Method for producing plastic compounds with improved properties

By adjusting the screw machine parameters and using a variety of thermoplastic components in a multi-axis screw machine, the problems of plasticity and flux of thermoplastic components in the screw machine are solved, and efficient plasticity and economical production are achieved.

CN119053427APending Publication Date: 2024-11-29COVESTRO DEUTSCHLAND AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034487.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-19
Filing Date
2023-04-11
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In a multi-axis screw machine with a co-rotating parallel screw shaft with constant speed rotation, it is difficult to achieve good plasticity and high throughput in the production process of two or more thermoplastic components with different viscosity. , the prior art lacks effective methods to adjust parameters affecting plasticization quality to achieve economic feasibility.

Method used

By adjusting parameters in the screw machine, such as melting rate, screw shaft rate and the use of additives, ensure that the proportion of unmelted particles in the plastic body is less than 5%, and maintaining a specific melting rate range within the longitudinal section of the screw machine, achieving Good plasticity. The specific method includes using at least two thermoplastic components, one of which is polycarbonate, and controlling dynamic viscosity and temperature conditions in a screw machine.

Benefits of technology

It realizes the production of plastic bodies with good plasticity in a co-rotating parallel screw shaft multi-axis screw machine with constant speed rotation, ensuring high throughput and economical feasibility of the plastic bodies, and the proportion of unmelted particles is acceptable Within range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005087456370000041
    Figure BDA0005087456370000041
  • Figure BDA0005087456370000072
    Figure BDA0005087456370000072
  • Figure BDA0005087456370000101
    Figure BDA0005087456370000101
Patent Text Reader

Abstract

The invention relates to a method for producing plastic bodies with improved properties from formulations comprising at least two thermoplastic components in a multi-shaft screw machine having screw shafts rotating in the same direction, parallel and constant speed, in which the plastic compound (i) does not contain additives that are free-flowing at 23 DEG C, and the plastic compound (ii) does not contain additives that are free-flowing at 23 DEG C. Or (ii) exactly one additive that is free-flowing at 23 DEG C, or (iii) at least two additives that are free-flowing at 23 DEG C. In particular, the invention relates to a method for producing plastic bodies from a formulation comprising at least two thermoplastic components, at least one of which is a polycarbonate. In particular, the screw machine is a twin-screw extruder having screw shafts rotating in the same direction, in parallel and at a constant speed.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention provides a method for producing a plastic body with improved properties from a formulation comprising at least two thermoplastic components in a multi-shaft screw machine having co-rotating parallel screw shafts rotating at equal speeds, wherein the plastic body

[0002] (i) does not contain any additive which is free-flowing at 23°C,

[0003] or

[0004] (ii) contains exactly one additive which is free-flowing at 23°C,

[0005] or

[0006] (iii) comprising at least two additives which are free-flowing at 23°C.

[0007] In particular, the invention provides a method for producing a plastic body from a formulation comprising at least two thermoplastic components, at least one of which is a polycarbonate. In addition, in particular, the screw machine is a twin-screw extruder with co-rotating parallel screw shafts rotating at equal speeds.

[0008] Multi-shaft screw machines with co-rotating parallel screw shafts rotating at the same speed can be found in the technical literature, for example [1] ([1] = Klemens Kohlgrüber: Der The corotating twin-shaft extruder is fully understood in the following literature:

[0009] The uses of such screw machines (also called extruders) include the mixing of plastics or viscoelastics, in particular the mixing of plastics, in particular for the mixing of melts or solutions of thermoplastic polymers or for the mixing of melts or solutions of rubber: [1], pages 50 to 63.

[0010] If two or more different thermoplastic components with significantly different viscosities are present in the formulation for producing the plastic bodies, it is difficult to achieve good plasticization and at the same time reconcile a high throughput of the plastic bodies through the screw machine with a low energy input to the plastic bodies.

[0011] The fact that good plasticization is difficult to achieve is documented, for example, in the paper "Melting Model for Co-Rotating Twin-Screw Extruders", Elemans, PHM et al., ANTEC 2002, Proceedings, Volume 1, Processing, pages 355 to 359. The solution proposed here is to significantly reduce the pellet size of the thermoplastic component used in order to achieve good plasticization. However, only a thermoplastic component containing only one thermoplastic component is used and considered. 40D formula.

[0012] From the results presented, no indication can be drawn regarding the use of polycarbonate-containing formulations with at least two thermoplastic components for the production of plastic bodies with good plasticization. Furthermore, since the thermoplastic components in the formulations are usually not produced in-house but purchased from external manufacturers, it is difficult to achieve a reduction in the particle size of the thermoplastic components used.

[0013] In the paper “Melting of polymer blends in co-rotating twin screw extruders. Part I, Part II, Part III” Potente, H. et al., Int Polymer Processing XVI (2001) 2, pp. 124-130, 131-142 and 143-150, a calculation model for the quality classification of thermoplastic components is proposed based on literature search and experiments, which is implemented in the SIGMA simulation software. The experiments to verify the model were carried out with a mixture of the thermoplastic components PA6 and PP. However, Figures 12-14 on pages 149 and 150 show that the agreement between the experiment and the calculation is very low. On the basis of the experiments, it is also shown that the size of the pellets of the thermoplastic component used and the ratio of the size of the pellets of the thermoplastic component to the groove depth of the screw element are important specific process variables for achieving good plasticization. The influence of the pellet size is only discussed theoretically; there are no experimental details on different pellet sizes. Furthermore, it is mentioned that the viscosity ratio of the thermoplastic components is essential for good plasticization. However, this is also only a qualitative statement.

[0014] Due to the low agreement between the model and the experimental results, it is not possible to draw any conclusions about the use of formulations with at least two thermoplastic components, at least one of which is a polycarbonate, for producing plastic bodies with good plasticization.

[0015] In the paper "Evaluation of melting performance of a co-rotating twin-screwextruder", eleman, PHM et al., ANTEC 2002, Proceedings, Volume I, Processing, pages 350-354, experiments with formulations consisting of thermoplastic components show that the plasticization quality increases linearly with increasing residence time in the extruder and also depends significantly on the screw speed. However, it is not clear what throughput was used to carry out the experiments. All that is stated is the torque to be set (in percent), but there is no information on what torque in nM corresponds to 100% of the torque. All experiments were carried out with a mixture containing only The formulation was carried out with 40D as the only thermoplastic component.

[0016] Since only one formulation with one thermoplastic component was studied and the experimental setup was not documented, it is not possible to infer any indication that plastic bodies with good plasticization can be produced using formulations with at least two thermoplastic components, at least one of which is a polycarbonate.

[0017] In the paper "Melting of high-heat Polyamide in a co-rotating twin-screwextruder" Janssen, JMH, Sierksma, WR, ANTEC 2002, Proceedings, Volume III, Special Areas, pages 3712-3715, experiments using a formulation consisting of nylon-4,6, nylon-4,6 and nylon 6 and adding other unspecified low melting point additives showed that high energy input, low speed, low torque and long and melt-filled kneading block zones improved the plasticization quality, but adding nylon-6 and / or low melting point additives to nylon-4,6 deteriorated the plasticization. In addition, it is pointed out that at higher speeds, due to insufficient residence time in the extruder, the energy input increases but the plasticization quality decreases at the same time.

[0018] From the presented results no indications can be drawn about the use of polycarbonate-containing formulations containing at least two thermoplastic components for the production of plastic bodies with good plasticization, since only qualitative statements are made about the influence of process parameters (screw group and formulation components). Furthermore, no indication is given as to how a high economic feasibility can be achieved while achieving good plasticization. Reducing the speed and torque inevitably leads to a reduction in throughput and thus to a reduction in economic feasibility.

[0019] No one in the prior art has pointed out how the parameters that influence the plasticization quality can be linked to one another in order to achieve good plasticization properties, and if possible, good plasticization properties can be achieved even in cases where one or more of these influencing parameters cannot or should not be changed (for example for cost or quality reasons), because one or more of the other influencing parameters are changed in a suitable manner.

[0020] Therefore, the object of the present invention is to provide a method for producing a plastic body with good plasticization in a multi-axis screw machine with co-rotating parallel screw shafts rotating at the same speed, wherein the influencing parameters affecting the plasticization quality are adjusted to achieve good plasticization. Another object of the present invention is to provide a method for producing a plastic body with good plasticization in a multi-axis screw machine with co-rotating parallel screw shafts rotating at the same speed, wherein the influencing parameters affecting the plasticization quality can be adjusted so that even in the case where at least one of these influencing parameters cannot or should not be changed, good plasticization is achieved because one or more other influencing parameters are changed in an appropriate manner. Therefore, the method of the present invention is to achieve good plasticization, which is essentially independent of the following parameters: the screw machine used, the screw group therein, the screw diameter therein, the number of screw shafts therein, the components of the formulation used to produce the plastic body, and the process parameters (such as the speed of the screw shafts and the mass flow rate of the plastic body through the screw machine). In particular, the formulation for producing the plastic body should contain at least two thermoplastic components, at least one of which is a polycarbonate.

[0021] In the context of the present invention, good plasticization is characterized by the fact that the number of completely or partially unmelted particles of the thermoplastic component present in the formulation does not exceed 5% by mass of the granules produced from the plastic body, in particular does not exceed 3% by mass of the granules produced from the plastic body, very particularly does not exceed 2% by mass of the granules produced from the plastic body, and very particularly does not exist in the granules produced from the plastic body. It is unacceptable for the number of granules containing completely or partially unmelted particles to exceed 2%, in particular to exceed 3%, very particularly to exceed 5%.

[0022] Surprisingly, this object is achieved by a method having the features of the main claim.

[0023] In particular, it has been found that good plasticity can be achieved when the so-called melting rate is kept within a certain range of values. The melting rate is a dimensionless index.

[0024] More particularly, it has been found that good plasticization is achieved at a melting rate of 1.18 to 8, preferably 1.18 to 5, more preferably 1.2 to 3 in a longitudinal section of the screw machine, starting from a distance of twice the inner shell diameter D upstream of the first screw element that is not a conveying element and ending at the last screw element of the screw machine;

[0025] The melting rate is as follows:

[0026]

[0027] and among them:

[0028] τ1 is the average residence time of the plastic bodies in a longitudinal section of the screw machine, said longitudinal section starting at a distance of twice the inner shell diameter D upstream of the first screw element which is not a conveying element, and

[0029] In case (i), the end is at the last screw element of the screw machine,

[0030] and in case (ii) or (iii), terminates at the first addition point of the additive which is free-flowing at 23° C. downstream of the first spiral element which is not a conveying element,

[0031] And among them,

[0032] δη1 is the ratio of the dynamic viscosity of the plastic to the shear rate corresponding to the screw shaft speed n. Next, and

[0033] In case (i), the plastic body temperature is 230°C,

[0034] and in case (ii), the temperature of the plastic body is 230° C. minus <230° C. multiplied by twice the mass ratio of the exactly one additive which is free-flowing at 23° C.>, the mass ratio being based on the mass of the plastic body,

[0035] and in case (iii), the temperature of the plastic body is 230° C. minus <230° C. multiplied by twice the sum of the mass ratios of the at least two free-flowing additives at 23° C.>, the mass ratios being based on the total mass of the plastic body,

[0036] Based on the dynamic viscometer of the thermoplastic component with the highest dynamic viscosity measured under the following conditions, the condition is a shear rate of 200 1 / s and

[0037] In case (i), at a temperature of 230°C,

[0038] and in case (ii), at a temperature of 230° C. minus <230° C. multiplied by twice the mass ratio of the exactly one additive that is free-flowing at 23° C.>, the mass ratio being based on the mass of the plastic body,

[0039] and in case (iii), at a temperature of 230° C. minus <230° C. multiplied by twice the sum of the mass ratios of the at least two free-flowing additives at 23° C.>, the mass ratio being based on the mass of the plastic body;

[0040] τ2 is

[0041] in cases (ii) and (iii), the average residence time of the plastic mass in a longitudinal section of the screw machine, starting from the first addition point of the free-flowing additive at 23° C. at a distance of twice the inner shell diameter D upstream of the first screw element which is not a conveying element, and ending at the last screw element of the screw machine,

[0042] and in case (i), is zero,

[0043] δη2 is the shear rate corresponding to the screw shaft speed n The ratio of the dynamic viscosities of the plastic body at a shear rate of 200 1 / s and at a temperature corresponding to the temperature of the plastic body at the end of the last screw element, based on a dynamic viscometer of the thermoplastic component with the highest dynamic viscosity measured at a shear rate of 200 1 / s and at a temperature corresponding to the temperature of the plastic body at the end of the last screw element,

[0044] λ is the thermal conductivity measured at 23 °C according to EN ISO 11357-8:2021, measured immediately after the plastic body comes out of the screw machine;

[0045] n is the speed of the screw shaft of the screw machine,

[0046] d is the diameter of the pellets of polycarbonate present in the formulation for producing the plastic body having the highest relative viscosity, measured in accordance with EN ISO 1628-1:2021,

[0047] D is the inner diameter of the screw machine casing, where the inner shell diameter D is the same for all screw machine casings here,

[0048] c p is the average specific heat capacity measured in the temperature range of 250°C to 300°C according to ISO 11357-4:2021,

[0049] It is the mass flow rate of the plastic body in the screw machine.

