.The fiber of nonwoven web can be thermally bonded.When utilizing at least two nonwoven webs, the fiber in each of at least two webs can be integrated.When utilizing at least two nonwoven webs, the fiber of at least two webs can be integrated.Alternatively, at least two nonwoven webs can be attached to each other by, for example, thermal bonding, adhesive bonding or a combination thereof.In one embodiment, the fiber of nonwoven of the present invention is integrated.In one embodiment, nonwoven of the present invention is spunlace.

[0040] A variety of configurations of fluid management layers can be achieved. However, it is important that the fluid management layer of the present disclosure has sufficient openness to allow rapid acquisition of fluids, and is also able to lock in liquid insults to reduce the possibility of re-seepage even in the event of repeated liquid insults. Accordingly, the nonwoven webs that make up the fluid management layer can be different from each other. For example, one of the nonwoven webs may include a fiber blend that is different from the other nonwoven webs. In one embodiment, assuming that the first nonwoven web will be closest to the wearer-facing surface in the absorbent article, the fiber selection for the first nonwoven web may allow for a greater openness associated with this web. The second nonwoven web may be similarly constructed, or may be constructed to collect liquid insults from the void spaces of the first nonwoven web and effectively distribute these liquid insults to the absorbent core. In another embodiment, the first nonwoven web may allow for a greater openness associated with this web. The second nonwoven web may be similarly constructed. In contrast, the third nonwoven web can be configured to collect liquid insults from the interstitial spaces of the first and second nonwoven webs and effectively distribute these liquid insults to the absorbent core. Alternatively, the first and second nonwoven webs can be configured to be identical.

[0041] In the case where the fiber composition of one nonwoven web is different from the fiber composition of another nonwoven web, the nonwoven is a heterogeneous configuration. Alternatively, the case where the nonwoven webs have the same fiber composition is referred to as a uniform configuration.

[0042] When the nonwoven webs are integrated, they cannot be separated manually - at least not without expending a great deal of effort and time. Each nonwoven web forms a layer within the overall fluid management layer. Each layer can retain the unique properties of at least a portion of that layer in the z-direction even when integrated into a larger fluid management layer. The fluid management layer can provide capillary suction to "pull" fluid through the topsheet, which counteracts drip / low flow conditions. The fluid management layer can also contain surges to efficiently utilize the absorbent core by providing a distribution function, and provide intermediate storage until the absorbent core can accept fluid.

[0043] As previously noted, absorbent articles according to the present disclosure exhibit soft cushioning texture and fluid handling properties. The absorbent articles of the present disclosure may also have good elasticity. It is noteworthy that the typical thickness of the fiber web from a conventional spunlace line achieves a thickness factor (thickness / 10 gsm basis weight) of 0.03 to 0.12. In contrast, the fluid management layer of the present disclosure may exhibit a thickness factor of at least 0.13 mm, or at least about 0.15 mm, or at least 0.2 mm, including any values ​​within these ranges and any ranges established thereby. The fluid management layer of the present disclosure may have a thickness factor between 0.13 mm and about 0.3 mm, or about 0.14 mm to about 0.25 mm, or about 0.15 mm to about 0.22 mm, including all values ​​within these ranges and any ranges established thereby. The thickness and thickness factor of the fluid management layer of the present disclosure can be determined by the Thickness and Thickness Factor Test Methods disclosed herein.

[0044] Whether the fluid management layer is used in adult incontinence products, catamenial products, liners, or other hygiene products, it is critical that the fluid management layer is able to acquire liquid insults from the topsheet and pull the liquid far enough away from the topsheet so that the topsheet is not perceived to be wet. To achieve this, the increased thickness factor of the fluid management layer described herein can promote fluid acquisition due to the increased void volume of the fluid management layer. Higher thickness at lower basis weight equals greater void volume with higher permeability. In addition, the increased thickness of the fluid management layer can also provide stain masking benefits. That is, stains visible through the topsheet of absorbent articles using the fluid management layer of the present disclosure appear much smaller than their conventional fluid management layer counterparts.

[0045] The fluid management layer of the present disclosure may have a basis weight of up to 120 grams per square meter (gsm), up to 100 gsm; or between about 20 gms to about 120 gsm; or between about 30 gsm to about 100 gsm, or between about 45 gsm to about 80 gsm, and or between about 50 gsm to about 65 gsm, including any values ​​within these ranges and any ranges created therefrom. Some absorbent articles may not require as much basis weight as described above. For example, a liner that does not typically have the same level of absorbent capacity as a sanitary napkin may be able to have a basis weight that exceeds the basis weight reduction described above. For example, the fluid management layer may have a basis weight of between 20 gsm and 70 gsm, or between 35 gsm to about 65 gsm, or about 30 gsm to about 55 gsm, specifically including all values ​​within these ranges and any ranges created therefrom.

[0046] In one embodiment, the fluid management layer is hydroentangled, i.e., produced via a conventional hydroentanglement process widely known in the industry. In this case, it is also worth noting that the fluid management layer may not require an adhesive or latex binder to maintain stability due to fiber integration. In addition, the nonwoven of the fluid management layer can be made from a wide variety of suitable fiber types that produce desired performance characteristics.

[0047] As will be discussed in further detail below, the fiber types in the fluid management layer of the present disclosure are described according to their function within the fluid management layer. For example, due to the high radius relative form factor, non-swelling wicking fibers are used to distribute liquid through channels in the surface of the fiber. The non-swelling wicking fibers do not absorb liquid and do not swell when exposed to liquid, so that the fluid management layer can maintain channels and pores when fluid invades and ultimately can maintain fluid acquisition speed. Reinforcing fibers are used to bond together through heat treatment, thereby providing stiffness and resiliency to the fluid management layer. Elastic fibers are used to provide recovery from compressive forces acting on the fluid management layer. Optional absorbent fibers can be used to absorb liquid insults.

[0048] In order to enhance the stabilizing effect of integration, crimped fibers may be used. One or more of the non-swelling wicking fibers, the stiffening fibers, and the elastic fibers may be crimped prior to integration. For example, in the case of synthetic fibers, these fibers may be mechanically crimped by intermeshing teeth.

[0049] The fluid management layer of the present disclosure includes non-swelling wicking fibers in the range of about 10 wt % to about 60 wt %, or about 15 wt % to about 50 wt %, or about 20 wt % to about 40 wt %, specifically including all values ​​within these ranges and any ranges formed therefrom.

[0050] Additionally, the fluid management layer also includes a sufficient weight percentage of elastic fibers that affect the recovery of the absorbent article from compressive loads experienced during use. The fluid management layer of the present disclosure includes elastic fibers in the following ranges: from about 15 wt % to about 70 wt %, or from about 20 wt % to about 60 wt %, or from about 25 wt % to about 50 wt %, specifically including all values ​​within these ranges and any ranges formed therefrom.

[0051] In addition, reinforcing fibers can be used to help the fluid management layer of the present disclosure provide resiliency to the absorbent article. For example, as described below, the reinforcing fibers can be bonded to each other during production by heat treating the fluid management layer. This bonding of the reinforcing fibers forms a support matrix that contributes to the resiliency and stiffness of the fluid management layer. Accordingly, the fluid management layer includes stiffening fibers in the range of about 25% to about 70% by weight, or about 30% to about 60% by weight, or about 40% to about 55% by weight, specifically including all values ​​within these ranges and any ranges formed therefrom.

[0052] In the case of targeting thickness, elasticity and soft cushion feel, the weight percentage of reinforcing fibers can be greater than or equal to the weight percentage of elastic fibers. The weight percentages of non-swelling wicking fibers, elastic fibers and stiffening fibers can be determined according to product design objectives.

[0053] The ratio of non-swelling wicking fibers to stiffening fibers in the fluid management layer of the present disclosure can be from about 1:7 to about 2:1, or from about 1:4 to about 1.5:1, or from about 1:2 to about 1:1, specifically including all values ​​within these ranges and any ranges formed therefrom. Similarly, the ratio of non-swelling wicking fibers to elastic fibers can be from about 1:7 to about 3:1, or from about 1:2 to about 2:1, or from about 1:1.5 to about 1:1, specifically including all values ​​within these ranges and any ranges formed therefrom.

[0054] Accordingly, the inventors have also surprisingly discovered that careful selection of fiber types and linear densities of fiber types in the fluid management layer can achieve the desired results of rapid acquisition and mitigated rewet even in the case of repeated fluid insults. The fiber types of the fluid management layer and the individual layers when the fluid management layer includes at least one layer are discussed in more detail below. It is worth noting that the discussion below about fiber types in the layers of the fluid management layer assumes that when the fluid management layer has more than one nonwoven web, the first nonwoven web is closer to the top sheet than the additional carded web.

