Polymer latex for wood adhesives

Prepare polymer latex through free radical emulsion polymerization and mix it with polyisocyanate compounds, which solves the problem of insufficient bonding performance of water-based polymer isocyanate adhesives in water resistance and boiling water resistance, improves wood bonding strength and shelf life, and is suitable for strict D4 wood glue in harsh environments.

CN119053631APending Publication Date: 2024-11-29SYNTHOMER DEUTSCHLAND GMBH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380034824.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-21
Filing Date
2023-04-05
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing water-based polymer isocyanate adhesives have insufficient performance in water-resistant and boiling water-resistant bonding, and the adhesive itself is not stable (storage period) and it is difficult to maintain in severe high temperature or high humidity environments. performance.

Method used

Polymer latex is prepared by radical emulsion polymerization using vinyl aromatic monomers, conjugated diene monomers and ethylenically unsaturated monomers with acid and/or hydroxy functional groups to form a polymerization with a median particle size of at least 220 nanometers and mixed with the polyisocyanate compound to prepare an aqueous binder composition.

Benefits of technology

It improves the strength of wood bonding and the shelf life of adhesives, is suitable for D4 wood glue, and enhances performance stability in high temperature and high humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005090603420000251
    Figure BDA0005090603420000251
  • Figure BDA0005090603420000261
    Figure BDA0005090603420000261
  • Figure BDA0005090603420000262
    Figure BDA0005090603420000262
Patent Text Reader

Abstract

The invention relates to a polymer latex for an adhesive composition, to a method for the production thereof and to the use thereof. Furthermore, in particular but not exclusively, the present invention relates to an aqueous adhesive composition comprising such a polymer latex and a process for preparing such an aqueous adhesive composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polymer latex for an adhesive composition, a preparation method and use of the polymer latex. In addition, the present invention particularly but not exclusively relates to an aqueous adhesive composition comprising the polymer latex and a method for preparing the aqueous adhesive composition. Background Art

[0002] D4 wood adhesives require specific durability because they are used in interior areas that are often exposed to tap water or condensation for long periods of time and / or exterior areas that are exposed to weather. Suitable adhesives should not only excel in dry adhesion performance, but also in secondary properties such as water-resistant adhesion, boiling water-resistant adhesion, and heat-resistant adhesion. Conventional water-based polymer isocyanate adhesives are insufficient in water-resistant adhesion, especially boiling water-resistant adhesion, but they are satisfactory in dry adhesion. Another challenge is an extended period of time in harsher environments than usual, such as high temperature or high humidity.

[0003] In addition to the requirement for adhesion, extension of the stability (shelf life) of the adhesive itself after blending the isocyanate compound is desired.

[0004] EP1754766A1 relates to a water-based polymer dispersion for an isocyanate-crosslinked adhesive, the dispersion comprising a polymer (1) obtained by emulsion polymerization of a monomer composition, the monomer composition comprising at least one monomer selected from aromatic vinyl monomers and (meth)acrylate monomers, a crosslinkable monomer and a different monomer; and a polymer (2) obtained by emulsion polymerization of a monomer composition, the monomer composition comprising at least one monomer selected from aromatic vinyl monomers and (meth)acrylate monomers, a hydroxyl-containing vinyl monomer, an ethylenically unsaturated carboxylic acid monomer and a different monomer; wherein the polymers (1) and (2) have a Tg difference of 20 to 80°C.

[0005] An object of the present invention is to provide a polymer latex for an adhesive composition which provides a long shelf life after mixing with a hardener component and provides a high wood joint strength, which is suitable for wood glue and particularly for D4 wood glue. Summary of the invention

[0006] The following clauses summarize certain aspects of the invention.

[0007] According to a first aspect, the present invention relates to a polymer latex for use in an adhesive composition, obtainable by free radical emulsion polymerization of a mixture of ethylenically unsaturated monomers comprising:

[0008] (a) vinyl aromatic monomers;

[0009] (b) a conjugated diene monomer; and

[0010] (c) ethylenically unsaturated monomers having acid and / or hydroxyl functionality;

[0011] wherein the weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) is in the range of 1.60 to 2.30, and wherein the polymer latex has a median particle size of at least 220 nanometers.

[0012] The sum of the vinyl aromatic monomer (a) and the conjugated diene monomer (b) may range from 85.0 to 99.0 wt%, preferably from 90.0 to 98.0 wt%, based on the total weight of monomers in the monomer mixture.

[0013] The mixture of ethylenically unsaturated monomers may comprise:

[0014] (a) 40 to 80 weight percent, preferably 50 to 75 weight percent, more preferably 55 to 70 weight percent of a vinyl aromatic monomer, based on the total weight of the monomers in the monomer mixture.

[0015] The vinyl aromatic monomer (a) may be selected from styrene, α-methylstyrene, vinyltoluene and combinations thereof. The vinyl aromatic monomer (a) may be selected from styrene.

[0016] The mixture of ethylenically unsaturated monomers may comprise:

[0017] (b) 15 to 50 weight percent, preferably 20 to 45 weight percent, more preferably 25 to 40 weight percent of a conjugated diene monomer, based on the total weight of the monomers in the monomer mixture.

[0018] The conjugated diene monomer (b) can be selected from 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2,4-hexadiene, 1,3-octadiene, 2-methyl-1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 3,4-dimethyl-1,3-hexadiene, 2,3-diethyl-1,3-butadiene, 4,5-diethyl-1,3-octadiene, 3-butyl-1,3-octadiene, 3,7-dimethyl-1,3,6-octatriene, 2-methyl-6-methylene-1,7-octadiene, 7-methyl-3-methylene-1,3-octadiene, The conjugated diene monomer (b) can be selected from 1,3-butadiene, isoprene, 1,3,6-octatriene, 2-ethyl-1,3-butadiene, 2-pentyl-1,3-butadiene, 3,7-dimethyl-1,3,7-octatriene, 3,7-dimethyl-1,3,6-octatriene, 3,7,11-trimethyl-1,3,6,10-dodecatetraene, 7,11-dimethyl-3-methylene-1,6,10-dodecatetraene, 2,6-dimethyl-2,4,6-octatriene, 2-phenyl-1,3-butadiene, 2-methyl-3-isopropyl-1,3-butadiene, 1,3-cyclohexadiene, myrcene, ocimene, farnesene, and combinations thereof. The conjugated diene monomer (b) can be selected from 1,3-butadiene, isoprene, and combinations thereof. The conjugated diene monomer (b) may be selected from 1,3-butadiene.

[0019] The mixture of ethylenically unsaturated monomers may comprise:

[0020] (c) 0.2 to 6.0 wt %, preferably 0.3 to 5.0 wt %, more preferably 0.5 to 4.0 wt % of ethylenically unsaturated monomers having acid and / or hydroxy functionality, based on the total weight of monomers in the monomer mixture.

[0021] The ethylenically unsaturated monomer (c) with acid functionality can be selected from ethylenically unsaturated carboxylic acid monomers, ethylenically unsaturated sulfonic acid monomers, ethylenically unsaturated phosphorus acid monomers. The ethylenically unsaturated monomer (c) with acid functionality can be selected from (methyl) acrylic acid, crotonic acid, fumaric acid, itaconic acid, maleic acid, maleic anhydride, vinyl acetate, vinyl lactic acid, vinyl sulfonic acid, styrene sulfonic acid, (methyl) 2-carboxyethyl acrylate, vinyl sulfonate phenyl ester, 4-vinylbenzene sulfonate sodium, 2-methyl-2-propylene-1-sulfonic acid, 2-propylene-1-sulfonic acid, 4-styrene sulfonic acid, 2-acrylamido-2-methyl-1-propane sulfonic acid, vinylphosphonic acid, vinylphosphonic acid dimethyl ester, vinylphosphonic acid diethyl ester, allylphosphonic acid diethyl ester, allylphosphonic acid and combinations thereof. The ethylenically unsaturated monomer (c) with acid functionality can be selected from (methyl) acrylic acid, itaconic acid and combinations thereof.

[0022] The ethylenically unsaturated monomer (c) having a hydroxyl functional group may be selected from allyl alcohol, vinyl alcohol, N-hydroxymethyl (meth) acrylamide, 1-pentene-3-ol; hydroxyalkyl esters of ethylenically unsaturated acids, such as hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl (meth) acrylate, and hydroxyethyl caprolactone acrylate; and combinations thereof. The ethylenically unsaturated monomer (c) having a hydroxyl functional group may be selected from hydroxyalkyl esters of ethylenically unsaturated acids, such as hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl (meth) acrylate, and hydroxyethyl caprolactone acrylate. The ethylenically unsaturated monomer (c) having a hydroxyl functional group may be selected from hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl methacrylate, and combinations thereof.