[0050] This is especially true for the following methods:

[0051] Method for producing plastic bodies in a multi-screw machine with co-rotating parallel screw shafts rotating at equal speed,

[0052] The screw shaft rotates at a speed n,

[0053] wherein the plastic body is produced from a formulation comprising at least two thermoplastic components,

[0054] wherein at least one of the at least two thermoplastic components is a polycarbonate,

[0055] The plastic body

[0056] (i) does not contain any additive which is free-flowing at 23°C,

[0057] or

[0058] (ii) contains exactly one additive which is free-flowing at 23°C,

[0059] or

[0060] (iii) comprising at least two additives which are free-flowing at 23°C,

[0061] The dynamic viscosity of the plastic body is measured according to ISO 11443:2014 method A2 under the following conditions: at a shear rate of 200 1 / s Next, and

[0062] In case (i), the temperature is 230°C,

[0063] and in case (ii), the temperature is 230°C minus <230°C multiplied by the said exactly one

[0064] ℃> twice the mass ratio of the free-flowing additives, the mass ratio being based on the mass of the plastic body,

[0065] and in case (iii), the temperature is 230°C minus <230°C multiplied by the at least two

[0066] ℃> twice the sum of the mass ratios of the free-flowing additives, the mass ratios being based on the mass of the plastic body,

[0067] The dynamic viscosity is measured in the ratio 0.3 to 3, based on the shear rate of 200 1 / s according to ISO 11443:2014 method A2. a viscosity meter of at least one of the thermoplastic components measured at 20° C. and at a temperature of 230° C.;

[0068] and wherein at least two of the thermoplastic components differ in at least one of the following characteristics:

[0069] At least one structural unit is different,

[0070] or

[0071] The difference in relative solution viscosity, measured according to EN ISO 1628-1:2021, is at least 5%,

[0072] The method is characterized, among other things, by the melting rate.

[0073] For further clarification, it should be noted that:

[0074] The rate n is the number of rotations within a period of time based on the time period and corresponds to the inverse of the number of revolutions T, ie n=1 / T.

[0075] The relative solution viscosity difference is measured according to EN ISO 1628-1:2021 in dichloromethane at a concentration of 5 g sample per litre of dichloromethane at 25 °C using an Ubbelohde viscometer.

[0076] δη1 is the shear rate corresponding to the screw shaft speed n The simplified equation is possible because the shear rate is proportional to the velocity.

[0077] d is the diameter of the pellets of polycarbonate present in the formulation for producing the plastic body having the highest relative viscosity, measured in accordance with EN ISO 1628-1:2021 and calculated from the weight of 100 pellets and the diameter of an equivalent sphere of the solid density as follows:

[0078]

[0079] in

[0080] m 100 is the weight of 100 pellets of polycarbonate present in the formulation for producing a plastic body having the highest relative viscosity, measured in accordance with EN ISO 1628-1:2021, measured with a commercially available balance,

[0081] r 固体 is the density of the polycarbonate present in the formulation for producing the plastic body having the highest relative viscosity, measured according to EN ISO 1628-1:2021, and the density measured according to EN ISO 1183-1:2019 (method A),

[0082] p is the circular constant.

[0083] In the context of the present invention, based on a multi-shaft screw machine, details concerning position and direction in the conveying direction of the entire multi-shaft screw machine should always be taken into account.

[0084] Preferably, according to the invention, the multi-shaft screw machine is a twin-screw extruder with co-rotating parallel screw shafts rotating at equal speeds. These screw shafts are equipped with screw elements, each of which is preferably tightly meshed with the respective adjacent screw elements in the respective adjacent screw shafts. The outer surfaces of these screw shafts are surrounded by a housing having an inner profile that is also adapted to the screw shafts. The housing of a twin-screw extruder with screw shafts arranged parallel to each other can be designed to be heatable and coolable.

[0085] In addition, it is preferred according to the present invention that the multi-axis screw machine is a multi-axis extruder with co-rotating parallel screw shafts arranged in an annular manner and rotating at equal speeds. This multi-axis extruder has 8 to 16, usually 10 or 12 co-rotating screw shafts. In this screw machine, the screw shafts are also equipped with screw elements, and each screw element is preferably tightly meshed with the respective adjacent screw elements in the respective adjacent screw shafts. These screw shafts are arranged in an annular manner around an inner core having a profile that matches the screw shaft on which the screw elements are installed. Each screw shaft is adjacent to the other two screw shafts. The outer surfaces of these screw shafts are surrounded by an outer shell having an inner profile that is also compatible with the screw shaft. The outer shell and / or inner core of a multi-screw extruder with screw shafts arranged in an annular manner can be designed to be heatable and coolable.

[0086] In the context of the present invention, such a multi-screw extruder having screw shafts arranged in an annular manner relative to one another is also referred to below as annular extruder.

[0087] The screw elements of a ring extruder are no different from those of a twin-screw extruder, and are designed to solve the same process engineering goals. The processing area of ​​a ring extruder is also no different from that of a twin-screw extruder, and is designed to solve the same process engineering goals.

[0088] Ring extruders are known per se, for example:

[0089] DE4412725A1, DE4412741A1, DE19622582A1, DE202007004997U1, DE202007005010U1, WO03020493A1 and WO2006045412A2, and also the publication “Compoundieren mit Wellen” [“Compounding with Twelve Shafts”] Carl Hanser Verlag, Munich, KU Kunststoffe, volume 90 (2000) 8, pages 60-62.

[0090] The plastic body produced according to the method of the invention is in particular a melt of a formulation containing at least two thermoplastic components, at least one of which is a polycarbonate. The second thermoplastic component can also be a polycarbonate, but can also be a different thermoplastic polymer. The same is true for any other thermoplastic component. Each of these other thermoplastic components that can be used can be, independently of one another, a polycarbonate or a different thermoplastic polymer. Therefore, all thermoplastic components of the formulation of the invention can be polycarbonates.

[0091] In the context of the present invention, the formulation is present from the feed inlet of the multi-shaft screw machine up to a distance of two times the inner shell diameter upstream of the first screw element which is not a conveying element, and the plastic mass is present after the first screw element which is not a conveying element. In the length section of the multi-shaft screw machine covered by the conveying element, the formulation is converted into the plastic mass from a distance of two times the inner shell diameter up to a length region just before the end of the first screw element which is not a conveying element.

[0092] For the purposes of the present invention, "polycarbonate" refers to homopolycarbonates and copolycarbonates. These polycarbonates can be linear or branched in the usual manner. According to the invention, mixtures of polycarbonates can also be used.

[0093] In the polycarbonates used according to the invention, carbonate groups in a proportion of up to 80 mol %, preferably 20 mol % to 50 mol %, have preferably been replaced by aromatic dicarboxylic acid ester groups. Such polycarbonates in which acid moieties from carbonic acid and preferably from aromatic dicarboxylic acids are incorporated into the molecular chain are referred to as aromatic polyester carbonates.

[0094] The substitution of the carbonate groups by the aromatic dicarboxylate groups takes place essentially stoichiometrically and quantitatively, which means that the molar ratio of the coreactants is also reflected in the finished polyester carbonate.The aromatic dicarboxylate groups can be incorporated randomly or in blocks.

[0095] The average molecular weight Mw of thermoplastic polycarbonates (including thermoplastic polyester carbonates) is determined by GPC (gel permeation chromatography in dichloromethane with polycarbonate as standard) and is 15 to 50 kg / mol, preferably 20 to 35 kg / mol, more preferably 23 to 33 kg / mol.

[0096] Preferred aromatic polycarbonates and aromatic polyester carbonates are prepared in a known manner from diphenols, carbonic acid or carbonic acid derivatives, in the case of polyester carbonates, preferably aromatic dicarboxylic acids or dicarboxylic acid derivatives, optionally chain terminators and branching agents.

[0097] Details of the preparation of polycarbonates have been set out in numerous patent specifications over the past 40 years or so. Reference may be made here, for example, to Schnell “Chemistry and Physics of Polycarbonates”, Polymer Reviews, Vol. 9, Interscience Publishers, New York, London, Sydney 1964, to D. Freitag, U. Grigo, P. R. Müller, H. Nouvertné, Bayer AG, “Polycarbonates” in Encyclopedia of Polymer Science and Engineering, Vol. 11, 2nd edition, 1988, pp. 648-718, and finally to U. Grigo, K. Kirchner and P. R. Müller “Polycarbonate” in Becker / Braun, Kunststoff-Handbuch [Plastics Handbook], Vol. 3 / 1, “Polycarbonate, Polyacetale, Polyester, Celluloseester” [Polycarbonate, polyacetal, polyester, cellulose ester], Carl Hanser Verlag Munich, Vienna 1992, pp. 117-299.

[0098] For example, aromatic polycarbonates and polyester carbonates are prepared by reacting diphenols with carbonyl halides (preferably phosgene) and / or with aromatic dicarbonyl halides (preferably phthaloyl halides) by an interfacial process, optionally using a chain terminator and optionally using a trifunctional or higher branching agent; for the preparation of polyester carbonates, a portion of the carbonic acid derivatives is replaced by aromatic dicarboxylic acids or dicarboxylic acid derivatives, so that the carbonate structural units to be substituted in the aromatic polycarbonate are replaced by aromatic dicarboxylic acid ester structural units. It can also be prepared by reacting diphenols with, for example, diphenyl carbonate by means of a melt polymerization process.

[0099] Dihydroxyaryl compounds suitable for producing polycarbonates are those of formula (1)

[0100] HO-Z-OH(1)

[0101] in

[0102] Z is an aromatic group having 6 to 30 carbon atoms, may contain one or more aromatic rings, may be substituted, may contain aliphatic or alicyclic groups or alkyl aromatic groups or heteroatoms as bridging elements.

[0103] Preferably, Z in formula (1) is a part of formula (2)

[0104]

[0105] in

[0106] R6 and R7 independently represent H, C1 to C18 alkyl, C1 to C18 alkoxy, halogen such as Cl or Br or in each case optionally substituted aryl or aralkyl, preferably H or C1 to C12 alkyl, more preferably H or C1 to C8 alkyl, even more preferably H or methyl, and

[0107] X represents a single bond, -SO2-, -CO-, -O-, -S-, a C1 to C6 alkylene group, a C2 to C5 alkylidene group or a C5 to C6 cycloalkylene group, which may be substituted by a C1 to C6 alkyl group (preferably methyl or ethyl), or represents a C6 to C12 arylene group, which may be optionally fused to other aromatic rings containing heteroatoms.

[0108] Preferably, X represents a single bond, a C1 to C5 alkylene group, a C2 to C5 alkylene group or a C5 to C6 cycloalkylene group, -O-, -SO-, -CO-, -S-, -SO2-,

[0109] Or part of formula (2a)

[0110]

[0111] Examples of diphenols suitable for producing polycarbonates include hydroquinone, resorcinol, dihydroxybiphenyl, bis(hydroxyphenyl)alkanes, bis(hydroxyphenyl)cycloalkanes, bis(hydroxyphenyl)sulfides, bis(hydroxyphenyl)ethers, bis(hydroxyphenyl)ketones, bis(hydroxyphenyl)sulfones, bis(hydroxyphenyl)sulfides, bis(hydroxyphenyl)ethers, bis(hydroxyphenyl)ketones, bis(hydroxyphenyl)sulfones, bis(hydroxyphenyl)sulfides, bis(hydroxyphenyl)ethers, bis(hydroxyphenyl)ketones, bis(hydroxyphenyl)sulfones, bis(hydroxyphenyl)sulfoxides, α,α′-bis(hydroxyphenyl)diisopropylbenzene, benzopyrrolidines derived from derivatives of isatin or from derivatives of phenolphthalein, and ring-alkylated, ring-arylated and ring-halogenated compounds thereof.