[0055] The non-swelling wicking fibers can help distribute the fluid, especially in the XY direction perpendicular to the z direction. The non-swelling wicking fibers do not absorb liquids and do not swell when exposed to liquids, so that the fluid management layer can maintain channels and holes when the fluid invades and ultimately maintain the fluid acquisition speed. The non-swelling wicking fibers can be any suitable synthetic thermoplastic fibers having a linear density in the range of about 0.8 dtex to about 3.3 dtex, such as monocomponent fibers containing polypropylene ("PP"), polyethylene terephthalate ("PET"), polybutylene terephthalate ("PBT"), and bicomponent fibers containing polyolefin resins, as well as other suitable thermoplastic fibers known in the art. Some suitable linear density values ​​for the non-swelling wicking fibers used in the fluid management layer of the present disclosure can range from about 0.8 dtex to about 3.3 dtex, or from about 1.2 dtex to about 2.5 dtex, or from about 1.5 dtex to about 2 dtex, specifically including all values ​​within these ranges and any ranges formed thereby. The decitex (dtex) value of the non-swelling wicking fibers, stiffening fibers, and / or elastic fibers can be determined via the Fiber Decitex method disclosed herein.

[0056] As determined by the Radius Relative Shape Factor Test disclosed herein, the non-swelling wicking fibers for fluid management layers have a high radius relative shape factor ("RSFR") in the range of about 25% to about 100%, or in the range of about 25% to about 80%, or in the range of about 30% to about 80%. Fibers with high RSFR values ​​are considered to have deep channels along the fibers, so that the nonwoven containing the fibers can have high wicking capabilities. At this point, the upper limit of RSFR may not be critical. Fibers with too low RSFR values ​​are not suitable as non-good wicking fibers because such fibers have swallowing channels along the fibers, so that the nonwoven containing the fibers may not have the desired level of wicking capabilities. Some examples of non-swelling wicking fibers may have cross-sections such as cross-shaped, trilobal, pentagonal, "H"-shaped, "Y"-shaped, "X"-shaped, "T"-shaped, or flat ribbons. Each layer may include non-swelling wicking fibers with a different percentage by weight than the layer weight.

[0057] As previously noted, the fluid management layer of the present disclosure also includes stiffening fibers in addition to non-swelling wicking fibers. Reinforcing fibers may be utilized to help provide structural integrity to the fluid management layer. Reinforcing fibers may help improve the structural integrity of the fluid management layer in the longitudinal and / or transverse directions, which facilitates web manipulation during handling of the fluid management layer for incorporation into disposable absorbent articles.

[0058] Some suitable linear density values ​​of reinforcing fibers are provided. For example, the stiffening fiber linear density may be in the range of about 1.0 dtex to about 6 dtex, or about 1.5 dtex to about 5 dtex, or about 2.0 dtex to about 4 dtex, specifically including all values ​​within these ranges and any ranges formed therefrom.

[0059] Some examples of suitable hardening fibers include bicomponent fibers comprising polyolefins. In some embodiments, bicomponent fibers suitable for hardening fibers may include polyethylene and polyethylene terephthalate components or polyethylene terephthalate and copolyethylene terephthalate components. The components of the bicomponent fibers may be arranged in a core-sheath structure, a side-by-side structure, an eccentric core-sheath structure, a trilobal structure, etc. In a specific example, the hardening fiber may include a bicomponent fiber arranged in a concentric core-sheath structure having a polyethylene / polyethylene terephthalate component, wherein the polyethylene is the sheath.

[0060] Although other materials may be useful, the stiffness of polyethylene terephthalate can be used to form an elastic structure. In contrast, the polyethylene component of the reinforcing fiber can be used to bond to each other during heat treatment. This can help provide tensile strength to the web in MD and CD. In addition, the bonding of the polyethylene component to other polyethylene components of the reinforcing fiber can also produce fixed points in the nonwoven. These fixed points can reduce the amount of sliding between fibers, thereby increasing the elasticity of the material.

[0061] One of the benefits of reinforcing fibers is that the integrated nonwoven can be heat treated after fiber entanglement. Heat treatment can provide additional structural integrity to the integrated nonwoven by forming bonds between adjacent reinforcing fibers. Therefore, with a higher percentage of stiffening fibers, more connection points can be formed. Too many connection points can produce a much stiffer fluid management layer, which can have an adverse effect on comfort. Therefore, when designing absorbent articles, the weight percentage of reinforcing fibers is critical.

[0062] With respect to the thermal hardening process, any suitable temperature may be utilized. Moreover, the suitable temperature may be affected in part by the constituent chemistry of the reinforcing fibers and by the treatment of the fluid management layer web. For example, the fluid management layer web may be thermally strengthened at a temperature of 132 degrees Celsius. However, it should also be noted that in order to provide uniform stiffness properties throughout the fluid management layer, any heating operation should be configured to provide uniform heating to the fluid management layer web. Even small temperature variations may significantly affect the tensile strength of the fluid management layer.

[0063] The fluid management layer of the present disclosure also includes elastic fibers. The elastic fibers can help the fluid management layer maintain its permeability and compression recovery. Any suitable size of fiber can be used. For example, the elastic fiber can have a linear density of about 6 dtex to about 15 dtex, or about 7 dtex to about 12 dtex, or about 7 dtex to about 10 dtex, especially when the elastic fiber is a multi-component fiber such as a bicomponent fiber. The elastic fiber can have a linear density of about 4 dtex to about 15 dtex, or about 7 dtex to about 12 dtex, or about 7 dtex to about 10 dtex, especially when the elastic fiber is a single-component fiber such as PP, PET and PBT. Fibers with a small lining density may not provide the desired elasticity to the nonwoven. In another specific example, the fluid management layer may include elastic fibers with variable cross-sections such as circular and hollow spirals, and / or may include elastic fibers with variable dtex. In such a form, the elastic fiber may be hollow spiral.

[0064] The elastic fiber can be any suitable thermoplastic fiber, such as polypropylene (PP), polyethylene terephthalate or other suitable thermoplastic fibers known in the art. The length of the elastic fiber can range from about 20 mm to about 100 mm, or from about 30 mm to about 50 mm, or from about 35 mm to about 45 mm. The thermoplastic fiber can have any suitable structure or shape. For example, the thermoplastic fiber can be circular or have other shapes, such as spiral, oval with notch, trilobal, ribbon with notch, etc. In addition, the PP fiber can also be solid, hollow or hollow at multiple locations. The elastic fiber can be solid and circular in shape. Other suitable examples of elastic fibers include polyester / coextruded polyester fibers. In addition, other suitable examples of elastic fibers include bicomponent fibers, such as polyethylene / polypropylene, polyethylene / polyethylene terephthalate, polypropylene / polyethylene terephthalate. These bicomponent fibers can be constructed as skin and core. Bicomponent fibers can provide a cost-effective way to increase the basis weight of a material while additionally being able to optimize pore size distribution.

[0065] The elastic fiber may be polyethylene terephthalate (PET) fiber or other suitable non-cellulose fibers known in the art. The PET fiber may have any suitable structure or shape. For example, the PET fiber may be round or have other shapes, such as spiral, notched elliptical, trilobal, notched ribbon, hollow spiral, etc. In addition, the PET fiber may also be solid, hollow or hollow in multiple places. In a specific example, the fiber may be a fiber made of hollow / spiral PET. Optionally, the elastic fiber may be spiral pleated or flat pleated. The elastic fiber may have a pleat value of about 4 to about 12 pleats / inch (cpi), or about 4 to about 8cpi, or about 5 to about 7cpi, or about 9 to about 10cpi. Specific non-limiting examples of elastic fibers can be obtained from Wellman, Inc., Ireland under the trade names H1311 and T5974. Other examples of elastic fibers suitable for use in the carded staple fiber nonwovens described in detail herein are disclosed in US Patent 7,767,598 to Schneider et al.

[0066] It is worth noting that the reinforcing fibers and elastic fibers should be carefully selected. For example, although the constituent chemical compositions of the reinforcing fibers and the elastic fibers may be similar, the elastic fibers should be selected such that the melting temperature of their constituent materials is higher than the melting temperature of the reinforcing fibers. Otherwise, during heat treatment, the elastic fibers will bond to the reinforcing fibers, and vice versa, and an overly rigid structure may result.