[0023] The ethylenically unsaturated monomer (c) having acid and hydroxyl functional groups may be selected from 3-allyloxy-2-hydroxy-1-propanesulfonic acid.

[0024] The weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) may be in the range of 1.70 to 2.10.

[0025] The polymer latex may have a median particle size of at least 230 nanometers, preferably at least 250 nanometers.

[0026] The mixture of ethylenically unsaturated monomers may contain 0.05 to 3.0 wt %, preferably 0.10 to 2.0 wt %, more preferably 0.15 to 1.5 wt % of a chain transfer agent, wherein the weight percentages are based on the total amount of monomers in the monomer mixture.

[0027] The chain transfer agent can be selected from n-dodecyl mercaptan, carbon tetrachloride, carbon tetrabromide, bromotrichloromethane, 4-methylbenzenethiol, isooctyl 3-mercaptopropionate, tert-nonyl mercaptan, 4,4′-thiobisbenzenethiol, tert-dodecyl mercaptan, α-methylstyrene dimer, thioglycolic acid, 2-ethylhexyl thioglycolate, butyl 3-mercaptopropionate, 1,8-dimercapto-3,6-dioxaoctane and combinations thereof, preferably tert-dodecyl mercaptan.

[0028] The mixture of ethylenically unsaturated monomers may further comprise (d) 0 to 20 wt. % of an ethylenically unsaturated monomer different from (a) to (c), based on the total weight of monomers in the monomer mixture, wherein the ethylenically unsaturated monomer different from (a) to (c) is preferably selected from:

[0029] (d1) an ethylenically unsaturated nitrile compound, which is preferably selected from (meth)acrylonitrile, α-cyanoethylacrylonitrile, fumaronitrile, α-chloronitrile and combinations thereof;

[0030] (d2) alkyl esters of ethylenically unsaturated acids, which are preferably selected from methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and combinations thereof;

[0031] (d3) ethylenically unsaturated compounds having a primary or secondary amino group, which are preferably selected from (meth)acrylamide, 2-aminoethyl (meth)acrylate hydrochloride, 2-aminoethyl (meth)acrylamide hydrochloride, N-ethyl (meth)acrylamide, N-(3-aminopropyl) (meth)acrylamide hydrochloride, N-hydroxyethyl (meth)acrylamide, N-3-(dimethylamino)propyl (meth)acrylamide, [3-(methacryloylamino)propyl]trimethylammonium, N-[tris (hydroxymethyl)methyl] (meth)acrylamide, N-phenylacrylamide, alkyl acrylamide, methacrylamide poly (ethylene glycol) amine hydrochloride and combinations thereof;

[0032] and combinations thereof.

[0033] According to a further aspect, the present invention relates to a method for preparing a polymer latex, preferably as discussed above, for use in an adhesive, wherein the method comprises:

[0034] A mixture of ethylenically unsaturated monomers is polymerized by free radical emulsion polymerization, wherein the mixture comprises:

[0035] (a) vinyl aromatic monomers;

[0036] (b) a conjugated diene monomer; and

[0037] (c) ethylenically unsaturated monomers having acid and / or hydroxyl functionality;

[0038] wherein the weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) is in the range of 1.60 to 2.30, and wherein the polymer latex has a median particle size of at least 220 nanometers.

[0039] The weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) may be in the range of 1.70 to 2.10.

[0040] The sum of the vinyl aromatic monomer (a) and the conjugated diene monomer (b) may range from 85.0 to 99.0 wt%, preferably from 90.0 to 98.0 wt%, based on the total weight of monomers in the monomer mixture.

[0041] The mixture of ethylenically unsaturated monomers may comprise:

[0042] (a) 40 to 80 weight percent, preferably 50 to 75 weight percent, more preferably 55 to 70 weight percent of a vinyl aromatic monomer, based on the total weight of the monomers in the monomer mixture.

[0043] The vinyl aromatic monomer (a) may be selected from styrene, α-methylstyrene, vinyltoluene and combinations thereof. The vinyl aromatic monomer (a) may be selected from styrene.

[0044] The mixture of ethylenically unsaturated monomers may comprise:

[0045] (b) 15 to 50 weight percent, preferably 20 to 45 weight percent, more preferably 25 to 40 weight percent of a conjugated diene monomer, based on the total weight of the monomers in the monomer mixture.

[0046] The conjugated diene monomer (b) can be selected from 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2,4-hexadiene, 1,3-octadiene, 2-methyl-1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 3,4-dimethyl-1,3-hexadiene, 2,3-diethyl-1,3-butadiene, 4,5-diethyl-1,3-octadiene, 3-butyl-1,3-octadiene, 3,7-dimethyl-1,3,6-octatriene, 2-methyl-6-methylene-1,7-octadiene, 7 ... The conjugated diene monomer (b) can be selected from 1,3-butadiene, isoprene, 2-methyl-3-isopropyl-1,3-butadiene, 1,3-cyclohexadiene, 1,3-butylene, 2-pentyl-1,3-butadiene, 3,7-dimethyl-1,3,7-octatriene, 3,7-dimethyl-1,3,6-octatriene, 3,7,11-trimethyl-1,3,6,10-dodecatetraene, 7,11-dimethyl-3-methylene-1,6,10-dodecatetraene, 2,6-dimethyl-2,4,6-octatriene, 2-phenyl-1,3-butadiene, 2-methyl-3-isopropyl-1,3-butadiene, 1,3-cyclohexadiene, myrcene, ocimene, farnesene and combinations thereof. The conjugated diene monomer (b) can be selected from 1,3-butadiene, isoprene and combinations thereof. The conjugated diene monomer (b) may be selected from 1,3-butadiene.

[0047] The mixture of ethylenically unsaturated monomers may comprise:

[0048] (c) 0.2 to 6.0 wt %, preferably 0.3 to 5.0 wt %, more preferably 0.5 to 4.0 wt % of ethylenically unsaturated monomers having acid and / or hydroxy functionality, based on the total weight of monomers in the monomer mixture.

[0049] The ethylenically unsaturated monomer (c) with acid functionality can be selected from ethylenically unsaturated carboxylic acid monomers, ethylenically unsaturated sulfonic acid monomers, ethylenically unsaturated phosphorus acid monomers. The ethylenically unsaturated monomer (c) with acid functionality can be selected from (methyl) acrylic acid, crotonic acid, fumaric acid, itaconic acid, maleic acid, maleic anhydride, vinyl acetate, vinyl lactic acid, vinyl sulfonic acid, styrene sulfonic acid, (methyl) 2-carboxyethyl acrylate, vinyl sulfonate phenyl ester, 4-vinylbenzene sulfonate sodium, 2-methyl-2-propylene-1-sulfonic acid, 2-propylene-1-sulfonic acid, 4-styrene sulfonic acid, 2-acrylamido-2-methyl-1-propane sulfonic acid, vinylphosphonic acid, vinylphosphonic acid dimethyl ester, vinylphosphonic acid diethyl ester, allylphosphonic acid diethyl ester, allylphosphonic acid and combinations thereof. The ethylenically unsaturated monomer (c) with acid functionality can be selected from (methyl) acrylic acid, itaconic acid and combinations thereof.

[0050] The ethylenically unsaturated monomer (c) having a hydroxyl functional group may be selected from allyl alcohol, vinyl alcohol, N-hydroxymethyl (meth) acrylamide, 1-pentene-3-ol; hydroxyalkyl esters of ethylenically unsaturated acids, such as hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl (meth) acrylate, and hydroxyethyl caprolactone acrylate; and combinations thereof. The ethylenically unsaturated monomer (c) having a hydroxyl functional group may be selected from hydroxyalkyl esters of ethylenically unsaturated acids, such as hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl (meth) acrylate, and hydroxyethyl caprolactone acrylate. The ethylenically unsaturated monomer (c) having a hydroxyl functional group may be selected from hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl methacrylate, and combinations thereof.

[0051] The ethylenically unsaturated monomer (c) having acid and hydroxyl functional groups may be selected from 3-allyloxy-2-hydroxy-1-propanesulfonic acid.

[0052] The weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) may be in the range of 1.70 to 2.10.