[0112] Preferred bisphenols are 4,4'-dihydroxybiphenyl, 2,2-bis(4-hydroxyphenyl)-1-phenylpropane, 1,1-bis(4-hydroxyphenyl)phenylethane, 2,2-bis(4-hydroxyphenyl)propyl (bisphenol A (BPA)), 2,4-bis(4-hydroxyphenyl)-2-methylbutane, 1,3-bis[2-(4-hydroxyphenyl)-2-propyl]benzene (bisphenol M), 2,2-bis(3-methyl-4-hydroxyphenyl)propane, bis(3,5-dimethyl-4-hydroxyphenyl)methane, 2,2 -bis(3,5-dimethyl-4-hydroxyphenyl)propane, bis(3,5-dimethyl-4-hydroxyphenyl)sulfone, 2,4-bis(3,5-dimethyl-4-hydroxyphenyl)-2-methylbutane, 1,3-bis[2-(3,5-dimethyl-4-hydroxyphenyl)-2-propyl]benzene, 1,1-bis(4-hydroxyphenyl)cyclohexane and 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (bisphenol TMC (BPTMC)), and bisphenols of formula (IV) to (VI)

[0113]

[0114] wherein R' independently represents C1-C4-alkyl, aralkyl or aryl, preferably methyl or phenyl.

[0115] Particularly preferred bisphenols include 4,4'-dihydroxybiphenyl, 1,1-bis(4-hydroxyphenyl)phenylethane, 2,2-bis(4-hydroxyphenyl)propane (bisphenol A (BPA)), 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane and 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (bisphenol TMC (BPTMC)), as well as dihydroxy compounds of formula (IV), (V) and (VI), wherein R' independently represents a C1 to C4 alkyl, aryl or aromatic group, preferably a methyl or phenyl group.

[0116] These and other suitable diphenols are described, for example, in U.S. Pat. Nos. 3,028,635, 2,999,825, 3,148,172, 2,991,273, 3,271,367, 4,982,014, and 2,999,846, in DE-A 1570,703, 2,063,050, 2,036,052, 2,211,956, and 3,832,396, in FR-A 1,561,518, in the monograph "H. Schnell, Chemistry and Physics of Polycarbonates, Interscience Publishers, New York 1964" and in JP-A 62039 / 1986, JP-A 62040 / 1986 and JP A 105550 / 1986.

[0117] In the case of homopolycarbonates, only one diphenol is used; in the case of copolycarbonates, two or more diphenols are used. The diphenols used, like all other chemicals and auxiliaries added to the synthesis, may be contaminated by impurities arising during their own synthesis, handling and storage. However, it is advisable to use raw materials of the highest possible purity.

[0118] In particular, the polycarbonate of the present invention consists only of atoms of one or more elements selected from carbon (C), hydrogen (H), oxygen (O), nitrogen (N), sulfur (S), chlorine (Cl) and bromine (Br).

[0119] Examples of suitable carbonic acid derivatives include phosgene or diphenyl carbonate.

[0120] Suitable chain terminators useful in the preparation of polycarbonates are monophenols. Examples of suitable monophenols include phenol itself, alkylphenols (such as cresol, p-tert-butylphenol, cumylphenol) and mixtures thereof.

[0121] Preferred chain terminators are phenols which are mono- or polysubstituted by linear or branched, preferably unsubstituted, C1 to C30 alkyl or by tert-butyl. Particularly preferred chain terminators are phenol, cumylphenol and / or p-tert-butylphenol.

[0122] The chain terminators are preferably used in amounts of 0.1 to 5 mol %, based on the moles of diphenol used in each case. The chain terminators can be added before, during or after the reaction with the carbonic acid derivatives.

[0123] Suitable branching agents are the trifunctional or higher functional compounds known from polycarbonate chemistry, in particular compounds having three or more phenolic hydroxyl groups.

[0124] Examples of suitable branching agents include 1,3,5-tris(4-hydroxyphenyl)benzene, 1,1,1-tris(4-hydroxyphenyl)ethane, tris(4-hydroxyphenyl)phenylmethane, 2,4-bis(4-hydroxyphenylisopropyl)phenol, 2,6-bis(2-hydroxy-5'-methylbenzyl)-4-methylphenol, 2-(4-hydroxyphenyl)-2-(2,4-dihydroxyphenyl)propane, tetrakis(4-hydroxyphenyl)methane, tetrakis(4-(4-hydroxyphenylisopropyl)phenoxy)methane and 1,4-bis((4',4"-dihydroxytriphenyl)methyl)benzene and 3,3-bis(3-methyl-4-hydroxyphenyl)-2-oxo-2,3-dihydroindole.

[0125] The amount of branching agents optionally used is preferably from 0.05 mol % to 2.00 mol %, based on the moles of diphenol used in each case.

[0126] The branching agent can be initially charged together with the diphenol and the chain terminator in the alkaline aqueous phase or it can be added as a solution in an organic solvent before the phosgenation. In the transesterification process, the branching agent is used together with the diphenol.

[0127] Particularly preferred polycarbonates are homopolycarbonates based on bisphenol A, homopolycarbonates based on 1,3-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, and copolycarbonates based on monomers of the following aspects: on the one hand, the monomer bisphenol A, and on the other hand, monomers selected from the group consisting of 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane and diphenols of the formula (IV) to (VI)

[0128]

[0129] wherein R' independently represents a C1 to C4 alkyl group, an aralkyl group or an aryl group, preferably a methyl group or a phenyl group.

[0130] Preferred processes for producing the polycarbonates (including polyester carbonates) used according to the invention are the known interfacial processes and the known melt transesterification processes (see, for example, WO 2004 / 063249 A1, WO 2001 / 05866 A1, WO 2000 / 105867, US Pat. No. 5,340,905 A, US Pat. No. 5,097,002 A, US Pat. No. 5,717,057 A).

[0131] The most preferred polycarbonates are aromatic polycarbonates based on bisphenol A, especially linear aromatic polycarbonates based on bisphenol A.

[0132] The proportion of polycarbonate in the formulation for producing the plastic body is 20 to 98% by weight, in particular 40 to 80% by weight.

[0133] If one of the at least two thermoplastic components in the formulation of the invention is not a polycarbonate, or possibly, the other thermoplastic components in the formulation of the invention are not polycarbonates, the other thermoplastic component or possibly the other thermoplastic components are independently selected from the following:

[0134] Polyester carbonates, polyamides, polyesters (especially polybutylene terephthalate and polyethylene terephthalate), polylactic acid, polyethers, thermoplastic polyurethanes, polyacetals, fluoropolymers (especially polyvinylidene fluoride), polyether sulfones, polyolefins (especially polyethylene and polypropylene), polyimides, polyacrylates (especially polymethyl (meth)acrylate), polyphenylene ethers, polyphenylene sulfides, polyether ketones, polyarylether ketones, styrene polymers (especially polystyrene), styrene copolymers (especially styrene-acrylonitrile copolymers), rubber-modified vinyl (co)polymers and polyvinyl chloride.

[0135] If the thermoplastic component present in the formulation is one or two or more thermoplastic components which are not polycarbonates, it is preferred according to the present invention that these thermoplastic components are selected from rubber-modified vinyl (co)polymers.

[0136] In other words: In a specific embodiment of the present invention, the formulation for producing a plastic body, in addition to at least one thermoplastic component which is a polycarbonate (also generally referred to herein as component A), also contains at least one thermoplastic component which is a rubber-modified vinyl (co)polymer, also referred to herein as component B.

[0137] The rubber-modified vinyl (co)polymers preferably used according to the invention contain a rubber-based graft polymer and optionally a rubber-free vinyl (co)polymer.

[0138] According to the present invention, the graft polymer used in component B comprises:

[0139] B.1 5 to 95% by weight, preferably 20 to 92% by weight, in particular 30 to 91% by weight, of at least one vinyl monomer, based on the graft polymer.

[0140] B.2 95 to 5% by weight, preferably 80 to 8% by weight, in particular 70 to 9% by weight, of one or more rubber-elastic graft substrates, based on the graft polymer, having a glass transition temperature of <-50°C, more preferably <-60°C, particularly preferably <-70°C.

[0141] Unless expressly stated otherwise in the present invention, the glass transition temperatures of all components were determined in accordance with DIN EN 61006 (1994 edition) by differential scanning calorimetry (DSC) with a heating rate of 10 K / min and the midpoint temperature was determined as Tg (tangent method).

[0142] The median particle size (D50) of the graft base B.2 is generally from 0.05 to 10.00 μm, preferably from 0.1 to 5.0 μm, more preferably from 0.2 to 1.5 μm.

[0143] The median particle size D50 is the diameter above which 50% by weight of the particles are present and below which 50% by weight of the particles are present. Unless otherwise expressly stated in the present invention, it is determined for all components by means of ultracentrifugation measurement (W. Scholtan, H. Lange, Kolloid, Z. und Z. Polymere 250 (1972), 782-1796).

[0144] Monomer B.1 is preferably a mixture of the following substances:

[0145] B.1.1 65 to 85% by weight, more preferably 70 to 80% by weight, further preferably 74 to 78% by weight of vinyl aromatics and / or ring-substituted vinyl aromatics (e.g. styrene, α-methylstyrene, p-methylstyrene, p-chlorostyrene) and / or

[0146] or (C1-C8)-alkyl (meth)acrylates (e.g. methyl methacrylate, ethyl methacrylate), each based on the sum of B.1.1 and B.1.2, and

[0147] B.1.2 15% to 35% by weight, more preferably 20% to 30% by weight, further preferably 22%

[0148] up to 26% by weight of vinyl cyanides (unsaturated nitriles such as acrylonitrile and methacrylonitrile) and / or (C1-C8)alkyl (meth)acrylates (such as methyl methacrylate, n-butyl acrylate, tert-butyl acrylate) and / or derivatives of unsaturated carboxylic acids (such as anhydrides and imides, for example maleic anhydride), each based on the sum of B.1.1 and B.1.2.

[0149] Preferred monomers B.1.1 are selected from at least one of the monomers styrene, α-methylstyrene and methyl methacrylate; preferred monomers B.1.2 are selected from at least one of the monomers acrylonitrile, maleic anhydride and methyl methacrylate. Particularly preferred monomers are B.1.1 styrene and B.1.2 acrylonitrile. Optional preferred monomers are B.1.1 methyl methacrylate and B.1.2 methyl methacrylate.

[0150] Suitable graft substrates B.2 for the graft polymers include, for example, diene rubbers, EP(D)M rubbers (ie those based on ethylene / propylene and optionally dienes), acrylates, polyurethanes, silicones, chloroprene, ethyl acetate, vinyl acetate and acrylate-silicone composite rubbers.

[0151] Preferred graft substrates B.1.2 are diene rubbers, which preferably contain butadiene, or copolymers of dienes, which preferably contain butadiene, and further copolymerizable vinyl monomers (eg according to B.1.1 and B.1.2) or mixtures of one or more of the abovementioned components.

[0152] Particularly preferred graft substrates B.2 are pure polybutadiene rubbers. In a further preferred embodiment, B.2 is a styrene-butadiene rubber, more preferably a styrene-butadiene block copolymer rubber.

[0153] The gel content of the graft base B.2 is at least 30% by weight, preferably at least 40% by weight, in particular at least 60% by weight, in each case based on B.2 and measured as the fraction insoluble in toluene.

[0154] The gel content of the grafted substrate B.2 / the gel content of the grafted polymer in component B is the content of insoluble matter in suitable solvents, measured at 25° C. (M. Hoffmann, H. R. Kuhn, Polymeranalytik I and II, Georg Thieme-Verlag, Stuttgart 1977).

[0155] Suitable polymers for component B are, for example, those described in DE-A 2035 390 (= US Pat. No. 3,644,574), or DE-A 2248 242 (= GB-A 1 409 275), or Ullmanns ABS polymers or MBS polymers described in der Technischen Chemie [Ullmann's Encyclopedia of Industrial Chemistry], volume 19 (1980), page 280 et seq.