[0067] Without being bound by theory, when the fluid management layer includes absorbent fibers, it is believed that for weight percentages of absorbent fibers above about 30%, within the gsm range disclosed herein, elastic fibers and / or stiffening fibers should be carefully selected. In the case of a soft, cushion-textured fluid management layer having a thickness factor of at least 0.13 or greater as described herein, resilient and / or reinforcing fibers may be selected to offset the loss of structural integrity of the absorbent fibers when wetted. For example, higher dtex elastic fibers may be beneficial in offsetting the loss of integrity experienced by the absorbent fibers. In such cases, elastic fibers having a dtex between about 5 dtex and about 15 dtex, or about 6 dtex to about 12 dtex, or about 7 dtex to about 10 dtex may be utilized.

[0068] Additionally or alternatively, the reinforcing fibers may be configured to provide greater structural integrity. For example, the reinforcing fibers may include bicomponent fibers in a core-sheath configuration, wherein the sheath is copolyethylene terephthalate. However, with such changes in materials, additional problems may occur. For example, the joining of the material to the fluid management layer may thus be joined only by an adhesive, rather than via fusion bonding.

[0069] Wherein the absorbent fiber accounts for 30 weight % or more. In such a case, the linear density of the stiffening fiber can be about 3 dtex to about 6 dtex, or about 4 dtex to about 6 dtex.

[0070] The fluid management layer of the present disclosure may also include absorbent fibers. The absorbent fibers may provide absorption of liquid insults from the wearer-facing surface or the topsheet. However, as the absorbent fibers absorb liquid, they tend to lose some of their structural integrity. The loss of structural integrity may reduce the resiliency of the absorbent article and lead to increased bunching and increased leakage. Thus, while in principle a large percentage of absorbent fibers may work well to quickly drain liquid insults from the wearer-facing surface and / or the topsheet, a large percentage will lead to other problems with absorbent articles as previously described.

[0071] In view of potential problems associated with having too many weight percentages of absorbent fibers, the fluid management layer of the present disclosure may include absorbent fibers in the following ranges: from about 1 weight % to about 40 weight %, or from about 5 weight % to about 35 weight %, or from about 1 weight % to about 20 weight %, specifically including any values ​​within these ranges and any ranges created therefrom.

[0072] The absorbent fibers of the fluid management layer can have any suitable shape. Some examples include trilobal, "H", "Y", "X", "T", circular, or flat ribbons. In addition, the absorbent fibers can be solid, hollow, or hollow in multiple places.

[0073] Any suitable absorbent material for absorbent fibers may be utilized. Some examples of absorbent materials include cotton, pulp, rayon, or regenerated cellulose, or combinations thereof. In one example, the fluid management layer may include viscose cellulose fibers. The length of the absorbent fibers may be in the range of about 20 mm to about 100 mm, or about 30 mm to about 50 mm, or about 35 mm to about 45 mm, specifically including all values ​​within these ranges and any ranges formed therefrom. Generally speaking, pulp fibers have a fiber length of about 4 mm to 6 mm, and are too short to be used in conventional carding machines. Therefore, if pulp is desired as a fiber in the fluid management layer, additional processing may be required to add the pulp to the nonwoven web. For example, pulp may be air-laid between nonwoven webs, and the combination may then be integrated. As another example, tissue paper may be used in combination with a nonwoven web, and the combination may then be integrated.

[0074] Figure 1A schematic diagram of an exemplary fluid management layer according to the present disclosure is provided in FIG. As shown, the fluid management layer 30 includes a first surface 300A, an opposite second surface 300B, and opposite end edges 32A and 32B. Between the first surface 300A and the second surface 300B, the fluid distribution layer 30 includes at least one layer or at least two or more layers along the Z direction.

[0075] An exemplary method for forming the fluid management layer of the present disclosure is shown in Figure 2 As shown, a plurality of carding machines 210, 220, and 230 may each produce a nonwoven web, such as 214, 224, and 234, that is transferred to a conveyor belt 240. Each of the nonwoven webs 214, 224, and 234 may be provided to the conveyor belt 240 via web chutes 212, 222, and 232, respectively. It is also worth noting that after the nonwoven 214 is deposited on the conveyor belt 240, the nonwoven 224 is then deposited on the first nonwoven 214 on the conveyor belt 240. Similarly, the third nonwoven web 234 is deposited on the second nonwoven 224 and the first nonwoven 214 on the conveyor belt 240. Subsequently, each of the first nonwoven web 214, the second nonwoven web 224, and the third nonwoven web 234 is then provided to an integration process 250, which utilizes needles and / or high pressure water jets to entangle the fibers of the first nonwoven web, the second nonwoven web, and the third nonwoven web. Both the carding and integration processes are well known in the art.

[0076] Additional carding machines may be utilized. In addition, the fluid management layer of the present disclosure may be prepared using only two of the three carded nonwoven webs. In such cases, the first nonwoven web 214 will be deposited on the conveyor belt 240. And subsequently, the second nonwoven web 224 will be deposited on the first nonwoven web 214. The first nonwoven web 214 and the second nonwoven web 224 will then be integrated as described herein.

[0077] It is worth noting that using Figure 2The arrangement provided in the schematic diagram of can realize a variety of configurations for the fluid management layer. However, it is important that the fluid management layer of the present disclosure has sufficient openness to allow rapid acquisition of fluid, but can also lock liquid invaders to reduce the possibility of back seepage. Accordingly, the nonwoven fiber webs, namely 214, 224 and / or 234, can be different from each other. For example, one of the nonwoven fiber webs may include a fiber blend different from the other nonwoven fiber webs. Specifically, assuming that the first nonwoven fiber web will be closest to the wearer-facing surface in the absorbent article, the fiber selection for the first nonwoven fiber web 214 can be such that there is a greater openness associated with this fiber web. The second nonwoven fiber web 224 can be similarly constructed. In contrast, the third nonwoven fiber web 234 can be configured to collect liquid invaders from the void spaces of the first nonwoven fiber web 214 and the second nonwoven fiber web 224, and effectively distribute these liquid invaders to the absorbent core. Alternatively, the first nonwoven web 214, the second nonwoven web 224, and the third nonwoven web 234 can be constructed identically.

[0078] The fluid management systems of the present disclosure may be incorporated into a variety of absorbent articles.

[0079] Absorbent products

[0080] An exemplary schematic diagram showing an absorbent article of the present disclosure, namely a feminine hygiene pad, is shown in Figure 3A As shown, an absorbent article 10 according to the present disclosure includes a top sheet 20, a back sheet 50, and an absorbent core 40 disposed between the top sheet 20 and the back sheet 50. A fluid management layer 30 is disposed between the top sheet 20 and the absorbent core 40. The absorbent article has a wearer-facing surface 60 and an opposite garment-facing surface 62. The wearer-facing surface 60 primarily includes the top sheet 20, while the garment-facing surface 62 primarily includes the back sheet 50. Additional components may be included in the wearer-facing surface 60 and / or the garment-facing surface 62. For example, if the absorbent article is an incontinence pad, a pair of barrier cuffs extending generally parallel to the longitudinal axis L of the absorbent article 10 may also form a portion of the wearer-facing surface 60. Similarly, a fastening adhesive may be present on the back sheet 50 and form a portion of the garment-facing surface 62 of the absorbent article.

[0081] An exemplary configuration of the fluid management layer of the present disclosure is shown in Figure 3BAs shown, the fluid management layer 30 includes opposite end edges 32A and 32B that may extend generally parallel to the transverse axis T. Furthermore, the fluid management layer 30 includes side edges 31A and 32B that may extend generally parallel to the longitudinal axis L. Similarly, the absorbent core 40 includes opposite end edges 42A and 42B that may extend generally parallel to the transverse axis T. Furthermore, the absorbent core 40 may include side edges 41A and 41B that extend generally parallel to the longitudinal axis L.

[0082] As shown, each of the end edges 32A and 32B of the fluid management layer 30 can be disposed longitudinally outside the absorbent core 40. However, this need not be the case. For example, the end edges 32A and / or 32B can be coextensive with the absorbent core 40, or the end edges 32A and / or 32B can be disposed longitudinally inside the end edges 42A and / or 42B of the absorbent core 40.

[0083] Similarly, the side edges 31A and / or 31B can be disposed laterally outboard of the side edges 41A and 41B of the absorbent core 40. Alternatively, the side edges 31A and / or 31B can be coextensive with the side edges 41A and / or 41B of the absorbent core 40. In addition, the end edges and / or side edges of the absorbent core and / or the fluid management layer can be curvilinear in nature. For example, the side edges of the absorbent core and / or the fluid management layer can curve inwardly from the ends toward the transverse axis. Such configurations can contribute to the conformability of the absorbent article. Similarly, the end edges, in conjunction with or independent of the side edges of the absorbent core and / or the fluid management layer, can include a curvilinear path that is generally concave or generally convex.