[0053] The polymer latex may have a median particle size of at least 230 nanometers, preferably at least 250 nanometers.

[0054] The mixture of ethylenically unsaturated monomers may contain 0.05 to 3.0 wt %, preferably 0.10 to 2.0 wt %, more preferably 0.15 to 1.5 wt % of a chain transfer agent, wherein the weight percentage is based on the total amount of monomers in the monomer mixture. The chain transfer agent may be selected from n-dodecyl mercaptan, carbon tetrachloride, carbon tetrabromide, bromotrichloromethane, 4-methylbenzenethiol, 3-isooctyl mercaptopropionate, tert-nonyl mercaptan, 4,4′-thiobisbenzenethiol, tert-dodecyl mercaptan, α-methylstyrene dimer, mercaptoacetic acid, 2-ethylhexyl mercaptoacetate, 3-butyl mercaptopropionate, 1,8-dimercapto-3,6-dioxaoctane, and combinations thereof, preferably tert-dodecyl mercaptan.

[0055] The mixture of ethylenically unsaturated monomers may further comprise (d) 0 to 20 wt % of an ethylenically unsaturated monomer different from (a) to (c), based on the total weight of monomers in the monomer mixture; wherein the ethylenically unsaturated monomer different from (a) to (c) is preferably selected from:

[0056] (d1) an ethylenically unsaturated nitrile compound, which is preferably selected from (meth)acrylonitrile, α-cyanoethylacrylonitrile, fumaronitrile, α-chloronitrile and combinations thereof;

[0057] (d2) alkyl esters of ethylenically unsaturated acids, which are preferably selected from methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and combinations thereof;

[0058] (d3) ethylenically unsaturated compounds having a primary or secondary amino group, which are preferably selected from (meth)acrylamide, 2-aminoethyl (meth)acrylate hydrochloride, 2-aminoethyl (meth)acrylamide hydrochloride, N-ethyl (meth)acrylamide, N-(3-aminopropyl) (meth)acrylamide hydrochloride, N-hydroxyethyl (meth)acrylamide, N-3-(dimethylamino)propyl (meth)acrylamide, [3-(methacryloylamino)propyl]trimethylammonium, N-[tris (hydroxymethyl)methyl] (meth)acrylamide, N-phenylacrylamide, alkyl acrylamide, methacrylamide poly (ethylene glycol) amine hydrochloride and combinations thereof;

[0059] and combinations thereof.

[0060] Another aspect of the present invention relates to the use of the polymer latex as discussed above or the polymer latex prepared by the method as discussed above for preparing an aqueous adhesive composition, preferably a two-component aqueous adhesive composition.

[0061] Furthermore, a further aspect of the present invention relates to an aqueous adhesive composition comprising (i) a polymer latex as discussed above or a polymer latex prepared by a method as discussed above; and (ii) a polyisocyanate compound.

[0062] The (ii) polyisocyanate compound may include toluene diisocyanate, hydrogenated toluene diisocyanate, methylene diphenyl diisocyanate, hydrogenated methylene diphenyl diisocyanate, triphenylmethane triisocyanate, 1,2,4-benzene triisocyanate, polymethylene polyphenyl polyisocyanate, xylene diisocyanate, tetramethylxylylene diisocyanate, 1,6-hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, isophorone diisocyanate and 4,4′-methylene-bis(cyclohexyl isocyanate), and combinations thereof.

[0063] The aqueous adhesive composition as discussed above may further comprise polyvinyl alcohol, vinyl alcohol-ethylene copolymer, polyvinyl alcohol modified by silanol; cellulose derivatives such as methyl cellulose, ethyl cellulose, hydroxy cellulose and carboxy cellulose; chitin, chitosan, starch, polyethylene glycol, polypropylene glycol, polyvinyl ether, gelatin, casein, cyclodextrin and combinations thereof; preferably polyvinyl alcohol.

[0064] The aqueous adhesive composition as discussed above can be a two-component adhesive composition, wherein the first component comprises the polymer latex and optionally polyvinyl alcohol, vinyl alcohol-ethylene copolymer, polyvinyl alcohol modified with silanol; cellulose derivatives such as methyl cellulose, ethyl cellulose, hydroxy cellulose and carboxy cellulose; chitin, chitosan, starches, polyethylene glycol, polypropylene glycol, polyvinyl ether, gelatin, casein, cyclodextrin and combinations thereof, preferably polyvinyl alcohol; and the second component comprises the polyisocyanate compound.

[0065] The aqueous adhesive composition as discussed above may contain 1 to 50 wt %, preferably 2 to 45 wt %, more preferably 5 to 40 wt % of the polyisocyanate compound (ii), based on the total solid content of the aqueous adhesive composition.

[0066] The aqueous adhesive as discussed above may be in the form of a wood glue.

[0067] Another aspect of the present invention relates to a method for preparing an aqueous adhesive composition, comprising:

[0068] Providing (i) a polymer latex as discussed above or a polymer latex prepared by a method as discussed above; and mixing with (ii) a polyisocyanate compound, wherein the aqueous adhesive composition is preferably a wood glue. DETAILED DESCRIPTION DETAILED DESCRIPTION OF THE INVENTION

[0070] The present invention relates to a polymer latex for an adhesive composition. The polymer latex can be obtained by free radical emulsion polymerization of a mixture of ethylenically unsaturated monomers comprising the following: (a) a vinyl aromatic monomer; (b) a conjugated diene monomer; and (c) an ethylenically unsaturated monomer having acid and / or hydroxyl functional groups. According to the present invention, the weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) is in the range of 1.60 to 2.30. The polymer latex of the present invention has a median particle size of at least 220 nanometers. The median particle size can be measured according to ISO 22412:2017 by dynamic light scattering, for example, using a dynamic light scattering device Mastersizer 2000 (Malvern Panalyt ical (UK)). The polymer latex is preferably obtained by free radical emulsion polymerization of a mixture of ethylenically unsaturated monomers comprising the following: (a) a vinyl aromatic monomer; (b) a conjugated diene monomer; and (c) an ethylenically unsaturated monomer having acid and / or hydroxyl functional groups.

[0071] It has surprisingly been found that the weight ratio of vinyl aromatic monomer (a) to conjugated diene monomer (b) and the median particle size of the polymer latex of the present invention provide improved wood joint strength and improved shelf life.

[0072] According to the present invention, the sum of the vinyl aromatic monomer (a) and the conjugated diene monomer (b) can be at least 85.0 weight %, such as at least 87.0 weight %, or at least 90.0 weight %, or at least 93.0 weight %, or at least 95.0 weight %, or at least 97.0 weight %, based on the total weight of the monomers in the monomer mixture. The sum of the vinyl aromatic monomer (a) and the conjugated diene monomer (b) can be 99.0 weight % or less, such as 98.5 weight % or less, or 98.0 weight % or less, or 97.5 weight % or less, based on the total weight of the monomers in the monomer mixture. Those skilled in the art recognize that any range between any clearly disclosed lower and upper limits is disclosed herein. Therefore, the sum of the vinyl aromatic monomer (a) and the conjugated diene monomer (b) may be in the range of 85.0 to 99.0 wt %, preferably 90.0 to 98.0 wt %, more preferably 92.0 to 98 wt %, even more preferably 95.0 to 98.0 wt %, most preferably 95.0 to 98.0 wt %, based on the total weight of the monomers in the monomer mixture.

[0073] The mixture of ethylenically unsaturated monomers of the present invention may contain (a) at least 40% by weight, such as at least 43% by weight, or at least 45% by weight, or at least 47% by weight, or at least 50% by weight, or at least 53% by weight, or at least 55% by weight, or at least 57% by weight, or at least 60% by weight of vinyl aromatic monomers, based on the total weight of monomers in the monomer mixture. The mixture of ethylenically unsaturated monomers of the present invention may contain (a) 80% by weight or less, such as 78% by weight or less, or 75% by weight or less, or 70% by weight or less, or 68% by weight or less of vinyl aromatic monomers, based on the total weight of monomers in the monomer mixture. Those skilled in the art recognize that any range between any explicitly disclosed lower and upper limits is disclosed herein. Thus, the mixture of ethylenically unsaturated monomers may contain (a) 40 to 80% by weight, preferably 50 to 75% by weight, more preferably 55 to 70% by weight, and most preferably 60 to 70% by weight of vinyl aromatic monomers, based on the total weight of monomers in the monomer mixture.