[0156] The graft copolymers in component B are produced by free-radical polymerization, for example by emulsion, suspension, solution or bulk polymerization. Mixtures of graft polymers produced by different processes can also be used as component B.

[0157] When the graft polymer B is produced in an emulsion polymerization, it comprises

[0158] B.1 5 to 75% by weight, preferably 20 to 60% by weight, more preferably 25 to 50% by weight, of at least one vinyl monomer, based on the graft polymer,

[0159] B.2 95 to 25% by weight, preferably 80 to 40% by weight, more preferably 75 to 50% by weight, of one or more rubber-elastic graft substrates, based on the graft polymer, having a glass transition temperature of <-50°C, more preferably <-60°C, particularly preferably <-70°C.

[0160] The median particle size (D50) of the graft base B.2 of the graft polymer B produced in the emulsion polymerization is from 0.05 to 2.00 μm, preferably from 0.1 to 1.0 μm, more preferably from 0.2 to 0.5 μm.

[0161] The gel content of the graft polymer B produced in the emulsion polymerization, measured in acetone as solvent, is preferably at least 30% by weight, more preferably at least 60% by weight, further preferably at least 80% by weight.

[0162] The graft polymer B is produced in suspension, solution or bulk polymerization and comprises:

[0163] B.1 80% to 95% by weight, preferably 84% to 92% by weight, more preferably 87% to 91% by weight, of at least one vinyl monomer, based on the graft polymer,

[0164] B.2 20 to 5% by weight, preferably 16 to 8% by weight, more preferably 13 to 9% by weight, of one or more rubber-elastic graft substrates, based on the graft polymer, having a glass transition temperature of <-50°C, more preferably <-60°C, particularly preferably <-70°C.

[0165] The median particle size (D50) of the graft base B.2 of the graft polymer B produced in suspension, solution or bulk polymerization is from 0.3 to 10.00 μm, preferably from 0.4 to 5.0 μm, more preferably from 0.5 to 1.5 μm.

[0166] The gel content of the graft polymer B produced in suspension, solution or bulk polymerization, measured in acetone as solvent, is preferably from 10 to 50% by weight, more preferably from 15 to 40% by weight, further preferably from 18 to 30% by weight.

[0167] Particularly suitable graft polymers produced by the emulsion polymerization process are, for example, ABS polymers produced according to US Pat. No. 4,937,285 in an emulsion polymerization process by redox initiation using an initiator system consisting of an organic hydroperoxide and ascorbic acid.

[0168] Other particularly suitable graft polymers produced in the emulsion polymerization process are MBS modifiers having a core-shell structure.

[0169] Component B may contain free vinyl (co)polymers composed of the monomers described in B.1, i.e. in a form which is not chemically bonded to the rubber substrate and is not contained in the rubber particles. This may be present in component B as a result of production in the polymerization of the grafted polymer (the grafting on the grafted substrate is not always complete), or it may also be incorporated into component B as a result of a separate polymerization. It is also possible that part of the free vinyl (co)polymers in component B originate from the grafted polymer itself as a result of production, while another part of the free vinyl (co)polymers may be added to component B in the presence of a separate polymerization. The proportion of free vinyl (co)polymers (regardless of their origin) in component B (calculated as acetone-soluble fraction) is preferably at least 5% by weight, more preferably at least 30% by weight, particularly preferably at least 50% by weight (by weight), based on component B.

[0170] The weight average molecular weight Mw of this free vinyl (co)polymer in the rubber-modified vinyl copolymer according to component B is from 30 to 250 kg / mol, preferably from 70 to 200 kg / mol, in particular from 90 to 180 kg / mol.

[0171] In the context of the present invention, the weight average molecular weight Mw of the free vinyl (co)polymer in component B is determined by gel permeation chromatography (GPC) in tetrahydrofuran relative to polystyrene standards.

[0172] The formulation for producing the plastic body may comprise at least two thermoplastic components, in pure form or in a mixture with fillers and reinforcing agents, such as, in particular, glass fibers or talc.

[0173] In a preferred embodiment, one or more additives are added to the formulation. The specific additive may be a solid, liquid or solution and may be added to the multi-shaft screw machine together with the formulation, optionally with one additional additive or two or more additional additives (if present), or fed to the multi-shaft screw machine via a separate side stream.

[0174] Additives can impart various properties to polymers. For example, these additives can be colorants, pigments, processing aids, fillers, antioxidants, reinforcing agents, UV absorbers and light stabilizers, metal deactivators, peroxide scavengers, alkaline stabilizers, nucleating agents, benzofurans and indolones with stabilizing or antioxidant effects, mold release agents, flame retardant additives, antistatic agents, dyes and melt stabilizers. Examples of these additives are carbon black, glass fibers, clay, mica, graphite fibers, titanium dioxide, carbon fibers, carbon nanotubes, ionic liquids and natural fibers. Suitable additives are described, for example, in WO 99 / 55772, pages 15-25; "Plastics Additives", R. and H. Müller, Hanser Publishers 1983; "Additives for Plastics Handbook, John Murphy, Elsevier, Oxford 1999"; "Plastics Additives Handbook, Hans Zweifel, Hanser, Munich 2001".

[0175] Preferably, according to the present invention, an additive that is free-flowing at 23°C may be added to the plastic body, or a plurality of additives that are free-flowing at 23°C, such as two, three or four such additives that are free-flowing at 23°C may be added to the plastic body.

[0176] According to the invention, phosphorus-containing flame retardants are particularly preferred as free-flowing additives at 23° C.

[0177] In the context of the present invention, the phosphorus-containing flame retardant is preferably selected from mono- and oligomeric phosphoric and phosphonic esters, phosphazenes and hypophosphites, and mixtures of various compounds selected from one or more of these groups may also be used as flame retardants. Other phosphorus compounds not specifically mentioned here may also be used, either alone or in any desired combination with other phosphorus compounds.

[0178] Preferred mono- and oligomeric phosphoric and phosphonic esters are phosphorus compounds of the general formula (III),

[0179]

[0180] in

[0181] R1, R2, R3 and R4 are each independently optionally halogenated C1 to C8-alkyl, each optionally alkyl-substituted (preferably C1 to C4-alkyl-substituted) and / or halogen-substituted (preferably chlorine- or bromine-substituted) C5 to C6-cycloalkyl, C6 to C20-aryl or C7 to C12-aralkyl,

[0182] n is independently 0 or 1

[0183] q is 0 to 30, and

[0184] X is a monocyclic or polycyclic aromatic group having 6 to 30 carbon atoms, or a linear or branched aliphatic group having 2 to 30 carbon atoms, which may be substituted by a hydroxyl group and may contain up to 8 ether bonds.

[0185] Preferably, R1, R2, R3 and R4 independently represent C1 to C4-alkyl, phenyl, naphthyl or phenyl-C1-C4-alkyl. Aryl R1, R2, R3 and R4 can be substituted by halogen and / or alkyl accordingly, preferably chlorine, bromine and / or C1 to C4 alkyl. Particularly preferred aryl is tolyl, phenyl, xylyl, propylphenyl or butylphenyl and corresponding bromo and chloro derivatives thereof.

[0186] X in formula (III) is a monocyclic or polycyclic aromatic radical preferably having 6 to 30 carbon atoms. The latter is preferably derived from diphenols.

[0187] n in formula (III) can independently be 0 or 1; n is preferably 1.

[0188] q is a value from 0 to 30. When mixtures of different components of the formula (III) are used, the mixtures may preferably have a number-average q value of from 0.3 to 10, more preferably from 0.5 to 10, in particular from 1.05 to 1.4.

[0189] X is more preferably

[0190]

[0191] or a chlorinated or brominated derivative thereof; in particular, X is derived from resorcinol, hydroquinone, bisphenol A or diphenylphenol. Particularly preferably, X is derived from bisphenol A.

[0192] According to the invention, monophosphates (q=0), oligophosphates (q=1-30) or mixtures of monophosphates and oligophosphates can be used as component C.

[0193] The monophosphorus compound of the formula (III) is in particular tributyl phosphate, tris(2-chloroethyl) phosphate, tris(2,3-dibromopropyl) phosphate, triphenyl phosphate, tricresyl phosphate, diphenylcresyl phosphate, diphenyloctyl phosphate, diphenyl 2-ethylcresyl phosphate, tri(isopropyl) phosphate, halogenated aryl phosphates, dimethyl methylphosphonate, diphenyl methylphosphonate, diethyl phenylphosphonate, triphenylphosphine oxide or trihydroxytolylphosphine oxide.

[0194] The most preferred component D is a bisphenol-based oligophosphate of formula (IIIa):

[0195]

[0196] The phosphorus compounds of the formula (III) are known (see, for example, EP-A 363 608, EP-A 640 655) or can be prepared in an analogous manner by known methods (eg Ullmanns der technischen Chemie, volume 18, page 301 et seq. 1979; Houben-Weyl, Methoden der organischen Chemie [Methods of Organic Chemistry], volume 12 / 1, page 43; Beilstein, volume 6, page 177). A specific example of a phosphorus-containing compound selected from the formula (III) is bisphenol A bis(diphenyl phosphate), also referred to as BDP for short. This BDP is also a preferred additive as a free-flowing additive at 23° C.

[0197] The average q value can be determined by measuring the composition (molecular weight distribution) of the phosphate mixture using a suitable method (gas chromatography (GC)), high pressure liquid chromatography (HPLC), gel permeation chromatography (GPC)) and calculating the average q from this.

[0198] Phosphazenes are compounds of the formulae (IVa) and (IVb).

[0199]

[0200] in

[0201] R is identical or different at each occurrence and is amino, each optionally halogenated (preferably fluorinated) C1- to C8-alkyl, or C1- to C8-alkoxy, each optionally alkyl-substituted (preferably C1- to C4-alkyl-substituted) and / or halogen-substituted (preferably chloro- and / or bromo-substituted) C5- to C6-cycloalkyl, C6- to C20-aryl (preferably phenyl or naphthyl), C6- to C20-aryloxy (preferably phenoxy, naphthoxy), or C7- to C12-aralkyl (preferably phenyl-C1-C4-alkyl),

[0202] k is 0 or a number from 1 to 15, preferably a number from 1 to 10.

[0203] Examples include propoxyphosphazene, phenoxyphosphazene, methylphenoxyphosphazene, aminophosphazene and fluoroalkylphosphazene. Phenoxyphosphazene is preferred.

[0204] Phosphazenes can be used alone or as a mixture. The R groups in formula (IVa) and formula (IVb) can always be the same, or two or more groups can be different. Phosphazenes and their production are described in EP-A 728 811, DE-A 1961668 and WO 97 / 40092.

[0205] In the context of the present invention, phosphonates are understood to mean salts of phosphonic acid with any metal cation. Mixtures of salts in which the metal cations are different can also be used. The metal cation is a salt of the first main group of the periodic table (alkali metals, preferably Li + 、Na + , K + ), Group 2 (alkaline earth metals, preferably Mg 2+ , Ca 2+ , Sr 2+ , Ba 2+ , more preferably Ca 2+ ) or Group 3 (boron elements, preferably Al 3+ ) and / or transition group 2, 7 or 8 (preferably Zn 2+ , Mn 2+ , Fe 2+ , Fe 3+ ) of metal cations.

[0206] Preferably, a phosphonate or a mixture of salts of the formula (V) is used

[0207]

[0208] Among them, M m+ It is a metal cation of the 1st main group (metal cation of an alkali metal; m=1), the 2nd main group (alkaline earth metal; m=2) or the 3rd main group (m=3) or transition groups 2, 7 or 8 (wherein m is an integer from 1 to 6, preferably from 1 to 3, more preferably 2 or 3) of the periodic table.

[0209] More preferably, in formula (V),

[0210] When m=1, the metal cation M + =Li + 、Na + , K + ,

[0211] When m=2, the metal cation M 2+ =Mg 2+ , Ca 2+ , Sr 2+ , Ba 2+ ,as well as

[0212] When m=3, the metal cation M 3+ =Al3+ ; The first choice is

[0213] Preferred Ca 2+ (m=2).