[0084] See also Figure 3A and Figure 3B , the top sheet 20 may be joined to the back sheet 50 by attachment methods (not shown) such as those known in the art. The top sheet 20 and the back sheet 50 may be directly joined to each other in the periphery of the article, and may be indirectly joined together by directly joining them to the absorbent core 40, the fluid management layer 30, and / or additional layers disposed between the top sheet 20 and the back sheet 50. Such indirect or direct joining may be achieved by attachment methods well known in the art.

[0085] The top sheet 20 can be compliant, soft-feeling, and non-irritating to the wearer's skin. Suitable top sheet materials include liquid-permeable materials that are oriented toward and contact the wearer's body, allowing body exudates to quickly penetrate without allowing fluid to flow back through the top sheet onto the wearer's skin. Although the top sheet allows fluid to pass through it and transfer quickly, it also allows the lotion composition to transfer or migrate to the outside or inside of the wearer's skin.

[0086] A suitable top sheet 20 can be made of a variety of materials, such as woven and nonwoven materials; apertured film materials, including apertured formed thermoplastic films, apertured plastic films, and fiber-wound apertured films; hydraulically formed thermoplastic films; porous foams; reticulated foams; reticulated thermoplastic films; thermoplastic scrims; or combinations thereof.

[0087] Apertured film materials suitable for use as the topsheet include those apertured plastic films which are impervious to body exudates and which allow body exudates to pass therethrough while minimizing or preventing the return of fluids which pass through the topsheet.

[0088] Non-limiting examples of woven materials and non-woven materials suitable for use as top sheets include fibrous materials made of natural fibers (e.g., cotton, including 100% organic cotton), modified natural fibers, synthetic fibers, or combinations thereof. These fibrous materials can be hydrophilic or hydrophobic, but preferably, the top sheet is hydrophobic or presents as hydrophobic. As an option, some parts of the top sheet can be treated to be hydrophilic by using any known method for preparing a top sheet containing a hydrophilic component. Nonwoven fiber top sheet 20 can be produced by any known method for making nonwoven webs, and non-limiting examples of such methods include spunbond, carding, wet-laid, air-laid, melt-blown, needle-punched, mechanical entanglement, thermo-mechanical entanglement, and water entanglement.

[0089] Top sheet 20 can be formed by the combination of apertured film and nonwoven. For example, the film web and nonwoven web can be combined as described in U.S. Patent 9,700,463. Alternatively, the film can be extruded onto the nonwoven material, which is believed to provide enhanced contact between the film layer and the nonwoven material.

[0090] The backsheet 50 can be positioned adjacent to the garment-facing surface of the absorbent core 40 and can be joined thereto by attachment methods such as those known in the art. For example, the backsheet 50 can be secured to the absorbent core 40 by a uniform continuous adhesive layer, a patterned adhesive layer, or a series of separate adhesive lines, spirals, or spots. Alternatively, the attachment method can include the use of heat bonding, pressure bonding, ultrasonic bonding, dynamic mechanical bonding, or any other suitable attachment method or combination of these attachment methods as known in the art.

[0091] Backsheet 50 can be impermeable or substantially impermeable to liquid (e.g., urine), and can be made of thin plastic film, but other flexible liquid-impermeable materials can also be used. As used herein, term "flexible" refers to compliant and easily conformable to the general shape and contour of human body. Backsheet 50 can prevent or at least suppress the effluent absorbed by absorbent core 40 and contained from wetting the clothing products (such as underwear) contacted with absorbent article 10. However, backsheet 50 can allow steam to escape (i.e., breathable) from absorbent core 40, and in some cases, backsheet 50 can not allow steam to escape (i.e., impermeable). Therefore, backsheet 50 can include polymer film, such as thermoplastic film of polyethylene or polypropylene. Suitable material for backsheet 50 is thermoplastic film with a thickness of, for example, about 0.012mm (0.5mil) to about 0.051mm (2.0mil). Any suitable backsheet as known in the art can be used for the present invention.

[0092] Suitable breathable backsheets for use herein include all breathable backsheets known in the art. There are mainly two types of breathable backsheets: single layer breathable backsheets that are breathable and liquid impermeable, and backsheets with at least two layers that provide a combination of breathability and liquid impermeability.

[0093] The absorbent core 40 of the present disclosure may include any suitable shape, including but not limited to oval, oblong (discorectangle), rectangle, asymmetric shape and hourglass shape. For example, in some forms of the present invention, the absorbent core 40 may have a profile shape, such as being narrower than the end region in the middle region. For example, the absorbent core may have a tapered shape, having a wider portion at one end region of the pad, tapering to a narrower end region at the other end region of the pad. The absorbent core 40 may include a varying stiffness in the longitudinal and transverse directions.

[0094] The configuration and construction of the absorbent core 40 can vary (e.g., the absorbent core 40 can have varying thickness zones, hydrophilic gradients, superabsorbent gradients, or lower average density and lower average basis weight acquisition zones). In addition, the size and absorptive capacity of the absorbent core 40 can also vary to accommodate a variety of wearers. However, the total absorptive capacity of the absorbent core 40 should be consistent with the design load and intended use of the disposable absorbent article 10.

[0095] In some forms of the present invention, absorbent core 40 may include multiple multifunctional layers except the first laminate and the second laminate. For example, absorbent core 40 may include a core wrap (not shown), which may be used to encapsulate the first laminate and the second laminate and other optional layers. The core wrap may be formed by two nonwoven materials, substrates, laminates, films or other materials. In one form, the core wrap may only include a single material, substrate, laminate or other materials wrapped around itself at least in part.

[0096] The absorbent core 40 of the present disclosure may include one or more adhesives, for example, to help secure the SAP or other absorbent material within the first and second laminates.

[0097] Absorbent cores with various core designs containing relatively high levels of SAP are disclosed in U.S. Pat. No. 5,599,335 to Goldman et al., EP 1,447,066 to Busam et al., WO 95 / 11652 to Tanzer et al., U.S. Pat. Publication 2008 / 0312622A1 to Hundorf et al., and WO 2012 / 052172 to Van Malderen. These can be used to construct superabsorbent layers. The absorbent core includes a storage layer that may contain conventional absorbent materials. In addition to conventional absorbent materials such as crepe cellulose fillers, fluff cellulose fibers, rayon fibers, wood pulp fibers also known as air felt, and textile fibers, the storage layer often includes superabsorbent polymer materials that absorb fluid and form hydrogels. Such materials are also referred to as absorbent gelling materials (hereinafter referred to as AGMs), and may be included in granular form. AGMs are generally capable of absorbing large amounts of body fluids and retaining these body fluids under moderate pressure. Synthetic fibers may also be used in the second storage layer, including cellulose acetate, polyvinyl fluoride, polyvinylidene chloride, acrylic resins (such as Orlon), polyvinyl acetate, insoluble polyvinyl alcohol, polyethylene, polypropylene, polyamides (such as nylon), polyester, bicomponent fibers, tricomponent fibers, mixtures thereof, etc. The storage layer may also include filler materials such as perlite, diatomaceous earth, vermiculite, or other suitable materials that reduce rewet problems.

[0098] The storage layer may have the AGM in a uniform distribution or may have the AGM in a non-uniform distribution. The AGM may be in the form of channels, pockets, stripes, crisscross patterns, swirls, dots, or any other pattern (two-dimensional or three-dimensional) that one can imagine. The AGM may be sandwiched between a pair of fibrous cover layers. Or the AGM may be at least partially encapsulated by a single fibrous cover layer.

[0099] Portions of the storage layer may be formed solely of AGM, or may be formed of AGM dispersed in a suitable carrier such as cellulose fibers in the form of fluff or reinforced fibers. One example of a non-limiting storage layer is a first layer formed solely of superabsorbent material, the first layer being disposed on a second layer formed of superabsorbent material dispersed in cellulose fibers.

[0100] The absorbent article 10 may further include barrier cuffs.

[0101] Test Method

[0102] 1. Nonwoven Sample Preparation

[0103] If the nonwoven exists in its raw material form, a sample of about 25 mm × 25 mm or larger size is cut from the raw material to include at least one complete protruding first area and a portion of two adjacent second areas. If the nonwoven is a component layer of an absorbent article such as a second top sheet, the absorbent article of this size is cut and a razor blade is used to cut the nonwoven layer from the layer below the absorbent article, thereby removing the nonwoven layer from the absorbent article. If necessary, a low temperature spray (such as Cyto-Freeze, Control Company, Houston TX) or other suitable solvent that does not permanently change the properties of the nonwoven layer composition can be used to remove the nonwoven layer sample from the layer below. Tetrahydrofuran (THF) can be used as a solvent to remove any residual adhesive from the sample by the following steps.

[0104] 1) In a fume hood, transfer 1 L of THF to a 3 L - 4 L beaker.

[0105] 2) Immerse the sample in 1 liter of THF.