[0074] According to the present invention, the vinyl aromatic monomer (a) may be selected from styrene, α-methylstyrene, vinyltoluene and combinations thereof. Preferably, the vinyl aromatic monomer (a) may be styrene.

[0075] The mixture of ethylenically unsaturated monomers of the present invention may contain (b) at least 15 wt %, such as at least 17 wt %, or at least 20 wt %, or at least 22 wt %, or at least 25 wt %, or at least 27 wt %, or at least 30 wt % of conjugated diene monomers, based on the total weight of monomers in the monomer mixture. The mixture of ethylenically unsaturated monomers of the present invention may contain (b) 50 wt % or less, such as 48 wt % or less, or 45 wt % or less, or 43 wt % or less, or 40 wt % or less, or 38 wt % or less of conjugated diene monomers, based on the total weight of monomers in the monomer mixture. One skilled in the art recognizes that any range between any explicitly disclosed lower and upper limits is disclosed herein. Thus, the mixture of ethylenically unsaturated monomers may contain (b) 15 to 50 wt %, preferably 20 to 45 wt %, more preferably 25 to 40 wt %, even more preferably 27 to 40 wt %, and most preferably 27 to 38 wt % of conjugated diene monomers, based on the total weight of monomers in the monomer mixture.

[0076] According to the present invention, the conjugated diene monomer (b) can be selected from 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2,4-hexadiene, 1,3-octadiene, 2-methyl-1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 3,4-dimethyl-1,3-hexadiene, 2,3-diethyl-1,3-butadiene, 4,5-diethyl-1,3-octadiene, 3-butyl-1,3-octadiene, 3,7-dimethyl-1,3,6-octatriene, 2-methyl-6-methylene-1,7-octadiene, 7-methyl-3-methylene-1,3-octadiene, 1,6-octadiene, 1,3,7-octatriene, 2-ethyl-1,3-butadiene, 2-pentyl-1,3-butadiene, 3,7-dimethyl-1,3,7-octatriene, 3,7-dimethyl-1,3,6-octatriene, 3,7,11-trimethyl-1,3,6,10-dodecatetraene, 7,11-dimethyl-3-methylene-1,6,10-dodecatriene, 2,6-dimethyl-2,4,6-octatriene, 2-phenyl-1,3-butadiene, 2-methyl-3-isopropyl-1,3-butadiene, 1,3-cyclohexadiene, myrcene, ocimene, farnesene and combinations thereof; preferably selected from 1,3-butadiene, isoprene and combinations thereof. The conjugated diene monomer (b) may be 1,3-butadiene.

[0077] The mixture of ethylenically unsaturated monomers of the present invention may contain (c) at least 0.2 wt%, such as at least 0.3 wt%, or at least 0.4 wt%, or at least 0.5 wt%, or at least 0.6 wt%, or at least 0.7 wt%, or at least 0.8 wt%, or at least 0.9 wt%, or at least 1.0 wt% of ethylenically unsaturated monomers having acid and / or hydroxyl functional groups, based on the total weight of monomers in the monomer mixture. The mixture of ethylenically unsaturated monomers of the present invention may contain (c) 6.0 wt% or less, such as 5.5 wt% or less, or 5.0 wt% or less, or 4.5 wt% or less, or 4.0 wt% or less of ethylenically unsaturated monomers having acid and / or hydroxyl functional groups, based on the total weight of monomers in the monomer mixture. One skilled in the art recognizes that any range between any explicitly disclosed lower and upper limits is disclosed herein. Thus, the mixture of ethylenically unsaturated monomers may comprise (c) 0.2 to 6.0 wt %, preferably 0.3 to 5.0 wt %, more preferably 0.5 to 4.0 wt %, even more preferably 0.7 to 4.0 wt %, most preferably 1.0 to 4.0 wt % of ethylenically unsaturated monomers having acid and / or hydroxyl functionality, based on the total weight of monomers in the monomer mixture.

[0078] The ethylenically unsaturated monomer (c) having an acid functional group that can be used in the present invention can be selected from ethylenically unsaturated carboxylic acid monomers, ethylenically unsaturated sulfonic acid monomers, ethylenically unsaturated phosphorus acid monomers and combinations thereof. The ethylenically unsaturated carboxylic acid monomers suitable for use in the present invention may include monocarboxylic acid and dicarboxylic acid monomers, monoesters of dicarboxylic acids, carboxyalkyl esters of ethylenically unsaturated acids such as 2-carboxyethyl (meth)acrylate, and ethylenically unsaturated carboxylic acid derivatives such as ethylenically unsaturated dicarboxylic acid anhydrides. For the purpose of the present invention, it is preferred to use ethylenically unsaturated aliphatic mono- or dicarboxylic acids or anhydrides containing 3 to 5 carbon atoms. Examples of the monocarboxylic acid monomers include (meth)acrylic acid, crotonic acid; and examples of the dicarboxylic acid monomers include fumaric acid, itaconic acid, maleic acid and maleic anhydride.

[0079] Examples of the ethylenically unsaturated sulfonic acid monomer include vinyl sulfonic acid, phenyl vinyl sulfonate, sodium 4-vinylbenzenesulfonate, 2-methyl-2-propylene-1-sulfonic acid, 2-propylene-1-sulfonic acid, 4-styrenesulfonic acid, 3-allyloxy-2-hydroxy-1-propanesulfonic acid, 2-acrylamido-2-methyl-1-propanesulfonic acid, and salts thereof.

[0080] Examples of the ethylenically unsaturated phosphorus acid monomer include vinylphosphonic acid, dimethyl vinylphosphonate, diethyl vinylphosphonate, diethyl allylphosphonate, allylphosphonic acid and salts thereof.

[0081] Preferably, the ethylenically unsaturated monomer (c) having an acid functional group is selected from ethylenically unsaturated carboxylic acid monomers, ethylenically unsaturated sulfonic acid monomers, ethylenically unsaturated phosphorus acid monomers and combinations thereof; preferably selected from (meth) acrylic acid, crotonic acid, fumaric acid, itaconic acid, maleic acid, maleic anhydride, vinyl acetate, vinyl lactic acid, vinyl sulfonic acid, styrene sulfonic acid, (meth) acrylate 2-carboxyethyl, vinyl sulfonate phenyl, 4-vinylbenzene sulfonate sodium, 2-methyl-2-propylene-1-sulfonic acid, 2-propylene-1-sulfonic acid, 4-styrene sulfonic acid, 2-acrylamido-2-methyl-1-propane sulfonic acid, vinyl phosphonic acid, vinyl phosphonic acid dimethyl ester, vinyl phosphonic acid diethyl ester, allyl phosphonic acid diethyl ester, allyl phosphonic acid and combinations thereof. More preferably, the ethylenically unsaturated monomer (c) having an acid functional group is selected from (meth) acrylic acid, itaconic acid and combinations thereof.

[0082] The ethylenically unsaturated monomer (c) having a hydroxyl functional group that can be used in the present invention can be selected from allyl alcohol, vinyl alcohol, N-hydroxymethyl (meth) acrylamide, 1-penten-3-ol, hydroxyalkyl esters of ethylenically unsaturated acids and combinations thereof, preferably hydroxyalkyl esters of ethylenically unsaturated acids.

[0083] The hydroxyalkyl ester of the ethylenically unsaturated acid may include hydroxyalkyl acrylate and methacrylate monomers based on ethylene oxide, propylene oxide and higher alkylene oxides or mixtures thereof. Suitable examples of the hydroxyalkyl ester of the ethylenically unsaturated acid may be selected from hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxyethyl caprolactone acrylate and combinations thereof.

[0084] The ethylenically unsaturated monomer (c) having acid and hydroxyl functional groups which can be used in the present invention can be selected from 3-allyloxy-2-hydroxy-1-propanesulfonic acid.

[0085] The ethylenically unsaturated monomer (c) having acid and / or hydroxyl functional groups which can be used in the present invention can be selected from (meth)acrylic acid, crotonic acid, fumaric acid, itaconic acid, maleic acid, maleic anhydride, vinyl acetate, vinyl lactic acid, vinyl sulfonic acid, styrene sulfonic acid, 2-carboxyethyl (meth)acrylate, phenyl vinyl sulfonate, sodium 4-vinylbenzenesulfonate, 2-methyl-2-propylene-1-sulfonic acid, 2-propylene-1-sulfonic acid, 4-styrenesulfonic acid, 2-acrylamido-2-methyl-1-propanesulfonic acid, vinylphosphonic acid, dimethyl vinylphosphonate, diethyl vinylphosphonate, diethyl allylphosphonate, allylphosphonic acid, allyl alcohol, vinyl alcohol, N-hydroxymethyl (methyl) 3-allyloxy-2-hydroxy-1-propanesulfonic acid, preferably selected from (meth)acrylic acid, itaconic acid; hydroxyalkyl esters of ethylenically unsaturated acids, such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate and hydroxyethyl hexalactone acrylate; and combinations thereof; more preferably selected from (meth)acrylic acid, itaconic acid, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate and combinations thereof.