[0214] In a preferred embodiment, the median particle size d50 of the phosphonate (component C) is less than 80 μm, preferably less than 60 μm; d50 is more preferably between 10 μm and 55 μm. The median particle size d50 refers to the diameter above which the particles account for 50% by weight (and below which the particles also account for 50% by weight). Mixtures of salts having different median particle sizes d50 can also be used.

[0215] Furthermore, according to the invention, the free-flowing and particularly preferred additive according to the invention at 23° C. is preferably added to the plastic mass via a side stream from the last conveying element before the first screw element which is not a conveying element. More preferably, the free-flowing and particularly preferred additive according to the invention at 23° C. is added to the plastic mass downstream of the last conveying element before the first screw element which is not a conveying element. Most preferably, the free-flowing and particularly preferred additive according to the invention at 23° C. is added to the plastic mass downstream of the melting zone.

[0216] Examples of suitable antioxidants / heat stabilizers include:

[0217] Alkylated monophenols, alkylthiomethylphenols, hydroquinone and alkylated hydroquinones, tocopherols, hydroxylated thiodiphenyl ethers, alkylene bisphenols, O-, N- and S-benzyl compounds, hydroxybenzylated malonic esters, aromatic hydroxybenzyl compounds, triazine compounds, acylaminophenols, esters of β-(3,5-tert-butyl-4-hydroxy-3-methylphenyl)propionic acid, esters of β-(5-tert-butyl-4-hydroxy-3-methylphenyl)propionic acid, esters of β-(3,5-dicyclohexyl-4-hydroxyphenyl)propionic acid, esters of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid, amides of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, suitable thiosynergists, secondary antioxidants, phosphites and phosphonites, benzofuranones and indolones.

[0218] Preference is given to organic phosphites, phosphonates and phosphanes in which the majority of the organic moieties consists completely or partly of optionally substituted aryl groups.

[0219] Suitable complexing agents for heavy metals and for neutralizing traces of alkali are orthophosphoric acid and metaphosphoric acid, fully or partially esterified phosphates or phosphites.

[0220] Suitable light stabilizers (UV absorbers) are 2-(2'-hydroxyphenyl)benzotriazole, 2-hydroxybenzophenone, esters of substituted and unsubstituted benzoic acids, acrylates, hindered amines, oxalamides and 2-(hydroxyphenyl)-1,3,5-triazines and substituted hydroxyalkoxyphenyl-1,3,5-triazoles, preferably substituted benzotriazoles, for example 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)benzotriazole, benzotriazole, 2-(2'-hydroxy-3',5'-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole, 2-[2'-hydroxy-3'-(3",4",5",6"-tetrahydrophthalimidoethyl)-5'-methylphenyl]benzotriazole and 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol].

[0221] Polypropylene glycol can be used alone or in combination with, for example, sulfones or sulfonamides as stabilizers to counteract gamma ray damage.

[0222] These and other stabilizers may be used alone or in combination and may be added to the formulation according to the invention in the form described.

[0223] Processing aids such as mold release agents may also be added, mainly derivatives of long-chain fatty acids. Preferably, for example, pentaerythritol tetrastearate and glyceryl monostearate. They may be used alone or as a mixture.

[0224] Suitable flame retardant additives are phosphates, ie triphenyl phosphate, resorcinol diphosphate, brominated compounds such as brominated phosphates, brominated oligocarbonates and polycarbonates, preferably salts of fluorinated organic sulfonic acids.

[0225] Suitable impact modifiers are butadiene rubber grafted onto styrene-acrylonitrile or methyl methacrylate, ethylene-propylene rubber grafted onto maleic anhydride, ethyl acrylate and butyl acrylate rubber grafted onto methyl methacrylate or styrene-acrylonitrile, interpenetrating networks of siloxanes and acrylates grafted onto methyl methacrylate or styrene-acrylonitrile.

[0226] Furthermore, colorants such as organic dyes or pigments or inorganic pigments, infrared absorbers, which may be used alone, as a mixture or in combination with stabilizers, glass fibers, (hollow) glass beads and inorganic (especially mineral) fillers, these mineral fillers also include reinforcing fillers, especially titanium dioxide (TiO2), talc (Mg3Si4O10 (OH)2), dolomite CaMg[CO3]2, kaolinite Al4[(OH)8|Si4O 10 ] and wollastonite Ca3[Si3O9], and very particularly titanium dioxide (TiO2) and talc (Mg3Si4O 10 (OH)2).

[0227] The plastic bodies produced according to the invention can be used in any known plastic bodies containing at least two thermoplastic components, at least one of which is a polycarbonate.

[0228] The invention also provides a plastic body produced by the process according to the invention.

[0229] The invention also provides for the use of the plastic bodies produced according to the invention for producing shaped articles.

[0230] The plastic bodies produced according to the invention can be used to produce any kind of shaped articles. For example, they can be produced by injection molding, extrusion and blow molding processes. Another form of processing is to produce molded articles by thermoforming from previously produced sheets or films.

[0231] Examples of such shaped articles which can be produced from the formulations and plastic bodies according to the invention are films, profiles, various housing parts, for example for household appliances such as juicers, coffee machines, mixers, etc.; for office equipment such as displays, flat-panel displays, notebook computers, printers, copiers, etc.; for sheets, pipes, electrical installation pipes, windows, doors and other profiles for the construction industry (interior decoration and exterior applications), as well as electrical and electronic components such as switches, plugs and sockets, and parts for commercial vehicles, in particular for the automotive industry. The formulations and plastic bodies according to the invention are also suitable for the production of the following shaped articles or moldings: ships, aircraft, buses and other motor vehicles, body parts for motor vehicles, housings for electrical equipment equipped with small transformers, housings for information processing and transmission equipment, housings and panels for medical equipment, massage equipment and housings thereof, children's toy vehicles, sheet-like wall parts, housings for safety equipment, insulated transport boxes, moldings for sanitary and bathroom equipment, protective grilles for ventilation openings and housings for gardening equipment.

[0232] The present invention will be explained below in conjunction with embodiments, but it is not intended that the present invention is limited to these embodiments. Example

[0233] Determination of average residence times t1 and t2

[0234] The average residence times t1 and t2 in the extruder are determined as described below.

[0235] First, set the desired speed on the extruder and feed all the components of the formulation into the extruder at the desired positions and at the desired throughput. 10 minutes after all the components of the formulation were added, manually feed 1 gram of tracer granules (Makrolon 2805, color 901510 [corresponding to black]) into the extruder as a pulse tracer per 50 kg / h total formulation throughput.

[0236] To determine the mean residence time t1 in the case of a formulation containing no additives which are free-flowing at 23°C, the tracer pellets were added to the opening of the extruder housing at a distance of twice the inner diameter of the housing (2D) upstream of the first screw element which is not a conveying element.

[0237] In the case of formulations containing an additive free-flowing at 23° C., to determine the mean residence time t2, the tracer pellets were added to an opening of the extruder housing axially parallel to the point of addition of the additive free-flowing at 23° C.

[0238] In the case of a formulation containing an additive that is free-flowing at 23°C, the residence time t1 is calculated by subtracting the residence time when the tracer particles are added at a housing opening 2D upstream of the first screw element that is not a conveying element from the residence time when the tracer is added at a housing opening axially parallel to the addition point of the additive that is free-flowing at 23°C.

[0239] Simultaneously with the addition of the tracer pellets, the time measurement begins.

[0240] An online spectrophotometer (COLVISTEC InSpectro X2) was used to measure the intensity of the tracer in the plastic mass at the flange directly downstream of the end of the extruder shaft.

[0241] For this purpose, for plastic bodies with an average transmittance of less than 40% in the wavelength range from 400 nm to 800 nm, a measuring probe is installed in the flange and the measurement is carried out as reflectance; however, for all other plastic bodies, two measuring probes opposite each other are placed in the flange and the measurement is carried out as transmittance. Each measuring probe is connected to a spectrophotometer via a glass fiber conduit. The spectrophotometer is used to measure and record the color spectrum of the plastic body from 230 nm to 800 nm every second for 5 minutes starting from the addition of the tracer, and the L value (lightness; according to CIE LAB) is calculated.

[0242] The mean residence time is calculated from the cumulative function of the distribution curve of the L values ​​using the ReTA evaluation program from COLVISTEC. To determine the mean residence time for an experimental setup, the mean value is determined from 3 measurements in each case. However, other suitable software packages can also be used to determine the mean residence time from the distribution curve of the L values.

[0243] Melting temperature measurement

[0244] In all experiments, the melt temperature of the plastic body was measured by inserting a thermocouple into the intermediate melt strand emerging from the extruder or, in case of an even number of nozzle holes, directly at the exit of the nozzle bar by inserting a thermocouple into one of the two intermediate melt strands.

[0245] Measurement of unmelted particles

[0246] To evaluate the quality of plasticization, for each experimental setup, 330 pellets were randomly selected from the total number of pellets produced in each experiment, and the number of pellets containing at least one unmelted particle among these 330 pellets was determined. For this purpose, in each case, 110 pellets were laid on a light box with their cut edges arranged at right angles to the light box. Subsequently, a cardboard roll with a diameter of about 4 cm was placed around the pellets. A digital camera was placed on the top of the roll. The exposure and focus were set on the camera so that the top side of the pellets was clearly imaged and the unmelted particles formed a good contrast with the plastic body. Figure 1 The pictures taken in this way are shown as examples.

[0247] The pictures taken with a digital camera were visually inspected on a monitor to check for unmelted particles in the pellets. When evaluating the images, a distinction was made between cavitation bubbles and unmelted particles. Unmelted particles differ from cavitation bubbles in shape and position. Cavitation bubbles are usually located in the center of the pellet, while unmelted particles are located outside the center. Cavitation bubbles are usually oval or elongated, while unmelted particles are much narrower and usually have a sickle shape. Figure 2 Cavitation and unmelted particles are distinguished by way of example. 2.1.1, 2.1.2, 2.1.3 and 2.1.4 represent granular materials with cavitation; 2.1.1.1, 2.1.2.1, 2.1.3.1 and 2.1.4.1 represent cavitation in these granular materials; 2.2.1, 2.2.2, 2.2.3 and 2.2.4 represent granular materials with unmelted particles; 2.2.1.1, 2.2.1.2, 2.2.2.1, 2.2.2.2, 2.2.3.1, 2.2.3.2, 2.2.4.1 and 2.2.4.2 represent unmelted particles in these granular materials.

[0248] exist Figure 3 In, from Figure 1In the photo, the pellets with cavitation are marked as (3.1) and the pellets with unmelted particles are marked as (3.2).

[0249] If the digital photograph does not allow the distinction between cavitation and unmelted particles, the pellets are examined visually one by one. Here, a clear distinction can be made between unmelted particles and cavitation: cavitation is always a hole, while unmelted particles are transparent inclusions that extend across the entire length of the pellet in the direction of strand extraction. If a pellet containing unmelted particles is held up to light, a clear light reflection will occur. This light reflection does not occur in the presence of cavitation, since the cavitation is filled only with gas.

[0250] For the assessment of plasticization quality, the number of pellets containing at least one unmelted particle was calculated based on the total number of pellets examined per experimental setup, ie 330. 5 pellets containing unmelted particles therefore means 5 / 330 = 1.5% unmelted particles.

[0251] Example 1-6: Mass flow rate and process parameter changes of screw shaft speed n

[0252] In Examples 1 to 6, a ZE60B UTXi twin-screw extruder from KraussMaffei Extrusion was used to produce the plastic bodies. The design features of the extruder can be found in Table 1, columns k to n. Figure 4 The basic structure of the extruder used in Examples 1-6 is shown.

[0253] In Examples 1-6, all components of the formulations were measured by a conventional gravimetric differential metering balance and fed into the main feed port of the screw machine housing 2 via a feed hopper 1 (as shown in the figure).

[0254] The delivery zone for all components of the formulation is in the region of the housings 2 to 7 .

[0255] The plasticizing zone is in the region of the housing 8, whose screw structure consists of various two- and three-stage kneading blocks with different widths and toothed mixing elements.

[0256] Mixing takes place in the region of the housings 9 to 10, whose screw structure consists of kneading elements, toothed mixing elements and conveying elements.

[0257] In the housing part 11 there is a ventilation opening 13 which is connected to an extraction device (not shown).

[0258] The pressurized zone is in the housing 12, downstream of which is a nozzle plate having 29 holes.