[0106] 3) Place the beaker on a shaker and gently stir for 15 minutes, and let the solution with the added sample stand for another 5 minutes.

[0107] 4) Take the sample out of the THF solution and carefully squeeze the THF solution out of the sample.

[0108] 5) Allow the samples to air dry in a fume hood for a minimum of 15 minutes.

[0109] To obtain a nonwoven cross-section sample, the nonwoven is placed on a flat work surface (with the first side facing up) and cut to expose a cross-section of the sample.

[0110] 2. Thickness and thickness factor

[0111] 2.1 Thickness

[0112] The thickness of the specimen is measured as the distance between the reference platform on which the specimen rests and the pressure foot that applies a specified amount of pressure to the specimen for a specified amount of time. All measurements are made in a laboratory maintained at 23°C ± 2°C and 50% ± 2% relative humidity, and the specimens are conditioned in this environment for at least 2 hours prior to testing.

[0113] Thickness is measured with a manually operated micrometer equipped with a pressure foot capable of applying a steady pressure of 0.50 kPa ± 0.01 kPa to the specimen. The manually operated micrometer is a deadweight instrument with readings accurate to 0.01 mm. A suitable instrument is a Mitutoyo series 543ID-C Digimatic, or equivalent, available from VWR International. The pressure foot is a flat circular movable surface with a diameter smaller than the specimen and capable of applying the required pressure. A suitable pressure foot has a diameter of 25.4 mm, but smaller or larger pressure feet may be used depending on the size of the specimen being measured. The specimen is supported by a horizontal, flat reference platform that is larger than and parallel to the surface of the pressure foot. The system is calibrated and operated in accordance with the manufacturer's instructions.

[0114] If necessary, obtain the sample by removing it from the absorbent article. When cutting the sample from the absorbent article, be careful not to cause any contamination or deformation to the sample layer during the process. The sample is taken from an area without folds or wrinkles and must be larger than the pressure foot.

[0115] To measure thickness, first zero the micrometer relative to a horizontal flat reference platform. Place the specimen on the platform with the test position centered under the pressure foot. Gently lower the pressure foot at a rate of descent of 3.0mm ± 1.0mm per second until full pressure is applied to the specimen. Wait 5 seconds, then record the thickness of the specimen to the nearest 0.001mm. Repeat in a similar manner for a total of ten replicate test specimens. Calculate the arithmetic mean of all thickness measurements and report as "Thickness" to the nearest 0.001mm.

[0116] 2.2 Thickness coefficient

[0117] As previously stated the thickness factor is the thickness per 10 gsm of sample basis weight. Therefore, the formula is thickness / (basis weight / 10).

[0118] At least 10 replicates of the sample are tested and the average (arithmetic mean) of the at least 10 replicates is reported as the thickness factor.

[0119] 3. Basis weight

[0120] The basis weight of the test sample is the mass (in grams) per unit area (in square meters) of a single material layer and is measured according to the pharmacopoeia method WSP 130.1. The mass of the test sample is cut into a known area and the mass of the test sample is determined using an analytical balance accurate to 0.0001 grams. All measurements are carried out in a laboratory maintained at 23°C ± 2°C and 50% ± 2% relative humidity, and the test samples are conditioned in this environment for at least 2 hours before testing.

[0121] The test sample taken from the raw material roll or raw material sheet or the test sample obtained from the material layer removed from the absorbent article is measured. When the material layer is cut out from the absorbent article, it is noted that no contamination or deformation is caused to the layer during the process. The cut layer should not contain residual adhesive. In order to ensure that all adhesives are removed, the layer is soaked in a suitable solvent that will dissolve the adhesive and will not adversely affect the material itself. One such solvent is THF (tetrahydrofuran, CAS109-99-9, which is used for general purposes and is purchased from any convenient source). After the solvent is soaked, the material layer is allowed to be thoroughly air-dried in a manner that prevents excessive stretching or other deformation of the material. After the material has dried, the sample is obtained. The sample must be as large as possible to take into account any inherent material variability.

[0122] Measure the dimensions of the single layer specimen using a calibrated steel metal ruler from NIST or equivalent. Calculate the area of ​​the specimen and record it to the nearest 0.0001 square centimeter. Use an analytical balance to obtain the mass of the specimen and record it to the nearest 0.0001 gram. Calculate the basis weight by dividing the mass (in grams) by the area (in square meters) and record it to the nearest 0.01 grams per square meter (gsm). Repeat in a similar manner for a total of ten replicates. Calculate the arithmetic mean of the basis weight and report it to the nearest 0.01 grams per square meter.

[0123] 4. Material composition analysis

[0124] The quantitative chemical composition of the specimens comprising a mixture of fiber types was determined using ISO 1833-1. All tests were performed in a laboratory maintained at 23°C ± 2°C and 50% ± 2% relative humidity.

[0125] The test sample taken from the raw material roll or raw material sheet or the test sample obtained from the material layer removed from the absorbent article is analyzed. When the material layer is cut out from the absorbent article, it is noted that no contamination or deformation is caused to the layer during the process. The cut layer should not contain residual adhesive. In order to ensure that all adhesives are removed, the layer is immersed in a suitable solvent that will dissolve the adhesive and will not adversely affect the material itself. A kind of such solvent is THF (tetrahydrofuran, CAS109-99-9, which is used for general purposes and is purchased from any convenient source). After the solvent is soaked, the material layer is allowed to be thoroughly air-dried in a manner to prevent excessive stretching or other deformation of the material. After the material has dried, the sample is obtained and tested according to ISO 1833-1 to quantitatively determine its chemical composition.

[0126] 5. Fiber decitex (Dtex)

[0127] Textile webs (e.g., woven webs, nonwoven webs, air-laid webs) are composed of individual fibers of a material. The fibers are measured in the form of linear mass density, which is reported in decitex. The decitex value is the mass of the fibers present in 10,000 meters of the fiber (in grams). The decitex value of the fibers in the web of the material is often reported by the manufacturer as part of the specification. If the decitex value of the fiber is unknown, it can be calculated by measuring the cross-sectional area of ​​the fiber via a suitable microscopic technique such as a scanning electron microscope (SEM), determining the composition of the fiber with a suitable technique such as FT-IR (Fourier transform infrared) spectroscopy and / or DSC (dynamic scanning calorimetry), and then calculating the mass of the fibers present in 10,000 meters of fiber using the literature value of the density of the composition (in grams). All tests were conducted in a room maintained at a temperature of 23°C ± 2.0°C and a relative humidity of 50% ± 2%, and the samples were conditioned for at least 2 hours under the same environmental conditions before testing.

[0128] If desired, a representative sample of the web material of interest can be cut out from the absorbent article. In this case, the web material is removed in order to prevent the sample from being stretched, deformed or contaminated.

[0129] SEM images were obtained and analyzed as follows to determine the cross-sectional area of ​​the fibers. In order to analyze the cross-section of a sample of a fiber web material, a specimen was prepared as follows. A sample of about 1.5 cm (height) × 2.5 cm (length) and without creases or wrinkles was cut from the fiber web. The sample was immersed in liquid nitrogen and the edge was broken along the length of the sample with a razor blade (No. 9 VWR single-edged industrial razor blade, surgical carbon steel). The sample was sputter-coated with gold and then adhered to the SEM mount using double-sided conductive tape (Cu, 3M, purchased from electron microscopy sciences). The sample was oriented so that the cross section was as perpendicular to the detector as possible to minimize any tilt distortion of the measured cross section. SEM images were obtained at a resolution sufficient to clearly illustrate the cross section of the fibers present in the sample. The fiber cross section may vary in shape, and some fibers may be composed of multiple individual filaments. In any case, the area of ​​each cross section in the fiber cross section is determined (e.g., using the diameter of a circular fiber, the major and minor axes of an elliptical fiber, and image analysis for more complex shapes). If the fiber cross section indicates a non-uniform cross-sectional composition, the area of ​​each identifiable component is recorded and the decitex contribution of each component is calculated and then summed. For example, if the fiber is bicomponent, the cross-sectional areas of the core and sheath are measured separately and the decitex contributions from the core and sheath are calculated separately and summed. If the fiber is hollow, the cross-sectional area does not include the interior portion of the fiber composed of air, which does not contribute significantly to the fiber decitex. In general, at least 100 such measurements of the cross-sectional area are made for each fiber type present in the sample and are reported in square micrometers (μm 2 ) is used as the unit to record the cross-sectional area a of each fiber k The arithmetic mean (accurate to 0.1 μm) 2 ).