[0086] According to the present invention, the mixture of ethylenically unsaturated monomers may comprise:

[0087] (a) 40 to 80 wt %, preferably 50 to 75 wt %, more preferably 55 to 70 wt %, most preferably 60 to 70 wt % of vinyl aromatic monomers;

[0088] (b) 15 to 50 wt %, preferably 20 to 45 wt %, more preferably 25 to 40 wt %, even more preferably 27 to 40 wt %, most preferably 27 to 38 wt % of a conjugated diene monomer; and

[0089] (c) 0.2 to 6.0 wt. %, preferably 0.3 to 5.0 wt. %, more preferably 0.5 to 4.0 wt. %, even more preferably 0.7 to 4.0 wt. %, most preferably 1.0 to 4.0 wt. % of ethylenically unsaturated monomers having acid and / or hydroxy functionality, based on the total weight of the monomers in the monomer mixture.

[0090] According to the present invention, the mixture of ethylenically unsaturated monomers may comprise:

[0091] (a) 40 to 80 wt %, preferably 50 to 75 wt %, more preferably 55 to 70 wt %, most preferably 60 to 70 wt % of vinyl aromatic monomers;

[0092] (b) 15 to 50 wt %, preferably 20 to 45 wt %, more preferably 25 to 40 wt %, even more preferably 27 to 40 wt %, most preferably 27 to 38 wt % of a conjugated diene monomer; and

[0093] (c) 0.2 to 6.0 wt. %, preferably 0.3 to 5.0 wt. %, more preferably 0.5 to 4.0 wt. %, even more preferably 0.7 to 4.0 wt. %, most preferably 1.0 to 4.0 wt. % of ethylenically unsaturated monomers having acid and / or hydroxy functionality, based on the total weight of the monomers in the monomer mixture;

[0094] The vinyl aromatic monomer (a) is selected from styrene, α-methylstyrene, vinyltoluene and combinations thereof, preferably styrene;

[0095] The conjugated diene monomer (b) is selected from 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2,4-hexadiene, 1,3-octadiene, 2-methyl-1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 3,4-dimethyl-1,3-hexadiene, 2,3-diethyl-1,3-butadiene, 4,5-diethyl-1,3-octadiene, 3-butyl-1,3-octadiene, 3,7-dimethyl-1,3,6-octatriene, 2-methyl-6-methylene-1,7-octadiene, 7-methyl-3-methylene-1,6-octadiene, 1,3,7-octatriene, 2-ethyl-1,3-butadiene, 2-pentyl-1,3-butadiene, 3,7-dimethyl-1,3,7-octatriene, 3,7-dimethyl-1,3,6-octatriene, 3,7,11-trimethyl-1,3,6,10-dodecatetraene, 7,11-dimethyl-3-methylene-1,6,10-dodecatriene, 2,6-dimethyl-2,4,6-octatriene, 2-phenyl-1,3-butadiene, 2-methyl-3-isopropyl-1,3-butadiene, 1,3-cyclohexadiene, myrcene, ocimene, farnesene and combinations thereof, preferably selected from 1,3-butadiene, isoprene and combinations thereof, more preferably 1,3-butadiene,

[0096] The ethylenically unsaturated monomer (c) having an acid and / or hydroxyl functional group is selected from (meth)acrylic acid, crotonic acid, fumaric acid, itaconic acid, maleic acid, maleic anhydride, vinyl acetate, vinyl lactic acid, vinyl sulfonic acid, styrene sulfonic acid, 2-carboxyethyl (meth)acrylate, phenyl vinyl sulfonate, sodium 4-vinylbenzenesulfonate, 2-methyl-2-propylene-1-sulfonic acid, 2-propylene-1-sulfonic acid, 4-styrenesulfonic acid, 2-acrylamido-2-methyl-1-propanesulfonic acid, vinylphosphonic acid, dimethyl vinylphosphonate, diethyl vinylphosphonate, diethyl allylphosphonate, allylphosphonic acid, allyl alcohol, vinyl alcohol, N-hydroxymethyl (meth)propylene amide, 1-penten-3-ol; hydroxyalkyl esters of ethylenically unsaturated acids, such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate and hydroxyethyl caprolactone acrylate; and 3-allyloxy-2-hydroxy-1-propanesulfonic acid, preferably selected from (meth)acrylic acid, itaconic acid; hydroxyalkyl esters of ethylenically unsaturated acids, such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate and hydroxyethyl caprolactone acrylate; and combinations thereof; more preferably selected from (meth)acrylic acid, itaconic acid, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate and combinations thereof.

[0097] According to the present invention, the weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) is at least 1.60, such as at least 1.62, or at least 1.65, or at least 1.67, or at least 1.70. The weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) is no more than 2.30, such as no more than 2.25, or no more than 2.20, or no more than 2.15, or no more than 2.10. Those skilled in the art recognize that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) can be in the range of 1.62 to 2.25, preferably 1.65 to 2.20, more preferably 1.70 to 2.15, and most preferably 1.70 to 2.10.

[0098] According to the present invention, the polymer latex has a median particle size of at least 220 nanometers, preferably at least 230 nanometers, and more preferably at least 250 nanometers. The polymer latex may have a median particle size of no more than 400 nanometers, such as no more than 350 nanometers, or no more than 300 nanometers. Those skilled in the art recognize that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the polymer latex may have a median particle size in the range of 220 nanometers to 400 nanometers, preferably 230 nanometers to 400 nanometers, and more preferably 250 nanometers to 400 nanometers. The median particle size can be determined according to ISO 22412:2017 by dynamic light scattering, for example, using a dynamic light scattering device Mastersizer 2000 (Malvern Panalytical (UK)).

[0099] The mixture of ethylenically unsaturated monomers may contain a chain transfer agent. According to the present invention, the mixture of ethylenically unsaturated monomers may contain at least 0.05% by weight, such as at least 0.07% by weight, or at least 0.10% by weight, or at least 0.12% by weight, or at least 0.15% by weight of chain transfer agent, wherein the weight percentage is based on the total amount of monomers in the monomer mixture. The mixture of ethylenically unsaturated monomers may contain 3.0% by weight or less, such as 2.5% by weight or less, or 2.0% by weight or less, or 1.5% by weight or less of chain transfer agent, wherein the weight percentage is based on the total amount of monomers in the monomer mixture. Those skilled in the art recognize that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the mixture of ethylenically unsaturated monomers may contain 0.05 to 3.0% by weight, preferably 0.10 to 2.0% by weight, and more preferably 0.15 to 1.5% by weight of chain transfer agent, wherein the weight percentage is based on the total amount of monomers in the monomer mixture.

[0100] The chain transfer agent can be selected from n-dodecyl mercaptan, carbon tetrachloride, carbon tetrabromide, bromotrichloromethane, 4-methylbenzenethiol, isooctyl 3-mercaptopropionate, tert-nonyl mercaptan, 4,4′-thiobisbenzenethiol, tert-dodecyl mercaptan, α-methylstyrene dimer, thioglycolic acid, 2-ethylhexyl thioglycolate, butyl 3-mercaptopropionate, 1,8-dimercapto-3,6-dioxaoctane and combinations thereof, more preferably tert-dodecyl mercaptan.

[0101] The mixture of ethylenically unsaturated monomers may further comprise (d) an ethylenically unsaturated monomer different from (a) to (c). According to the present invention, the mixture of ethylenically unsaturated monomers may further comprise (d) 0 to 20% by weight, preferably 0 to 15% by weight, more preferably 0 to 10% by weight of an ethylenically unsaturated monomer different from (a) to (c), based on the total weight of monomers in the monomer mixture. The ethylenically unsaturated monomer different from (a) to (c) may be selected from (d1) an ethylenically unsaturated nitrile compound, (d2) an alkyl ester of an ethylenically unsaturated acid, (d3) an ethylenically unsaturated compound with a primary or secondary amino group, and combinations thereof.