[0259] In Examples 1 to 6, granulation was carried out in the form of strand granulation after cooling in a water bath.

[0260] The formulation fed into the extruder in Examples 1-6 consisted of the following mixture:

[0261] - 60.3% by weight of granules of linear polycarbonate based on bisphenol A, relative viscosity η rel

[0262] =1.28 (measured at 25°C and 0.5 g / 100 ml concentration with CH2Cl2 as solvent); and

[0263] - 17.2 wt% of emulsion-type ABS granules, containing A:B:S in a weight ratio of 20:24:56, and

[0264] - 8.9 wt% of bulk ABS granules containing A:B:S in a weight ratio of 25:10:65, and

[0265] - 9.5% by weight of styrene-acrylonitrile copolymer (SAN) having an A:S weight ratio of 24:76, and

[0266] 4.1% by weight of a powder mixture containing 3% by weight of an emulsion ABS graft in powder form with an A:B:S weight ratio of 12:58:30, and 0.35% by weight of a stabilizer and 0.75% by weight of a mold release agent.

[0267] In comparative examples 1 and 2 and inventive examples 3 to 6, the formulations were mixed according to the following parameters as given in Table 1: screw shaft speed (Table 1, column p), mass flow rate (Table 1, column o) and the resulting specific mechanical energy input (Table 1, column q) and the temperature of the melt flowing out of the nozzle plate (Table 1, column r). Table 1 also gives the amount of pellets containing unmelted particles thus obtained (Table 1, column w).

[0268] As shown in Examples 1-6, regardless of the rate or mass flow rate selected for the formulation, the plastic body of the present invention is always obtained at a melting rate (Table 1, column x) of at least 1.18, especially at least 1.23, however, in the case of a melting rate of less than 1.18, especially in the case of a melting rate of 1.08 or less, the amount of pellets containing unmelted particles is unacceptable.

[0269] Example 7-19: Changes in viscosity ratio dh1 and dh2

[0270] In Examples 7 to 19, a ZE60B UTXi twin-screw extruder from KraussMaffei Extrusion GmbH was used to produce the plastic bodies. The design features of the extruder can be found in Table 1, columns k to n. Figure 4 The basic structure of the extruder used in Examples 7-19 is shown.

[0271] In Examples 7-10, all ingredients of the formulations were measured by a conventional gravimetric differential metering balance and fed into the main feed port of the screw machine housing 2 via a feed hopper 1 (as shown in the figure).

[0272] The delivery zone for all components of the formulation is in the region of the housings 2 to 7 .

[0273] The plasticizing zone is in the region of the housing 8, whose screw structure consists of various two- and three-stage kneading blocks with different widths and toothed mixing elements.

[0274] The mixing zone is in the region of the housings 9 to 10 , whose screw structure consists of kneading elements, toothed mixing elements and conveying elements.

[0275] In the housing part 11 there is a ventilation opening 13 which is connected to an extraction device (not shown).

[0276] The pressurized zone is in the housing 12, downstream of which is a nozzle plate having 29 holes.

[0277] In Examples 7 to 10, granulation was carried out in the form of strand granulation after cooling in a water bath.

[0278] The formulation fed into the extruder in Examples 7-10 consisted of the following mixture:

[0279] - 76% by weight of granules of linear polycarbonate based on bisphenol A, relative viscosity η rel =1.28 (measured at 25°C and 0.5 g / 100 ml concentration with CH2Cl2 as solvent); and

[0280] - 3.96 wt% of bulk ABS granules containing A:B:S in a weight ratio of 25:10:65, and

[0281] -24.74 wt% of bulk ABS granules containing A:B:S in a weight ratio of 21:10:69 and

[0282] 2.04% by weight of a powder mixture containing 1% by weight of an emulsion-type ABS graft in powder form containing an A:B:S weight ratio of 12:58:30, as well as 0.3% by weight of a stabilizer and 0.74% by weight of a mold release agent.

[0283] The average specific heat capacity of the plastic bodies in Examples 7-10 is shown in column h of Table 1.

[0284] In comparative examples 7 and 8 and inventive examples 9 to 10, the formulations were mixed according to the following parameters as given in Table 1: screw shaft speed (Table 1, column p), mass flow rate (Table 1, column o) and the resulting specific mechanical energy input (Table 1, column q) and the temperature of the melt flowing out of the nozzle plate (Table 1, column r). Table 1 also gives the amount of pellets containing unmelted particles thus obtained (Table 1, column w).

[0285] In Examples 11-14, all ingredients of the formulation, except the additives which flow freely at 23°C, were metered by a conventional gravimetric differential metering balance and fed into the main feed port of the screw casing 2 via a feed hopper 1 (as shown).

[0286] The delivery zone for all components of the formulation is in the region of the housings 2 to 7 .

[0287] The plasticizing zone is in the region of the housing 8 and consists of various two- and three-stage kneading blocks and toothed mixing elements of different widths.

[0288] In the housing 9 , the additive, which is free-flowing at 23° C., is injected into the plastic body by means of a commercially available membrane piston pump (not shown) via a valve (not shown) which has been screwed into the bore 14 of the housing 9 .

[0289] In the region of the housings 9 to 10 there is the mixing zone, which is composed of kneading elements, toothed mixing elements and conveying elements.

[0290] In the housing part 11 there is a ventilation opening 13 which is connected to an extraction device (not shown).

[0291] The pressurized zone is in the housing 12, downstream of which is a nozzle plate having 29 holes.

[0292] In Examples 11 to 14, granulation was carried out in the form of strand granulation after cooling in a water bath.

[0293] The formulation fed into the extruder in Examples 11-14 consisted of the following mixture:

[0294] - 73% by weight of granules of linear polycarbonate based on bisphenol A, relative viscosity η rel =1.28 (measured at 25°C and 0.5 g / 100 ml concentration with CH2Cl2 as solvent); and

[0295] - 4.7% by weight of styrene-acrylonitrile copolymer (SAN) having an A:S weight ratio of 24:76, and

[0296] - 7.7% by weight of an emulsion-type ABS graft in powder form containing an A:B:S weight ratio of 12:58:30, and

[0297] - 10% by weight of an oligophosphate based on bisphenol A which is free-flowing at 23° C., in particular BDP, and

[0298] - 4.6% by weight of a powder mixture containing 3% by weight of bisphenol A based on linear polycarbonate, with a relative viscosity η rel =1.28 (measured with CH2Cl2 as solvent at 25°C and a concentration of 0.5 g / 100 ml), as well as 0.4 wt% of a stabilizer, 0.8 wt% of a flame retardant and 0.4 wt% of a release agent.

[0299] The average specific heat capacities of the plastic bodies of Examples 11-14 are shown in Table 1h.

[0300] In comparative example 11 and inventive examples 12 to 14, the formulations were mixed according to the following parameters as given in Table 1: screw shaft speed (Table 1, column p), mass flow rate (Table 1, column o) and the specific mechanical energy input (Table 1, column q) and the temperature of the melt flowing out of the nozzle plate (Table 1, column r). Table 1 also gives the amount of pellets containing unmelted particles thus obtained (Table 1, column w).

[0301] In Examples 15-19, all ingredients of the formulation, except the additives which flow freely at 23°C, were metered by a conventional gravimetric differential metering balance and fed into the main feed port of the screw casing 2 via a feed hopper 1 (as shown).

[0302] The delivery zone for all components of the formulation is in the region of the housings 2 to 7 .

[0303] The plasticizing zone is in the region of the housing 8 and consists of various two- and three-stage kneading blocks and toothed mixing elements of different widths.

[0304] In the housing 9 , the additive, which is free-flowing at 23° C., is injected into the plastic body by means of a commercially available membrane piston pump (not shown) via a valve (not shown) which has been screwed into the bore 14 of the housing 9 .

[0305] In the region of the housings 9 to 10 there is the mixing zone, which is composed of kneading elements, toothed mixing elements and conveying elements.

[0306] In the housing part 11 there is a ventilation opening 13 which is connected to an extraction device (not shown).

[0307] The pressurization zone is in the region of the housing 12, downstream of which is a nozzle plate having 29 holes.

[0308] In Examples 15 to 19, granulation was carried out in the form of strand granulation after cooling in a water bath.

[0309] The formulation fed into the extruder in Examples 15-19 consisted of the following mixture:

[0310] - 40.2% by weight of granules of linear polycarbonate based on bisphenol A, with a relative viscosity η rel =1.28 (measured at 25°C and 0.5 g / 100 ml concentration with CH2Cl2 as solvent); and

[0311] 23.5% by weight of granules of a linear polycarbonate based on bisphenol A, with a relative viscosity η rel = 1.20 (measured at 25°C and 0.5 g / 100 ml concentration with CH2Cl2 as solvent); and

[0312] - 7% by weight of styrene-acrylonitrile copolymer (SAN) having an A:S weight ratio of 24:76, and

[0313] - 11% by weight of an emulsion-type ABS graft in powder form containing an A:B:S weight ratio of 12:58:30; and

[0314] - 14% by weight of an oligophosphate based on bisphenol A which is free-flowing at 23° C., in particular BDP, and

[0315] - 4.3% by weight of a powder mixture containing 3% by weight of a linear polycarbonate based on bisphenol A with a relative viscosity η rel =1.28 (measured with CH2Cl2 as solvent at 25°C and a concentration of 0.5 g / 100 ml) and 0.1 wt% of a stabilizer, 0.8 wt% of a flame retardant and 0.4 wt% of a release agent.

[0316] The average specific heat capacity of the plastic bodies in Examples 15-19 is shown in Column h of Table 1.

[0317] In comparative examples 15-17 and inventive examples 18 and 19, the formulations were mixed according to the following parameters as given in Table 1: screw shaft speed (Table 1, column p), mass flow rate (Table 1, column o) and the specific mechanical energy input (Table 1, column q) and the temperature of the melt flowing out of the nozzle plate (Table 1, column r). Table 1 also gives the amount of pellets containing unmelted particles thus produced (Table 1, column w).

[0318] As shown in Examples 1-6, 7-10, 11-14 and 15-19, which have different formulations, respectively, regardless of the formulation or its average specific heat capacity, and regardless of the selected rate or the selected mass flow rate, the plastic body of the present invention is always obtained at a melting rate (Table 1, column x) of at least 1.18, especially at least 1.20. However, when the melting rate is less than 1.18, especially when the melting rate is 1.14 or lower, the amount of pellets containing unmelted particles is unacceptable.

[0319] Examples 20-29: Variation of particle diameter d

[0320] In Examples 20 to 29, a ZE60B UTXi twin-screw extruder from KraussMaffei Extrusion GmbH was used to produce the plastic bodies. The design features of the extruder can be found in Table 1, columns k to n. Figure 4 The basic structure of the extruder used in Examples 7-19 is shown.

[0321] In Examples 20-29, all ingredients of the formulations except the additives which flowed freely at 23°C were metered by a conventional gravimetric differential metering balance and fed into the main feed port of the screw casing 2 via a feed hopper 1 (as shown).

[0322] The delivery zone for all components of the formulation is in the region of the housings 2 to 7 .

[0323] The plasticizing zone is in the region of the housing 8, whose screw structure consists of various two- and three-stage kneading blocks with different widths and toothed mixing elements.

[0324] In the housing 9 , the additive, which flows freely at 23° C., is injected into the plastic body by means of a commercially available membrane piston pump (not shown) via a valve (not shown) which has been screwed into the bore 14 of the housing 9 .

[0325] The mixing zone is in the region of the housings 9 to 10 , in which the screw structure consists of kneading elements, toothed mixing elements and conveying elements.

[0326] In the housing part 11 there is a ventilation opening 13 which is connected to an extraction device (not shown).

[0327] The pressurized zone is in the housing 12, downstream of which is a nozzle plate having 29 holes.

[0328] In Examples 20 to 29, granulation was carried out in the form of strand granulation after cooling in a water bath.