[0130] The fiber composition is determined using common characterization techniques such as FTIR spectroscopy. For more complex fiber compositions (such as polypropylene core / polyethylene sheath bicomponent fibers), a combination of common techniques (e.g., FTIR spectroscopy and DSC) may be required to fully characterize the fiber composition. This process is repeated for each fiber type present in the web material.

[0131] Decitex of each fiber type in the web material k The value is calculated as follows:

[0132] d k =10 000m×a k ×ρ k ×10 -6

[0133] where d kIn grams (per 10,000 m of calculated length), a k In μm 2 is a unit, and ρ k In grams per cubic centimeter (g / cm 3 Report the decitex to the nearest 0.1 g per 10,000 m of calculated length and the fiber type (e.g., PP, PET, cellulose, PP / PET bicomponent).

[0134] 6. Preparation of artificial menstrual fluid (AMF)

[0135] Artificial menstrual fluid (AMF) consists of a mixture of defibrillated sheep blood, phosphate buffered saline solution and a mucus component. AMF is prepared so that it has a viscosity between 7.15 and 8.65 centistokes at 23°C.

[0136] The viscosity of AMF is measured using a low viscosity rotational viscometer (a suitable instrument is a Cannon LV-2020 rotational viscometer with a UL adapter from Cannon Instrument Co., State College, PA, or an equivalent instrument). A spindle of appropriate size within the viscosity range is selected, and the instrument is operated and calibrated according to the manufacturer. The measurements are performed at 23°C ± 1°C and at 60rpm. Results are reported to the nearest 0.01 centistoke.

[0137] The reagents required for AMF preparation include: defibrinated sheep blood with a packed cell volume of 38% or greater (collected under sterile conditions and purchased from Cleveland Scientific, Inc., Bath, OH, or equivalent), gastric mucin with a viscosity target of 3-4 centistokes when prepared as a 2% aqueous solution (crude form, purchased from Sterilized American Laboratories, Inc., Omaha, NE, or equivalent), 10% v / v lactic acid in water, 10% w / v potassium hydroxide in water, anhydrous disodium hydrogen phosphate (reagent grade), sodium chloride (reagent grade), sodium dihydrogen phosphate monohydrate (reagent grade), and distilled water, each purchased from VWR International or equivalent source.

[0138] Phosphate buffered saline solution consists of two separately prepared solutions (Solution A and Solution B). To prepare 1 L of Solution A, add 1.38 ± 0.005 g of sodium phosphate monobasic monohydrate and 8.50 ± 0.005 g of sodium chloride to a 1000 mL volumetric flask and add deionized water to volume. Mix thoroughly. To prepare 1 L of Solution B, add 1.42 ± 0.005 g of anhydrous sodium phosphate disodium hydrogen and 8.50 ± 0.005 g of sodium chloride to a 1000 mL volumetric flask and add deionized water to volume. Mix thoroughly. To prepare phosphate buffered saline solution, add 450 ± 10 mL of Solution B to a 1000 mL beaker and stir at low speed on a stir plate. Insert a calibrated pH probe (accurate to 0.1) into the beaker of Solution B and add enough Solution A while stirring to bring the pH to 7.2 ± 0.1.

[0139] The mucus component is a mixture of phosphate buffered saline solution, potassium hydroxide aqueous solution, gastric mucin and lactic acid aqueous solution. The amount of gastric mucin added to the mucus component directly affects the final viscosity of the prepared AMF. In order to determine the amount of gastric mucin required to obtain AMF in the target viscosity range (7.15-8.65 centistokes at 23°C), 3 batches of AMF with different amounts of gastric mucin were prepared in the mucus component, and then the exact amount required was interpolated from the concentration-viscosity curve using a three-point least squares linear fit. The successful range of gastric mucin is usually between 38 grams and 50 grams.

[0140] To prepare approximately 500 mL of the mucus fraction, 460 ± 10 mL of the previously prepared phosphate buffered saline solution and 7.5 ± 0.5 mL of a 10% w / v potassium hydroxide aqueous solution are added to a 1000 mL heavy glass beaker. The beaker is placed on a stirring hot plate and the temperature is raised to 45°C ± 5°C while stirring. A predetermined amount of gastric mucin (± 0.50 g) is weighed and slowly sprinkled into the previously prepared liquid that has reached 45°C without agglomeration. The beaker is covered and mixing continues. Within 15 minutes, the temperature of the mixture is brought to above 50°C, but not more than 80°C. While maintaining this temperature range, heating is continued for 2.5 hours with gentle stirring. After 2.5 hours, the beaker is removed from the hot plate and cooled to below 40°C. Next, 1.8 ± 0.2 mL of a 10% v / v lactic acid aqueous solution is added and mixed thoroughly. The mucus fraction mixture is autoclaved at 121°C for 15 minutes and cooled for 5 minutes. The mixture of mucus components was removed from the autoclave and stirred until the temperature reached 23°C ± 1°C.

[0141] Allow the temperature of the sheep blood and mucus components to reach 23°C ± 1°C. Using a 500 mL graduated cylinder, measure the volume of the entire batch of previously prepared mucus components and add it to a 1200 mL beaker. Add an equal amount of sheep blood to the beaker and mix thoroughly. Using the viscosity method described above, ensure that the viscosity of the AMF is between 7.15-8.65 centistokes. If not, dispose of the batch and make another batch as needed for adjusting the mucus component.

[0142] Unless intended for immediate use, qualified AMF should be refrigerated at 4°C. After preparation, AMF may be stored in an airtight container at 4°C for up to 48 hours. Prior to testing, the AMF must be brought to 23°C ± 1°C. After testing is complete, discard any unused portion.

[0143] 7. Collection time

[0144] The acquisition time of an absorbent article loaded with artificial menstrual fluid (AMF) as described herein was measured using a strike-through plate and an electronic circuit interval timer. The time required for the absorbent article to acquire one dose of AMF was recorded. All tests were conducted in a laboratory maintained at 23°C ± 2°C and 50% ± 2% relative humidity.

[0145] See also 7A to 7E , the strike-through plate 9001 is constructed of plexiglass with an overall size of 10.2 cm long by 10.2 cm wide by 3.2 cm high. The longitudinal channel 9007 extending along the length of the plate is 13 mm deep and 28 mm wide at the top plane of the plate, with the side walls sloping down at 65° to a 15 mm wide base. The central test fluid well 9009 is 26 mm long, 24 mm deep and 38 mm wide at the top plane of the plate, with the side walls sloping down at 65° to a 15 mm wide base. At the bottom of the test fluid well 9009, there is an "H" shaped test fluid reservoir 9003, which leads to the bottom of the plate to introduce fluid to the article below. The test fluid reservoir 9003 has a total length ("L") of 25 mm, a width ("W") of 15 mm, and a depth ("D") of 8 mm. The longitudinal legs of the reservoir are 4 mm wide and have rounded ends with a radius 9010 of 2 mm. The legs are 3.5 mm apart. The center post has a radius 9011 of 3 mm and houses opposing electrodes 9004 that are 6 mm apart. The sides of the reservoir are arched outward at a radius 9012 of 14 mm defined by an overall width W of 15 mm. Two wells 9002 (80.5 mm long x 24.5 mm wide x 25 mm deep) located outside the lateral channels are filled with lead shot to adjust the overall mass of the plate to provide 0.25 psi (17.6 gf / cm 2) of the restraining pressure. Electrodes 9004 are embedded in plate 9001, thereby connecting an external banana-shaped socket 9006 to the inner wall of fluid reservoir 9003. A circuit interval timer is inserted into the socket 9006 to the inner wall 9005 of fluid reservoir 9003. A circuit interval timer (not shown in the drawings) is inserted into the socket 9006 and monitors the impedance between the two electrodes 9004 and measures the time from the introduction of AMF into reservoir 9003 until the AMF is discharged from the reservoir. The timer has a resolution of 0.01 seconds.

[0146] Remove the test product from all packaging, being careful not to press or pull on the product while handling. Do not attempt to smooth out wrinkles. Condition the test specimens at 23°C ± 2°C and 50% ± 2% relative humidity for at least 2 hours prior to testing.

[0147] The required mass of the strike-through panel must be calculated for the specific dimensions of the test article so that a confining pressure of 1.72 kPa is applied. Determine the longitudinal midpoint and lateral midpoint of the absorbent core of the article. Measure and record the lateral width of the core to the nearest 0.1 cm. The required mass of the strike-through panel is calculated as the core width multiplied by the strike-through panel length (10.2 cm) multiplied by 17.6 gf / cm 2 , and record the required mass to the nearest 0.1 g. Add lead pellets to the plate to obtain the calculated mass.

[0148] Connect the electronic circuit interval timer to the strike-through plate 9001 and reset the timer to zero. Place the test product on a flat, level surface with the body side facing up. Gently place the strike-through plate 9001 onto the center of the test product to ensure that the "H" shaped reservoir 9003 is centered over the test area.