[0102] The ethylenically unsaturated nitrile compound (d1) may be selected from (meth)acrylonitrile, α-cyanoethylacrylonitrile, fumaronitrile, α-chloronitrile and combinations thereof.

[0103] The alkyl ester of the ethylenically unsaturated acid (d2) can be selected from methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate and combinations thereof, preferably methyl (meth)acrylate and combinations thereof.

[0104] The ethylenically unsaturated compound (d3) having a primary or secondary amino group can be selected from (meth)acrylamide, 2-aminoethyl (meth)acrylate hydrochloride, 2-aminoethyl (meth)acrylamide hydrochloride, N-ethyl (meth)acrylamide, N-(3-aminopropyl) (meth)acrylamide hydrochloride, N-hydroxyethyl (meth)acrylamide, N-3-(dimethylamino)propyl (meth)acrylamide, [3-(methacryloylamino)propyl]trimethylammonium, N-[tris (hydroxymethyl)methyl] (meth)acrylamide, N-phenylacrylamide, alkyl acrylamide, methacrylamide poly (ethylene glycol) amine hydrochloride and combinations thereof.

[0105] According to the present invention, the amounts of the above-defined monomers used for the preparation of the polymer latex may add up to 100% by weight, based on the total amount of monomers in the monomer mixture.

[0106] Method for preparing polymer latex

[0107] The present invention relates to a method for preparing a polymer latex for an adhesive, which comprises polymerizing a mixture of ethylenically unsaturated monomers by free radical emulsion polymerization. The mixture of ethylenically unsaturated monomers comprises (a) a vinyl aromatic monomer; (b) a conjugated diene monomer; and (c) an ethylenically unsaturated monomer having acid and / or hydroxyl functional groups. According to the present invention, the weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) is in the range of 1.60 to 2.30. The polymer latex of the present invention has a median particle size of at least 220 nanometers. The median particle size can be measured according to ISO 22412:2017 by dynamic light scattering, for example, using a dynamic light scattering device Mastersizer 2000 (Malvern Panalyt ical (UK)).

[0108] According to the present invention, the sum of the vinyl aromatic monomer (a) and the conjugated diene monomer (b) can be at least 85.0 weight %, such as at least 87.0 weight %, or at least 90.0 weight %, or at least 93.0 weight %, or at least 95.0 weight %, or at least 97.0 weight %, based on the total weight of the monomers in the monomer mixture. The sum of the vinyl aromatic monomer (a) and the conjugated diene monomer (b) can be 99.0 weight % or less, such as 98.5 weight % or less, or 98.0 weight % or less, or 97.5 weight % or less, based on the total weight of the monomers in the monomer mixture. Those skilled in the art recognize that any range between any clearly disclosed lower and upper limits is disclosed herein. Therefore, the sum of the vinyl aromatic monomer (a) and the conjugated diene monomer (b) may be in the range of 85.0 to 99.0 wt %, preferably 90.0 to 98.0 wt %, more preferably 92.0 to 98.0 wt %, even more preferably 95.0 to 98.0 wt %, most preferably 95.0 to 98.0 wt %, based on the total weight of monomers in the monomer mixture.

[0109] All variations as to the compounds and relative amounts used to prepare the polymer latexes of the present invention may be as described above.

[0110] According to the present invention, the weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) is at least 1.60, such as at least 1.62, or at least 1.65, or at least 1.67, or at least 1.70. The weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) is no more than 2.30, such as no more than 2.25, or no more than 2.20, or no more than 2.15, or no more than 2.10. Those skilled in the art recognize that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) can be in the range of 1.62 to 2.25, preferably 1.65 to 2.20, more preferably 1.70 to 2.15, and most preferably 1.70 to 2.10.

[0111] According to the present invention, the polymer latex has a median particle size of at least 220 nanometers, preferably at least 230 nanometers, and more preferably at least 250 nanometers. The polymer latex may have a median particle size of no more than 400 nanometers, such as no more than 350 nanometers, or no more than 300 nanometers. Those skilled in the art recognize that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the polymer latex may have a median particle size in the range of 220 nanometers to 400 nanometers, preferably 230 nanometers to 400 nanometers, and more preferably 250 nanometers to 400 nanometers. The median particle size can be determined according to ISO 22412:2017 by dynamic light scattering, for example, using a dynamic light scattering device Mastersizer 2000 (Malvern Panalytical (UK)).

[0112] The mixture of ethylenically unsaturated monomers may contain a chain transfer agent. According to the present invention, the mixture of ethylenically unsaturated monomers may contain at least 0.05% by weight, such as at least 0.07% by weight, or at least 0.10% by weight, or at least 0.12% by weight, or at least 0.15% by weight of chain transfer agent, wherein the weight percentage is based on the total amount of monomers in the monomer mixture. The mixture of ethylenically unsaturated monomers may contain 3.0% by weight or less, such as 2.5% by weight or less, or 2.0% by weight or less, or 1.5% by weight or less of chain transfer agent, wherein the weight percentage is based on the total amount of monomers in the monomer mixture. Those skilled in the art recognize that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the mixture of ethylenically unsaturated monomers contains 0.05 to 3.0% by weight, preferably 0.10 to 2.0% by weight, and more preferably 0.15 to 1.5% by weight of chain transfer agent, wherein the weight percentage is based on the total amount of monomers in the monomer mixture.

[0113] The chain transfer agent can be selected from n-dodecyl mercaptan, carbon tetrachloride, carbon tetrabromide, bromotrichloromethane, 4-methylbenzenethiol, isooctyl 3-mercaptopropionate, tert-nonyl mercaptan, 4,4′-thiobisbenzenethiol, tert-dodecyl mercaptan, α-methylstyrene dimer, thioglycolic acid, 2-ethylhexyl thioglycolate, butyl 3-mercaptopropionate, 1,8-dimercapto-3,6-dioxaoctane and combinations thereof, more preferably tert-dodecyl mercaptan.

[0114] The mixture of ethylenically unsaturated monomers may further comprise (d) an ethylenically unsaturated monomer different from (a) to (c). According to the present invention, the mixture of ethylenically unsaturated monomers may further comprise (d) 0 to 20% by weight, preferably 0 to 15% by weight, more preferably 0 to 10% by weight of an ethylenically unsaturated monomer different from (a) to (c), based on the total weight of the monomers in the monomer mixture. The ethylenically unsaturated monomer different from (a) to (c) may be selected from (d1) an ethylenically unsaturated nitrile compound, (d2) an alkyl ester of an ethylenically unsaturated acid, (d3) an ethylenically unsaturated compound with a primary or secondary amino group, and combinations thereof.

[0115] The ethylenically unsaturated nitrile compound (d1) may be selected from (meth)acrylonitrile, α-cyanoethylacrylonitrile, fumaronitrile, α-chloronitrile and combinations thereof.

[0116] The alkyl ester of the ethylenically unsaturated acid (d2) can be selected from methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate and combinations thereof, preferably methyl (meth)acrylate and combinations thereof.

[0117] The ethylenically unsaturated compound (d3) having a primary or secondary amino group can be selected from (meth)acrylamide, 2-aminoethyl (meth)acrylate hydrochloride, 2-aminoethyl (meth)acrylamide hydrochloride, N-ethyl (meth)acrylamide, N-(3-aminopropyl) (meth)acrylamide hydrochloride, N-hydroxyethyl (meth)acrylamide, N-3-(dimethylamino)propyl (meth)acrylamide, [3-(methacryloylamino)propyl]trimethylammonium, N-[tris (hydroxymethyl)methyl] (meth)acrylamide, N-phenylacrylamide, alkyl acrylamide, methacrylamide poly (ethylene glycol) amine hydrochloride and combinations thereof.

[0118] According to the invention, the above-defined monomers for the preparation of the polymer latex may be added in an amount of up to 100% by weight, based on the total amount of monomers in the monomer mixture.

[0119] The polymer latex of the present invention may be prepared by any emulsion polymerization method known to those skilled in the art, provided that a monomer mixture as defined herein is used.

[0120] In the emulsion polymerization for preparing the polymer latex of the present invention, a seed dispersion may be used. Any seed particles as already known by those skilled in the art may be used.

[0121] The seed particles are preferably present in an amount of 0.01 to 10 parts by weight, preferably 0.1 to 5 parts by weight, based on 100 parts by weight of the total ethylenically unsaturated monomers used in the polymer. Therefore, the lower limit of the amount of the seed particles can be 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4 or 2.5 parts by weight. The upper limit of the amount can be 10, 9, 8, 7, 6, 5.5, 5, 4.5, 4, 3.8, 3.6, 3.4, 3.3, 3.2, 3.1 or 3 parts by weight. One skilled in the art will understand that any range formed by any explicitly disclosed lower and upper limits is expressly included in this patent specification.