[0329] The formulation fed into the extruder in Examples 20-29 consisted of the following mixture:

[0330] - 40.2% by weight of granules of linear polycarbonate based on bisphenol A, with a relative viscosity η rel =1.28 (measured at 25°C and 0.5 g / 100 ml concentration with CH2Cl2 as solvent); and

[0331] 23.5% by weight of granules of linear polycarbonate based on bisphenol A, with a relative viscosity η rel = 1.20 (measured at 25°C and 0.5 g / 100 ml concentration with CH2Cl2 as solvent); and

[0332] - 7% by weight of styrene-acrylonitrile copolymer (SAN) having an A:S weight ratio of 24:76, and

[0333] - 11% by weight of an emulsion-type ABS graft in powder form containing an A:B:S weight ratio of 12:58:30; and

[0334] - 14% by weight of an oligophosphate based on bisphenol A which is free-flowing at 23° C., in particular BDP, and

[0335] - 4.3% by weight of a powder mixture containing 3% by weight of a linear polycarbonate based on bisphenol A with a relative viscosity η rel =1.28 (measured with CH2Cl2 as solvent at 25°C and a concentration of 0.5 g / 100 ml), as well as 0.1 wt% of a stabilizer, 0.8 wt% of a flame retardant and 0.4 wt% of a release agent.

[0336] In Examples 20-29, the formulations were mixed according to the following parameters as described in Table 1: screw shaft speed (Table 1, column p), mass flow rate (Table 1, column o) and the resulting specific mechanical energy input (Table 1, column q) and the temperature of the melt flowing out of the nozzle plate (Table 1, column r). Table 1 also gives the amount of pellets containing unmelted particles thus produced (Table 1, column w).

[0337] In Examples 20-23, the diameter of the pellets of the low viscosity polycarbonate formulation component increased from 3.264 mm or 3.195 mm to 3.603 mm (see Table 1, column c.2) compared to Examples 15-19, while the higher viscosity polycarbonate formulation component remained unchanged (see Table 1, column c.1).

[0338] In Examples 24-27, the diameter of the pellets of the higher viscosity polycarbonate formulation component increased from 3.143 mm or 3.122 mm to 3.547 mm (see Table 1, column c.1), while the low viscosity polycarbonate formulation component remained unchanged (see Table 1, column c.2), compared to Examples 15-19.

[0339] In Examples 28-29, the diameter of the pellets of the SAN formulation component increased from 3.488 mm to 4.002 mm (see Table 1, column c.3) compared to Examples 15-19, while the polycarbonate formulation component remained unchanged (see Table 1, columns c.1 and c.2).

[0340] Comparison of Examples 20-23 with Examples 15-19 shows that the increase in the particle diameter of the low viscosity polycarbonate formulation component has no effect on the plasticization quality. The process parameters of equal mass flow rate and screw shaft speed give equivalent plasticization quality (see columns o, p, w in Table 1).

[0341] Comparison of Examples 24-27 with Examples 15-19 shows that, using equal process parameters of mass flow rate and screw shaft speed, the increase in pellet diameter of the high viscosity polycarbonate formulation component significantly deteriorates the plasticization quality (see columns o, p, w in Table 1).

[0342] Comparison of Examples 28-29 with Examples 15-19 shows that the increase in the particle diameter of the SAN formulation component has no effect on the plasticization quality. The process parameters of equal mass flow rate and screw shaft speed give equivalent plasticization quality (see columns o, p, w in Table 1).

[0343] As shown by the comparison of Examples 15-29, regardless of the pellet diameter and the selected rate or the selected mass flow rate, the plastic body of the present invention is always obtained at a melting rate (Table 1, column x) of at least 1.18, in particular at least 1.36, however, in the case of a melting rate of less than 1.18, in particular in the case of a melting rate of 1.16 or lower, the amount of pellets containing unmelted particles is unacceptable.

[0344] Examples 30-33: Variation of raw materials for the same formulation

[0345] In Examples 30-33, a ZE60B UTXi twin-screw extruder from KraussMaffei Extrusion GmbH was used to produce the plastic bodies. The design features of the extruder can be found in Table 1, columns k to n. Figure 4 The basic structure of the extruder used in Examples 30-33 is shown.

[0346] In Examples 30-33, all ingredients of the formulation, except the additives which flow freely at 23°C, were metered by a conventional gravimetric differential metering balance and fed into the main feed port of the screw casing 2 via a feed hopper 1 (as shown).

[0347] The delivery zone for all components of the formulation is in the region of the housings 2 to 7 .

[0348] The plasticizing zone is located in the region of the housing 8 and consists of various two- and three-stage kneading blocks and toothed mixing elements of different widths.

[0349] In the housing 9 , the additive, which flows freely at 23° C., is injected into the plastic body by means of a commercially available membrane piston pump (not shown) through a valve (not shown) which has been screwed into the bore 14 of the housing 9 .

[0350] The mixing zone is in the region of the housings 9 to 10 , whose screw structure consists of kneading elements, toothed mixing elements and conveying elements.

[0351] In the housing part 11 there is a ventilation opening 13 which is connected to an extraction device (not shown).

[0352] The pressurized zone is in the housing 12, downstream of which is a nozzle plate having 29 holes.

[0353] In Examples 30-33, granulation was carried out in the form of strand granulation after cooling in a water bath.

[0354] The formulation fed into the extruder in Examples 30-33 consisted of the following mixture:

[0355] - 63.7% by weight of granules of linear polycarbonate based on bisphenol A, with a relative viscosity η rel =1.28 (measured at 25°C and 0.5 g / 100 ml concentration with CH2Cl2 as solvent); and

[0356] - 7% by weight of styrene-acrylonitrile copolymer (SAN) having an A:S weight ratio of 24:76, and

[0357] - 11% by weight of an emulsion-type ABS graft in powder form containing an A:B:S weight ratio of 12:58:30, and

[0358] - 14% by weight of an oligophosphate based on bisphenol A which is free-flowing at 23° C., in particular BDP, and

[0359] - 4.3% by weight of a powder mixture containing 3% by weight of a linear polycarbonate based on bisphenol A with a relative viscosity η rel =1.28 (measured with CH2Cl2 as solvent at 25°C and a concentration of 0.5 g / 100 ml), as well as 0.1 wt% of a stabilizer, 0.8 wt% of a flame retardant and 0.4 wt% of a release agent.

[0360] In Examples 30-33, the formulations were mixed according to the following parameters as described in Table 1: screw shaft speed (Table 1, column p), mass flow rate (Table 1, column o) and the resulting specific mechanical energy input (Table 1, column q) and the temperature of the melt flowing out of the nozzle plate (Table 1, column r). Table 1 also gives the amount of pellets containing unmelted particles produced thereby (Table 1, column w).

[0361] Comparison of Examples 30-33 with Examples 15-19 shows that, using the same process parameters (mass flow rate and screw shaft speed), the plasticization quality obtained by using only one polycarbonate in the formulation (Examples 30-33) is much better than the plasticization quality obtained by using two polycarbonate components with different viscosities but having exactly the same total viscosity after mixing (Examples 15-19) (see Table 1, columns o, p, w).

[0362] Comparison of Examples 30-33 with Examples 15-19 also shows that, regardless of the polycarbonate component selected in the formulation and the selected rate or mass flow rate, the plastic body of the present invention is always obtained at a melting rate (Table 1, column x) of at least 1.18, especially at least 1.19, however, in the case of a melting rate of less than 1.18, especially in the case of a melting rate of 1.14 or less, the amount of pellets containing unmelted particles is unacceptable.

[0363] Examples 34-35: Variation of Extruder Diameter D

[0364] In Examples 34 and 35, a ZSK92 Mc twin-screw extruder from Coperion GmbH was used to produce the plastic bodies. The design features of the extruder can be found in Table 1, columns k to n. Figure 5 The basic structure of the extruder used in Examples 34 and 35 is shown.

[0365] In Examples 34 and 35, all ingredients of the formulations were metered by a conventional gravimetric differential metering balance and fed into the main feed port of the screw casing 16 via a feed hopper 15 (as shown).

[0366] The delivery zone for all components of the formulation is in the region of the housings 17 to 18 .

[0367] The plasticizing zone is in the region of the housings 19 to 20, whose screw structure consists of various two- and three-stage kneading blocks with different widths and toothed mixing elements.

[0368] The mixing zone is in the region of the housing 21 , whose screw structure consists of toothed mixing elements and conveying elements.

[0369] In the housing part 22 there is a ventilation opening 24 which is connected to an extraction device (not shown).

[0370] The pressurized zone is in housing 23, downstream of which is a nozzle plate with 100 holes.

[0371] In Examples 34 and 35, granulation was carried out as underwater granulation.

[0372] The formulation fed to the extruder in Examples 34 and 35 consisted of the following mixture:

[0373] - 60.3% by weight of granules of linear polycarbonate based on bisphenol A, with a relative viscosity η rel =1.28 (measured at 25°C and 0.5 g / 100 ml concentration with CH2Cl2 as solvent); and

[0374] - 17.2 wt% of emulsion-type ABS granules, containing A:B:S in a weight ratio of 20:24:56, and

[0375] - 8.9 wt% of bulk ABS granules containing A:B:S in a weight ratio of 25:10:65, and

[0376] - 9.5 wt% styrene-acrylonitrile copolymer (SAN) having an A:S weight ratio of 24:76, and

[0377] 4.1% by weight of a powder mixture containing 3% by weight of an emulsion ABS graft in powder form with an A:B:S weight ratio of 12:58:30, and 0.35% by weight of a stabilizer and 0.75% by weight of a mold release agent.

[0378] In comparative example 34 and inventive example 35, the formulations were mixed according to the following parameters as given in Table 1: screw shaft speed (Table 1, column p), mass flow rate (Table 1, column o) and the specific mechanical energy input (Table 1, column q) and the temperature of the melt flowing out of the nozzle plate (Table 1, column r). Table 1 also gives the amount of pellets containing unmelted particles thus produced (Table 1, column w).

[0379] Comparison of Examples 34 and 35 with Examples 1-6 shows that, regardless of the extruder diameter and the selected rate or mass flow rate selected for the formulation, the plastic bodies of the present invention are always obtained at a melting rate (Table 1, column x) of at least 1.18, in particular at least 1.53, whereas, at a melting rate of less than 1.18, in particular at a melting rate of 0.77 or less, the amount of pellets containing unmelted particles is unacceptable.

[0380] Examples 36-40: Variation of the metering point of free-flowing additives at 23°C

[0381] In Examples 36 to 40, a ZE60B UTXi twin-screw extruder from KraussMaffei Extrusion GmbH was used to produce the plastic bodies. The design features of the extruder can be found in Table 1, columns k to n. Figure 4 The basic structure of the extruder used in Examples 36-40 is shown.

[0382] In Examples 36-40, all ingredients of the formulation, except the free-flowing additives at 23°C, were metered by a conventional gravimetric differential metering balance and fed into the main feed port of the screw casing 2 via a feed hopper 1 (as shown).

[0383] The delivery zone for all components of the formulation is in the region of the housings 2 to 7 .

[0384] The plasticizing zone is located in the region of the housing 8 and consists of various two- and three-stage kneading blocks and toothed mixing elements of different widths.

[0385] In the housing 9 , the additive, which is free-flowing at 23° C., is injected into the plastic body by means of a commercially available membrane piston pump (not shown) through a valve (not shown) which has been screwed into the bore 14 of the housing 9 .

[0386] The mixing zone is located in the region of the housings 9 to 10 and consists of kneading elements, toothed mixing elements and conveying elements.

[0387] In the housing part 11 there is a ventilation opening 13 which is connected to an extraction device (not shown).

[0388] The pressurized zone is in the housing 12, downstream of which is a nozzle plate having 29 holes.

[0389] In Examples 36-40, granulation was carried out in the form of strand granulation after cooling in a water bath.

[0390] The formulation fed to the extruder in Examples 36-40 consisted of the following mixture:

[0391] - 58.7% by weight of granules of linear polycarbonate based on bisphenol A, with a relative viscosity η rel =1.28 (measured at 25°C and 0.5 g / 100 ml concentration with CH2Cl2 as solvent); and

[0392] - 9.3% by weight of styrene-acrylonitrile copolymer (SAN) having an A:S weight ratio of 24:76, and

[0393] - 8.7% by weight of an emulsion-type ABS graft in powder form containing an A:B:S weight ratio of 12:58:30, and

[0394] - 20% by weight of an oligophosphate based on bisphenol A which is free-flowing at 23° C., in particular BDP, and

[0395] - 4.3% by weight of a powder mixture containing 3% by weight of a linear polycarbonate based on bisphenol A, with a relative viscosity η rel =1.28 (measured with CH2Cl2 as solvent at 25°C and a concentration of 0.5 g / 100 ml), as well as 0.1 wt% of a stabilizer, 0.8 wt% of a flame retardant and 0.4 wt% of a release agent.