[0149] Using a mechanical pipette, 3.00 mL ± 0.05 mL of AMF was accurately drawn into the test fluid reservoir 9003. The fluid was dispensed along the molded lip at the bottom of the reservoir 9003 in 3 seconds or less without splashing. After the fluid had been collected, the collection time was recorded to the nearest 0.01 second. The electrodes 9004 were fully cleaned before each test.

[0150] In a similar manner, a total of three (3) replicates were tested for each test product to be evaluated. The acquisition time (seconds) was reported as the average of the replicates to the nearest 0.01 second.

[0151] 8. Back-infiltration

[0152] For absorbent articles loaded with artificial menstrual fluid (AMF) as described herein, light pressure rewet is measured. After dispensing 3.0 grams and 12.0 grams of AMF, the amount of fluid left on the top sheet under 0.1 psi pressure, i.e., rewet, is measured. All tests are conducted in a laboratory maintained at 23°C ± 2°C and 50% ± 2% relative humidity.

[0153] Remove the test product from all packaging, being careful not to press or pull on the product while handling. Do not attempt to smooth out wrinkles. Condition the test specimens at 23°C ± 2°C and 50% ± 2% relative humidity for at least 2 hours prior to testing.

[0154] The required mass of the plate must be calculated (to the nearest 0.01 gram) for the specific dimensions of the test article so that a confining pressure of 0.1 psi pressure is applied. Determine the longitudinal midpoint and lateral midpoint of the absorbent article. Measure and record the lateral width of the absorbent article to the nearest 0.1 cm.

[0155] Place the test product onto a flat, level surface with the body side facing up. Place the test vial on a scale and return it to zero. Use a pipette to add 3.00 grams to the vial and weigh to the nearest 0.01 gram. Then carefully dispense the fluid onto the center of the test article. Wait 3 minutes.

[0156] Place 4-6 pieces of filter paper of known weight (referred to as "dry weight") (typical laboratory filter paper, such as Ahlstrom #632 12.7 cm x 12.7 cm filter paper) on top of the central fluid area. Apply the required mass to produce 0.1 psi pressure, which is held under pressure for 5 seconds.

[0157] The filter paper is weighed again (referred to as the "wet weight"). The difference between the wet weight and the dry weight of the filter paper is the light pressure re-permeation at the amount of fluid added.

[0158] The testing steps are repeated until 12.00 grams of fluid are dispensed on the absorbent article.

[0159] In a similar manner, a total of three (3) to six (6) replicates were tested for each test product to be evaluated. The light pressure re-bleed was reported as the arithmetic mean of the replicates to the nearest 0.01 gram.

[0160] 9. Vertical wicking height

[0161] The vertical wicking height of the nonwoven was measured according to INDA / EDANA standard test: WSP 10.1 (05) "7.3 The liquid wicking rate (capillarity)". Six replicates of each sample were tested and the average (arithmetic mean) of the six replicates was recorded as the vertical wicking height.

[0162] 10. Radius Relative Shape Factor

[0163] SEM images of vertical cross sections of the fibers were obtained and analyzed as follows to determine the radius relative shape factor ("RSFR") of the fibers. The fibers to be analyzed were randomly selected. Figure 6 , for each fiber analyzed, two circles are drawn. The first is the smallest circle that circumscribes the entire fiber cross section, and R1 is defined as the radius of this first circle. The second is the largest circle that can be completely inscribed in the fiber cross section, and R2 is defined as the radius of this second circle.

[0164] The RSFR of a fiber is calculated as follows:

[0165]

[0166] At least 10 replicates of the sample fiber are tested and the average (arithmetic mean) of the at least 10 replicates (rounded to the nearest thousandth) is reported as the RSFR of the fiber.

[0167] 11. Air permeability

[0168] The air permeability of the initial nonwoven and the wetted and re-dried nonwoven was tested. The wetted and re-dried samples were prepared as follows:

[0169] The sample nonwoven is placed in a basin with enough distilled water so that the fluid covers the sample nonwoven completely. The sample nonwoven is immersed in water and kept for 5 min so that the sample nonwoven absorbs water completely. Use a retainer to take out the sample nonwoven from the water, and allow it to dry naturally for 24 h in a laboratory maintained at 23 ± 2 ℃ and 50 ± 2% relative humidity.

[0170] All measurements were conducted in a laboratory maintained at 23°C ± 2°C and 50% ± 2% relative humidity, and the test specimens were conditioned in this environment for at least 2 hours prior to testing.

[0171] The air permeability of the substrate was determined according to INDA / EDANA nonwoven standard procedure NWSP 070.1.R0 (15) using a Textest FX3300 (Textest Instruments, Schwerzenbach, Switzerland) air permeability tester or equivalent. The area of ​​application was 38 cm 2 The circular test head is used and the pressure is maintained at a fixed level of 125 Pa on the sample at a rate of cubic meters per square meter per minute (m 3 / m 2 / min) through the sample. Twelve rectangular samples of the material (initial material and wetted and redried samples) were taken so that the center of each sample corresponded to the center of the material and so that the length and width of each sample were greater than the smallest dimension of the circular head. The sample was placed under the test head so that the center of the sample matched the center of the test head. Five lower samples were analyzed in this way and the airflow was measured in m 3 / m 2 / minRecord the air permeability of each sample, accurate to 1m 3 / m 2 / min. Calculate the arithmetic mean of the results for each sample and report it as the air permeability in m 3 / m 2 / min, accurate to 1m 3 / m 2 / min.

[0172] Example

[0173] Example 1

[0174] Various nonwovens for fluid management layers were constructed and tested. For each of the examples, the following Table 1 lists their component material compositions. All nonwoven substrates were hydroentangled and spunlaced.

[0175] Figure 4 and Figure 5 is a scanning electron microscope image of nonwoven 1. Figure 4 , nonwoven 1 400 contains non-swelling wicking fibers (in this case 1 dtex X-shaped PET fibers) 402, stiffening fibers (in this case 5.5 dtex PE / PET core / sheath bicomponent fibers) 404 and elastic fibers (in this case 10 dtex FENC hollow spiral PET fibers) 406. Figure 5 is a magnified image of the SEM image of nonwoven 1, which more clearly shows the non-swollen wicking fibers.

[0176] The RSFR of a 1.5 dtex X-shaped PET fiber was tested according to the Radius Relative Shape Factor test performed under Test Methods 17 replicas of the fiber were tested and a RSFR value of 41.8% was obtained.

[0177] For the thickness coefficient, 48 replicas of each sample were tested for thickness, and the average of the 48 replicas was recorded as the thickness coefficient.

[0178] The Vertical Wicking Height of Nonwovens 1 through 7 was tested according to the Vertical Wicking Height Test conducted under the CERTAINTY WICKING HEIGHT SYSTEM.

[0179] Table 1

[0180]

[0181]

[0182]

[0183] 1.5dtex X-type PET: Far Eastern New Century Corporation

[0184] 1.7dtex PE / PP bicomponent: Toray Advanced Materials Korea Inc. 2.2dtex PE / PET bicomponent: Jiangsu Jiangnan High Polymer Fiber Co., Ltd.

[0185] 5.5dtex PE / PET two-component: Jiangsu Jiangnan High Fiber Co., Ltd.

[0186] 4.4dtex PET fiber: Sinopec Yizheng Chemical Fiber Co., Ltd.

[0187] 10dtex hollow spiral PET: Far Eastern New Century Co., Ltd.

[0188] Nonwoven 1 and Nonwoven 2 (nonwovens of the present invention) have high thickness factors and show high vertical wicking height values ​​even over extended periods of time (5 min). The high vertical wicking height values ​​may explain the low rewet values ​​in the absorbent articles of the present invention.

[0189] Nonwovens 3 and 5 (comparative nonwovens), which did not include non-swelling wicking fibers, exhibited vertical wicking height values ​​that were significantly lower than the inventive nonwovens.

[0190] Nonwoven 6 (comparative nonwoven), which contains 1.5 dtex round PBT fibers instead of non-swelling wicking fibers and contains insufficient amounts of stiffening fibers and elastic fibers, has a relatively low thickness factor.

[0191] Nonwoven 7 (comparative nonwoven), which contains non-swollen synthetic fibers of high dtex, exhibits vertical wicking height values ​​that are significantly lower than the nonwovens of the present invention.

[0192] The air permeabilities of Nonwoven 1 and Nonwoven 3 under two conditions (initial condition and wet and re-dried condition) were tested according to the Air Permeability Test conducted under the Test Method and are shown in Table 2 below.