[0122] The process for preparing the above-mentioned polymer latex can be carried out in the absence of one or more emulsifiers, in the absence of one or more protective colloids and in the presence of one or more initiators at a temperature of 0 to 130° C., preferably 0 to 100° C., particularly preferably 20 to 95° C., very particularly preferably 40 to 90° C. This temperature includes all values ​​and subvalues ​​therebetween, in particular including 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120 and 125° C.

[0123] Initiators that can be used when carrying out the present invention may include water-soluble and / or oil-soluble initiators that are effective for polymerization purposes. Representative initiators are well known in the art and include, for example: azo compounds (such as, for example, AIBN, AMBN, and cyanovaleric acid); and inorganic peroxy compounds, such as hydrogen peroxide, sodium, potassium, and ammonium peroxodisulfates, peroxycarbonates, and peroxyborates; and organic peroxy compounds, such as alkyl hydroperoxides, dialkyl peroxides, acyl hydroperoxides, and diacyl peroxides; and esters, such as tert-butyl perbenzoate; and combinations of inorganic and organic initiators.Suitable initiators may be selected from 2,3-dimethyl-2,3-diphenylbutane, tert-butyl hydroperoxide, tert-amyl hydroperoxide, cumyl hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, isopropylcumyl hydroperoxide, p-menthane hydroperoxide, 2,5-di(tert-butylperoxy)-2,5-dimethyl-3-hexyne, 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane, di(tert-butyl peroxide), 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, di(tert-butylperoxy-isopropyl)benzene, tert-butylcumyl peroxide, di-(tert-amyl)-peroxy compounds, dicumyl peroxide, butyl 4,4-di(tert-butylperoxy)valerate, tert-butyl peroxybenzoate, 2,2-di(tert-butylperoxy)butane, tert-amyl peroxybenzoate, tert-butyl peroxyacetate, tert-butyl peroxy(2-ethylhexyl)carbonate, tert-butyl peroxyisopropylcarbonate, tert-butyl peroxy-3,5,5-trimethyl-hexanoate, 1,1-di(tert-butylperoxy)cyclohexane, tert-amyl peroxyacetate, tert-amyl peroxy(2-ethylhexyl)carbonate, 1,1-di(tert-butylperoxy)-3,5,5-trimethylcyclohexane, 1,1-di(tert-amylperoxy)cyclohexane, tert-butyl-monoperoxy 1,1′-azobis(hexahydrobenzonitrile), tert-butyl peroxyisobutyrate, tert-butyl peroxydiethyl acetate, tert-butyl peroxy-2-ethylhexanoate, dibenzoyl peroxide, tert-amyl peroxy-2-ethylhexanoate, di(4-methylbenzoyl)peroxide, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, ammonium peroxodisulfate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, 2,2′-azobis(2-methylbutyronitrile), 2,2′-azobis(isobutyronitrile), didecanoyl peroxide, potassium persulfate, dilauroyl peroxide, di(3,5 ,5-trimethylhexanoyl), tert-amyl peroxypivalate, tert-butyl peroxyneoheptanoate, 1,1,3,3-tetramethylbutyl peroxypivalate, tert-butyl peroxypivalate, dicetyl peroxydicarbonate, dimyristyl peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, di(4-tert-butylcyclohexyl) peroxydicarbonate, diisopropyl peroxydicarbonate, tert-butyl peroxyneodecanoate, di-sec-butyl peroxydicarbonate, tert-amyl peroxyneodecanoate, cumyl peroxyneoheptanoate, di(3-methoxybutyl) peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, cumyl peroxyneodecanoate, diisobutyryl peroxide, and mixtures thereof.

[0124] The initiator may be used in sufficient amounts to initiate polymerization at a desired rate. Generally, an initiator amount of 0.01 to 5 wt %, preferably 0.1 to 4 wt %, based on the total weight of the monomers in the monomer mixture is sufficient. The initiator amount is most preferably 0.01 to 2 wt %, based on the total weight of the monomers in the monomer mixture. The initiator amount includes all values ​​and subvalues ​​therebetween, particularly including 0.01, 0.1, 0.5, 1, 1.5, 2, 2.5, 3, 4 and 4.5 wt %, based on the total weight of the monomers in the monomer mixture.

[0125] The above-mentioned inorganic and organic peroxy compounds may also be used alone or in combination with one or more suitable reducing agents as known in the art. Examples of such reducing agents may include sulfur dioxide, alkali metal pyrosulfites, alkali metal bisulfites and ammonium bisulfites, thiosulfates, dithionites and formaldehyde sulfoxylates, and hydroxylamine hydrochlorides, hydrazine sulfates, iron (II) sulfate, cuprous naphthenate, glucose, sulfonic acid compounds such as sodium methanesulfonate, amine compounds such as dimethylaniline and ascorbic acid. The amount of the reducing agent is preferably 0.03 to 10 parts by weight per part by weight of the polymerization initiator.

[0126] The surfactant or emulsifier suitable for stabilizing the dispersion polymer may include those conventional surface active agents used in polymerization methods. The surfactant may be added to the aqueous phase and / or the monomer phase. The effective amount of the surfactant during the inoculation process is an amount selected to support the particle stability as a colloid, minimize the contact between the particles and prevent solidification. In the non-inoculation process, the effective amount of the surfactant is an amount selected to determine the particle size.

[0127] Representative surfactants include saturated and ethylenically unsaturated sulfonic acids or their salts, including, for example, unsaturated hydrocarbon sulfonic acids, such as vinyl sulfonic acid, allyl sulfonic acid and methallyl sulfonic acid, and their salts; aromatic hydrocarbon acids, such as, for example, p-styrene sulfonic acid, isopropenylbenzenesulfonic acid and vinyloxybenzenesulfonic acid and their salts; sulfoalkyl esters of acrylic and methacrylic acid, such as, for example, sulfoethyl methacrylate and sulfopropyl methacrylate and their salts, and 2-acrylamido-2-methylpropanesulfonic acid and its salts; alkylated oxidized diphenyl disulfonates, sodium dodecylbenzenesulfonate and dihexyl or dioctyl esters of sodium sulfosuccinate, sodium alkyl esters of sulfonic acids, ethoxylated alkylphenols and ethoxylated alcohols; fatty alcohol sulfates and fatty alcohol (poly)ether sulfates.

[0128] The type and amount of the surfactant are typically governed by the number of particles, their size and their composition. Typically, the surfactant is used in an amount of 0 to 20 weight %, preferably 0 to 10 weight %, more preferably 0 to 5 weight %, based on the total weight of the monomers in the monomer mixture. The amount of the surfactant includes all values ​​and subvalues ​​therebetween, particularly including 0, 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18 and 19 weight %, based on the total weight of the monomers in the monomer composition. The polymerization can be carried out without the use of a surfactant.

[0129] The polymer latex of the present invention may further comprise a protective colloid. The protective colloid may comprise polyvinyl alcohol, vinyl alcohol-ethylene copolymer, polyvinyl alcohol modified by silanol, cellulose derivatives such as methylcellulose, ethylcellulose, hydroxycellulose and carboxylcellulose; chitin, chitosan, starches, polyethylene glycol, polypropylene glycol, polyvinyl ether, gelatin, casein, cyclodextrin and combinations thereof. The protective colloid may stabilize the polymer latex in addition to or in place of the surfactants described above. The protective colloid may be present during polymerization or added later. A typical amount is 1 to 15 parts by weight, based on 100 parts by weight of the polymer latex.

[0130] Water-based adhesive composition

[0131] The present invention relates to the use of the polymer latex as described above or the polymer latex of the present invention prepared by the method as described above for preparing an aqueous adhesive composition. Preferably, the aqueous adhesive composition of the present invention is a two-component composition.

[0132] As used herein, a "two-component" or "2K" composition is a composition in which, when mixed, at least a portion of the reactive components readily react and at least partially cure without activation from an external energy source, such as at ambient temperature, e.g., a temperature in the range of 20 to 25° C., or slightly elevated temperature, e.g., a temperature in the range of 25° C. to 60° C. It is understood by those skilled in the art that the two components of the composition are stored separately from one another and mixed just prior to applying the composition.