[0396] In Examples 36-40, the formulations were mixed according to the following parameters reported in Table 1: screw shaft speed (Table 1, column p), mass flow rate (Table 1, column o) and the specific mechanical energy input (Table 1, column q) and the temperature of the melt flowing out of the nozzle plate (Table 1, column r). Table 1 also reports the amount of pellets produced thereby containing unmelted particles (Table 1, column w).

[0397] Comparison of Examples 36-40 shows that, with the same process parameters (mass flow rate and screw shaft speed), the plasticization quality increases with delayed addition of the additive (free-flowing additive at 23°C) (see Table 1, columns o, p, w).

[0398] The comparison of Examples 36-40 also shows that, regardless of the addition site and the selected rate or the selected mass flow rate of the additive that is free-flowing at 23° C., the plastic body of the present invention is always obtained at a melting rate (Table 1, column x) of at least 1.18, in particular at least 1.35, however, in the case of a melting rate of less than 1.18, in particular in the case of a melting rate of 1.11 or less, the amount of pellets containing unmelted particles is unacceptable.

[0399] Examples 41-44: Variation of the number of extruder screw shafts

[0400] In Examples 41 to 44, an annular extruder of the type RE1 with 12 co-rotating screw shafts from CPM Extricom Extrusion GmbH was used to produce the plastic bodies. The design features of the extruder can be found in Table 1, columns k to n. Figure 6 The basic structure of the extruder used in Examples 41-44 is shown.

[0401] In Examples 41-44, all ingredients of the formulations were metered by a conventional gravimetric differential metering balance and fed into the main feed port of the screw casing 26 via a feed hopper 25 (as shown).

[0402] The delivery zone for all components of the formulation is in the region of the housings 27 to 29 .

[0403] The plasticizing zone is in the region of the housing 30, and its screw structure consists of two-stage kneading blocks with various widths.

[0404] In the housing part 31 there is a ventilation opening 33 which is connected to an extraction device (not shown).

[0405] The pressurized zone is in the housing 32, downstream of which is a nozzle plate having 6 holes.

[0406] In Examples 41-44, granulation was carried out in the form of strand granulation after cooling in a water bath.

[0407] The formulation fed to the extruder in Examples 41-44 consisted of the following mixture:

[0408] - 28% by weight of granules of linear polycarbonate based on bisphenol A, relative viscosity η rel =

[0409] 1.28 (measured with CH2Cl2 as solvent, at 25°C and a concentration of 0.5 g / 100 ml);

[0410] and

[0411] - 15% by weight of granules of linear polycarbonate based on bisphenol A, relative viscosity η rel =

[0412] 1.20 (measured with CH2Cl2 as solvent, at 25°C and a concentration of 0.5 g / 100 ml);

[0413] and

[0414] - 31% by weight of styrene-acrylonitrile copolymer (SAN) having an A:S weight ratio of 24:76, and

[0415] - 22% by weight of an emulsion-type ABS graft in powder form containing an A:B:S weight ratio of 12:58:30, and

[0416] 4% by weight of a powder mixture containing 3.1% by weight of an emulsion ABS graft in powder form with an A:B:S weight ratio of 12:58:30, and 0.16% by weight of a stabilizer and 0.74% by weight of a mold release agent.

[0417] In comparative examples 41 and 42 and inventive examples 43 and 44, the formulations were compounded according to the following parameters reported in Table 1: screw shaft speed (Table 1, column p), mass flow rate (Table 1, column o) and temperature of the resulting melt flowing out of the nozzle plate (Table 1, column r). Table 1 also reports the amount of pellets containing unmelted particles produced thereby (Table 1, column w).

[0418] As shown in Examples 41-44, even in the case of an extruder having twelve shafts, regardless of the selected rate or the mass flow rate selected for the formulation, the plastic body of the present invention is always obtained at a melting rate (Table 1, column x) of at least 1.18, in particular at least 1.53, however, in the case of a melting rate of less than 1.18, in particular in the case of a melting rate of 1.03 or less, the amount of pellets containing unmelted particles is unacceptable.

[0419] In order to make the melting rates of the twelve-axis screw machine and the twin-axis screw machine comparable, the mass flow rate must be taken into account when calculating the melting rate of the twelve-axis screw machine. Dividing by 6 ignores the fact that a twelve-shaft screw machine is not six twin-shaft screw machines, but produces a throughput increase effect because each screw has two adjacent screws meshing simultaneously, rather than just one screw as in a twin-shaft screw machine. Dividing the mass flow rate by 6 gives an equal, dimensionless throughput, making the two screw machines comparable. For example, in Kohlgrüber, Bierdel, Rust, “Polymer-Aufbereitung und Kunststoff-Compoundierung” [Polymer Processing and PlasticsCompounding], Hanser-Verlag, 2019, p. 36, chapter 2.3.7, the dimensionless throughput is defined as the throughput index V * , where the reference diameter D for both twelve-shaft and twin-shaft screw machines is the inner shell diameter.

[0420] Conclusion of all examples

[0421] Examples 1 to 44 show that at a melt rate of at least 1.18, plastic bodies produced from a formulation containing at least two thermoplastic components, at least one of which is polycarbonate, always have good plasticization properties, regardless of the heat capacity of the plastic body, the pellet diameter of the highest viscous polycarbonate component in the formulation, the inner shell diameter of the extruder, the structure of the extruder, the metering point of the additive that is free-flowing at 23°C, the components of the formulation, the number of shafts in the extruder, and the process parameters of mass flow rate and screw shaft speed.

[0422] Table 1 (Examples 1-44)

[0423]

[0424]

[0425] Table 1 (Examples 1-44) continued

[0426]

[0427] Table 1 (Examples 1-44) continued

[0428]

[0429] Table 1 (Examples 1-44) continued

[0430]

Claims

1. A method for producing a plastic body, In a multi-screw machine with co-rotating parallel screw shafts rotating at equal speeds, The screw shaft rotates at a speed n, wherein the plastic body is produced from a formulation comprising at least two thermoplastic components, wherein at least one of the at least two thermoplastic components is polycarbonate, wherein the plastic body (i) does not contain any additive which is free-flowing at 23°C, or (ii) contains exactly one additive which is free-flowing at 23°C, or (iii) contains at least two additives that are free-flowing at 23°C, in, The dynamic viscosity of the plastic body is measured according to ISO 11443:2014 method A2 under the following conditions: at a shear rate of 200 1 / s Next, and In case (i), the temperature is 230°C, and in case (ii), the temperature is 230° C. minus <230° C. times twice the mass ratio of the exactly one free-flowing additive at 23° C.>, the mass ratio being based on the mass of the plastic body, and in case (iii), the temperature is 230° C. minus <230° C. times twice the sum of the mass ratios of the at least two free-flowing additives at 23° C.>, the mass ratios being based on the mass of the plastic body, The measured dynamic viscosity is a ratio of 0.3 to 3 based on the shear rate of 200 1 / s according to ISO 11443:2014 method A2. a viscometer of at least one of the thermoplastic components measured at a temperature of 230° C. and 30° C.; and wherein at least two thermoplastic components differ in at least one of the following characteristics: At least one structural unit is different, or The difference in relative solution viscosity is at least 5% as measured according to EN ISO 1628-1:2021, wherein the method is characterized by a melting rate, The melting rate in a longitudinal section of the screw machine, starting at a distance of twice the inner shell diameter D upstream of the first screw element that is not a conveying element and ending at the last screw element of the screw machine, is 1.18 to 8, wherein for this melting rate: and among them: τ1 is the average residence time of the plastic bodies in a longitudinal section of the screw machine, said longitudinal section starting at a distance of twice the inner casing diameter D upstream of the first screw element which is not a conveying element, and In case (i), the end is at the last screw element of the screw machine, and in case (ii) or (iii), ends at the first addition point of the free-flowing additive at 23° C. downstream of the first spiral element which is not a conveying element, And among them, δη1 is the ratio of the dynamic viscosity of the plastic to the shear rate corresponding to the screw shaft speed n. Next, and In case (i), the temperature is 230°C and In case (ii), the temperature is 230° C. minus <230° C. times twice the mass ratio of the precisely one free-flowing additive at 23° C.>, the mass ratio being based on the mass of the plastic body, and In case (iii), the temperature is 230° C. minus <230° C. times twice the sum of the mass ratios of the at least two free-flowing additives at 23° C.>, the mass ratios being based on the total mass of the plastic body, Based on the dynamic viscometer of the thermoplastic component with the highest dynamic viscosity measured under the following conditions, the conditions are a shear rate of 200 1 / s and In case (i), the temperature is 230°C, and in case (ii), the temperature is 230° C. minus <230° C. times twice the mass ratio of the exactly one free-flowing additive at 23° C.>, the mass ratio being based on the mass of the plastic body, and in case (iii), the temperature is 230° C. minus <230° C. multiplied by twice the sum of the mass ratios of the at least two free-flowing additives at 23° C.>, the mass ratios being based on the mass of the plastic body; τ2 is In case (ii) or (iii), the average residence time of the plastic bodies in the longitudinal section of the screw machine, The longitudinal section starts from the first addition point of the free-flowing additive at 23° C. at a distance of twice the inner shell diameter D upstream of the first screw element which is not a conveying element and ends at the last screw element of the screw machine, and in case (i), is zero, δη2 is the shear rate corresponding to the screw shaft speed n the ratio of the dynamic viscosities of the plastic body at a shear rate of 200 1 / s and at a temperature corresponding to the temperature of the plastic body at the end of the last screw element, based on a dynamic viscometer of the thermoplastic component with the highest dynamic viscosity measured at a shear rate of 200 1 / s and at a temperature corresponding to the temperature of the plastic body at the end of the last screw element, λ is the thermal conductivity measured at 23°C according to EN ISO 11357-8:2021, measured immediately after the plastic body comes out of the screw machine; n is the speed of the screw shaft of the screw machine, d is the diameter of the pellets of polycarbonate present in the formulation for producing the plastic body having the highest relative viscosity, measured in accordance with EN ISO 1628-1:2021, D is the inner diameter of the screw machine's casing, where the inner shell diameter D is the same for all screw machine casings. c p is the average specific heat capacity measured in the temperature range of 250°C to 300°C according to ISO 11357-4:2021, It is the mass flow rate of the plastic body in the screw machine [kg / s].

2. The method according to claim 1, wherein the melting rate is 1.18 to 5.

3. The method according to claim 1 or 2, wherein the melting rate is 1.2 to 3.

4. The method according to any one of claims 1 to 3, wherein If at least one additive that is free-flowing at 23° C. is used and added, one of these additives is bisphenol A bis(diphenyl phosphate).

5. A method according to any one of claims 1 to 4, wherein all thermoplastic components in the formulation are polycarbonate.

6. The method according to any one of claims 1 to 4, wherein If one of the at least two thermoplastic components is not a polycarbonate, the thermoplastic component that is not a polycarbonate is selected from the group consisting of: Polyester carbonates, polyamides, polyesters (especially polybutylene terephthalate and polyethylene terephthalate), polylactic acid, polyethers, thermoplastic polyurethanes, polyacetals, fluoropolymers (especially polyvinylidene fluoride), polyethersulfones, polyolefins (especially polyethylene and polypropylene), polyimides, polyacrylates (especially polymethyl (meth)acrylate), polyphenylene oxide, polyphenylene sulfide, polyetherketones, polyaryletherketones, styrene polymers (especially polystyrene), styrene copolymers (especially styrene-acrylonitrile copolymers), acrylonitrile-butadiene-styrene block copolymers and polyvinyl chloride.

7. The process according to claim 1, wherein the proportion of polycarbonate in the formulation for producing the plastic body is 20% to 98% by weight, in particular 40% to 80% by weight.

8. The method according to any one of claims 1 to 7, wherein at least one of the thermoplastic components is a polycarbonate and is an aromatic polycarbonate based on bisphenol A, in particular a linear aromatic polycarbonate based on bisphenol A.

9. The method according to claim 6, wherein: If one of the at least two thermoplastic components is not a polycarbonate, then the thermoplastic component is a rubber-modified vinyl (co)polymer.