[0193] Table 2

[0194]

[0195] SD*: Standard deviation

[0196] Nonwoven 1 showed essentially no change in air permeability values ​​between the initial condition and the wet and re-dried condition, confirming that there was essentially no change in the pore size and channels in the nonwoven. Nonwoven 3 showed a significant decrease in air permeability between the wet and re-dried condition and the initial condition, reflecting that the pore size and channels in the nonwoven may be reduced due to the presence of a large amount of absorbent fibers.

[0197] Example 2

[0198] Disposable absorbent articles including a fluid management layer according to the present invention were constructed and tested. In addition, a plurality of disposable absorbent articles including a comparative fluid management layer were constructed and tested. The difference between the samples was only the fluid management layer as shown in Table 3 below. Sample 1 and Sample 2 were inventive samples, and Samples 3 to 7 were comparative samples. The inventive samples included the fluid management layer of the present disclosure, while the comparative sample absorbent articles included the comparative fluid management layer. For each of the inventive samples and the comparative samples, the following components were used.

[0199] Topsheet - The topsheet used for each of the inventive and comparative samples was a 24 gsm carded air-permeable nonwoven made of 60% hydrophilic PE / PET bicomponent fibers and 40% hydrophobic PE / PET bicomponent fibers. The nonwoven was purchased from Yanjan Company, China.

[0200] Absorbent Core - The absorbent core was a 145 gsm MBAL core comprising pulp fibers, absorbent gelling materials and bicomponent fibers, commercially available from Fitsta, China.

[0201] Table 3

[0202]

[0203] The acquisition time and rewet test of each sample were measured according to the acquisition time test and the rewet test performed under the above test method, respectively, and the results are shown in Table 4.

[0204] Table 4

[0205]

[0206] Sample 1 and Sample 2 (inventive samples) exhibit high acquisition times even upon repeated liquid insults. In addition, Sample 1 and Sample 2 exhibit low rewet values ​​even upon repeated liquid insults.

[0207] Sample 3 and Sample 5 (comparative samples) that do not include non-swelling wicking fibers exhibit significantly lower acquisition times than the inventive samples. Note that the acquisition times in Samples 3 and 5 increase significantly upon repeated liquid insults.

[0208] Sample 4 (comparative sample), which does not include non-swelling wicking fibers, exhibits significantly higher rewet values ​​than the inventive samples. Note that the rewet values ​​in Sample 3 increase significantly upon repeated liquid insults.

[0209] Sample 6 (comparative sample), which contained 1.5 dtex round PBT fibers instead of non-swelling wicking fibers, exhibited a significantly lower acquisition time than the inventive samples, and the acquisition time increased significantly upon repeated liquid insults.

[0210] Sample 7 (comparative sample) containing 6.6 dtex trilobal PET and 6.6 dtex pentagonal PET fibers has a very high rewet value. Upon repeated liquid insults, the rewet value increases significantly.

[0211] The dimensions and values ​​disclosed herein are not to be understood as being strictly limited to the exact numerical values ​​cited. Instead, unless otherwise indicated, each such dimension is intended to represent the stated value and a functionally equivalent range around that value. For example, a dimension disclosed as "40 mm" is intended to mean "about 40 mm".

[0212] Unless expressly excluded or otherwise limited, each document cited herein, including any cross-referenced or related patent or application, is incorporated herein by reference in its entirety. Citation of any document is not an admission that it is prior art to any of the present invention disclosed or claimed herein, or that it, by itself or in combination with any one or more references, proposes, suggests, or discloses any such invention. In addition, to the extent that any meaning or definition of a term in this invention conflicts with any meaning or definition of the same term in a document incorporated by reference, the meaning or definition assigned to that term in this invention shall govern.

[0213] Although specific embodiments of the present invention have been illustrated and described, it will be apparent to those skilled in the art that various other changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, it is intended that all such changes and modifications within the scope of the present invention be covered in the appended claims.

Claims

1. An absorbent article having a skin-facing side and a garment-facing side, the absorbent article include: a liquid-permeable top sheet, a liquid-impermeable back sheet, an absorbent core disposed between the top sheet and the back sheet, and a fluid management layer disposed between the top sheet and the absorbent core, wherein the fluid management layer comprises from about 10% to about 60% by weight of the fluid management layer of non-swelling wicking fibers, from about 15% to about 70% by weight of the fluid management layer of elastic fibers, and from about 25% to about 70% by weight of the fluid management layer of stiffening fibers, as determined by material composition analysis, and wherein the non-swelling wicking fiber has a Radius Relative Shape Factor in a range from about 25% to about 100% as determined by the Radius Relative Shape Factor Test, and wherein the non-swelling wicking fiber has a linear density of about 0.8 dtex to about 3.3 dtex as determined by the Fiber Decitex Test.

2. The absorbent article of claim 1, wherein the fluid management layer further comprises from about 1% to about 40% absorbent fibers by weight of the fluid management layer as determined by the material composition analysis.

3. The absorbent article according to any one of the preceding claims, wherein the non-swelling wicking fibers have a cross-shaped, trilobal, pentagonal, "H"-shaped, "Y"-shaped, "X"-shaped, "T"-shaped or flat ribbon-shaped cross-section.

4. An absorbent article according to any of the preceding claims, wherein the fluid management layer comprises a first nonwoven web and a second nonwoven web, the first nonwoven web being closest to the wearer-facing surface of the absorbent article, the percentage of non-swelling wicking fibers in the first nonwoven web by weight of the first nonwoven web and the percentage of non-swelling wicking fibers in the second nonwoven web by weight of the second nonwoven web being different from each other.

5. The absorbent article according to any of the preceding claims, wherein the non-swelling wicking fibers comprise thermoplastic fibers selected from the group consisting of monocomponent fibers, bicomponent fibers comprising polyolefin fibers, and combinations thereof.

6. An absorbent article according to any one of the preceding claims, wherein the elastic fibers have a melting temperature higher than the melting temperature of the stiffened fibers 7. The absorbent article according to any one of the preceding claims, wherein the elastic fibers have a linear density of about 4 dtex or more.

8. The absorbent article according to any one of the preceding claims, wherein the fibers in the fluid management layer are integrated.

9. The absorbent article according to any one of the preceding claims, wherein the fibers in the fluid management layer are staple fibers.

10. The absorbent article according to any one of the preceding claims, wherein the fluid management layer is hydroentangled.

11. The absorbent article according to any one of the preceding claims, wherein the fluid management layer has a basis weight of from about 20 gsm to about 120 gsm.

12. The absorbent article of any of the preceding claims, wherein the absorbent article exhibits an Average Acquisition Speed ​​of less than about 30 seconds in a first gush and less than about 60 seconds in a third gush when measured according to the Acquisition Time Test disclosed herein.

13. A nonwoven sheet comprising, by weight of the fluid nonwoven, from about 10% to about 60% non-swelling wicking fibers, from about 15% to about 70% elastic fibers, and from about 25% to about 70% stiffening fibers as determined by the material composition analysis, and wherein the non-swelling wicking fibers have a radius relative shape factor in the range of from about 25% to about 100% as determined by the radius relative shape factor test, and the non-swelling wicking fibers have a linear density of 0.8 dtex to 3.3 dtex as determined by the fiber dtex test.

14. The nonwoven sheet according to claim 13, wherein the nonwoven sheet is hydroentangled.

15. An absorbent article having a skin-facing side and a garment-facing side, the absorbent article include: a liquid-permeable top sheet, a liquid-impermeable back sheet, an absorbent core disposed between the top sheet and the back sheet, and a fluid management layer disposed between the top sheet and the absorbent core, wherein the fluid management layer comprises from about 10% to about 60% by weight of the fluid management layer of non-swelling wicking fibers, and at least one of from about 15% to about 70% by weight of the fluid management layer of elastic fibers and from about 25% to about 70% by weight of the fluid management layer of stiffening fibers as determined by the material composition analysis, and wherein the non-swelling wicking fiber has a Radius Relative Shape Factor in a range of about 25% to about 100% as determined by the Radius Relative Shape Factor Test, and wherein the non-swelling wicking fiber has a linear density of about 0.8 dtex to about 3.3 dtex as determined by the Fiber Decitex Test.

16. A nonwoven sheet comprising, by weight of the fluid nonwoven, from about 10% to about 60% of non-swelling wicking fibers, and at least one of from about 15% to about 70% of elastic fibers and from about 25% to about 70% of stiffening fibers, as determined by said material composition analysis, and wherein the non-swelling wicking fiber has a Radius Relative Shape Factor in a range from about 25% to about 100% as determined by the Radius Relative Shape Factor Test, and wherein the non-swelling wicking fiber has a linear density of 0.8 dtex to 3.3 dtex as determined by the Fiber Decitex Test.