[0133] As used herein, the term "aqueous" means a medium consisting exclusively of water or mainly comprising water (e.g., at least 50 % by weight water) and in combination with a non-aqueous solvent. If necessary, a small amount of non-aqueous solvent can be used in the aqueous adhesive composition of the present invention. The amount of the non-aqueous solvent can be 3 % by weight or less, preferably 2 % by weight or less, more preferably 1.5 % by weight or less, most preferably 1 % by weight or less and particularly 0.5 % by weight or less, based on the solid content of the aqueous adhesive composition. The example of suitable non-aqueous solvent includes but is not limited to toluene, acetone, methyl ethyl ketone, cyclohexane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol methyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ether, dimethyl formamide, dimethyl sulfoxide, monoalcohols such as methanol and ethanol, and polyols. The aqueous adhesive composition is preferably free of non-aqueous solvent.

[0134] Furthermore, the present invention relates to an aqueous adhesive composition comprising (i) the polymer latex of the present invention as described above or the polymer latex of the present invention prepared by the method of the present invention as described above, and (ii) a polyisocyanate compound.

[0135] All variations concerning the polymer latex and concerning the compounds used to prepare the polymer latex of the present invention and their relative amounts may be as described above.

[0136] According to the present invention, the aqueous adhesive composition can include at least 15% by weight, such as at least 17% by weight, or at least 20% by weight, or at least 23% by weight of polymer latex (i), based on the total solids content of the aqueous adhesive composition. The aqueous adhesive composition can include up to 50% by weight, such as up to 48% by weight, or up to 45% by weight, or up to 43% by weight, or up to 40% by weight of polymer latex (i), based on the total solids content of the aqueous adhesive composition. Those skilled in the art recognize that any scope between the lower limit and the upper limit clearly disclosed is disclosed herein. Therefore, the aqueous adhesive composition can include 15 to 50% by weight, preferably 17 to 45% by weight, and more preferably 20 to 40% by weight of polymer latex (i), based on the total solids content of the aqueous adhesive composition.

[0137] As used herein, the term "polyisocyanate" refers to a compound having more than one isocyanate group per molecule, for example, 2, 3, 4, 5, 6 or more isocyanate groups per molecule. Suitable polyisocyanates may be aliphatic, aromatic or mixtures thereof. The polyisocyanate may include toluene diisocyanate, hydrogenated toluene diisocyanate, methylene diphenyl diisocyanate, hydrogenated methylene diphenyl diisocyanate, triphenylmethane triisocyanate, 1,2,4-benzene triisocyanate, polymethylene polyphenyl polyisocyanate, xylene diisocyanate, tetramethylxylene diisocyanate, 1,6-hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, isophorone diisocyanate and 4,4′-methylene-bis(cyclohexyl isocyanate). Suitable polyisocyanates that may be used according to the present invention may be exemplified by the Bayhydur and Desmodur grades of polyisocyanates commercially available from Covestro (Germany), and the Suprasec grades of polyisocyanates commercially available from Huntsman Corporation (USA).

[0138] The aqueous adhesive composition may include at least 1% by weight, such as at least 2% by weight, or at least 5% by weight, or at least 7% by weight of polyisocyanate compound (ii), based on the total solid content of the aqueous adhesive composition. The aqueous adhesive composition may include up to 50% by weight, such as up to 48% by weight, or up to 45% by weight, or up to 43% by weight, or up to 40% by weight of polyisocyanate compound (ii), based on the total solid content of the aqueous adhesive composition. Those skilled in the art recognize that any scope between any clearly disclosed lower and upper limits is disclosed herein. Therefore, the aqueous adhesive composition may include 1 to 50% by weight, preferably 2 to 45% by weight, and more preferably 5 to 40% by weight of polyisocyanate compound (ii), based on the total solid content of the aqueous adhesive composition.

[0139] The aqueous adhesive composition of the present invention may further comprise polyvinyl alcohol, vinyl alcohol-ethylene copolymer, polyvinyl alcohol modified by silanol; cellulose derivatives such as methylcellulose, ethylcellulose, hydroxy cellulose and carboxyl cellulose; chitin, chitosan, starch, polyethylene glycol, polypropylene glycol, polyvinyl ether, gelatin, casein, cyclodextrin and combinations thereof. Preferably, the aqueous adhesive composition of the present invention further comprises polyvinyl alcohol. As used herein, the term "polyvinyl alcohol" is generally recognized in the art as fully or partially hydrolyzed polyvinyl acetate. Polyvinyl alcohol may have a saponification degree of up to 99%. As used herein, the term "degree of saponification" represents the ratio of hydroxyl groups to the total number of hydroxyl groups and carbonyl groups such as acetoxy groups in the polyvinyl alcohol. The degree of saponification must be understood as an average value, which means that a mixture of less hydrolyzed and more hydrolyzed polyvinyl alcohols can be used. Preferably, a degree of saponification in the range of 70 to 99% is used, more preferably 80 to 97%. Examples of suitable polyvinyl alcohols include, but are not limited to, Poval grade polyvinyl alcohols commercially available from Kuraray (Japan).

[0140] According to the present invention, polyvinyl alcohol, vinyl alcohol-ethylene copolymer, polyvinyl alcohol modified by silanol; cellulose derivatives such as methylcellulose, ethylcellulose, hydroxycellulose and carboxycellulose; chitin, chitosan, starch, polyethylene glycol, polypropylene glycol, polyvinyl ether, gelatin, casein, cyclodextrin and combinations thereof can be used in an amount of at least 3 weight %, such as at least 5 weight %, or at least 7 weight %, or at least 9 weight %, based on the total solid content of the aqueous adhesive composition. The polyvinyl alcohol, vinyl alcohol-ethylene copolymer, polyvinyl alcohol modified by silanol; cellulose derivatives such as methylcellulose, ethylcellulose, hydroxycellulose and carboxycellulose; chitin, chitosan, starch, polyethylene glycol, polypropylene glycol, polyvinyl ether, gelatin, casein, cyclodextrin and combinations thereof can be used in an amount of up to 60 weight %, such as up to 50 weight %, or up to 45 weight %, or up to 40 weight %, based on the total solid content of the aqueous adhesive composition. Those skilled in the art recognize that any range between any explicitly disclosed lower and upper limits is disclosed herein. In addition, the polyvinyl alcohol, vinyl alcohol-ethylene copolymer, polyvinyl alcohol modified by silanol; cellulose derivatives, such as methyl cellulose, ethyl cellulose, hydroxy cellulose and carboxy cellulose; chitin, chitosan, starch, polyethylene glycol, polypropylene glycol, polyvinyl ether, gelatin, casein, cyclodextrin and combinations thereof can be used in an amount of 3 to 60 weight %, preferably from 5 to 50 weight %, more preferably 7 to 40 weight %, based on the total solid content of the aqueous adhesive composition.

[0141] This aqueous adhesive composition can comprise at least 3 % by weight, such as at least 5 % by weight, or at least 7 % by weight polyvinyl alcohol, based on the total solids content of this aqueous adhesive composition. This aqueous adhesive composition can comprise up to 60 % by weight, such as up to 50 % by weight, or up to 45 % by weight, or up to 40 % by weight polyvinyl alcohol, based on the total solids content of this aqueous adhesive composition. Those skilled in the art recognize that any scope between the lower limit and the upper limit clearly disclosed is disclosed herein. Therefore, this aqueous adhesive composition can comprise 3 to 60 % by weight, preferably 5 to 50 % by weight, more preferably 7 to 40 % by weight polyvinyl alcohol, based on the total solids content of this aqueous adhesive composition.

[0142] Optionally, the aqueous adhesive composition may further comprise a polymer latex different from those of the present invention, such as polyvinyl acetate, vinyl acetate-ethylene copolymers, polyurethanes, acrylonitrile-butadiene copolymers and combinations thereof, preferably polyvinyl acetate, vinyl acetate-ethylene copolymers and combinations thereof. The aqueous adhesive composition may comprise up to 40% by weight, such as up to 30% by weight, or up to 20% by weight, or up to 10% by weight, or up to 5% by weight of a polymer latex different from those of the present invention, preferably polyvinyl acetate, vinyl acetate-ethylene copolymers, the weight percentage being based on the total solid content of the aqueous adhesive composition.

[0143] The aqueous adhesive composition may further include additives such as plasticizers, antifoaming agents, thickeners, levelers, dispersants, colorants, water-resistant additives, lubricants, pH adjusters, bactericides, antioxidants, inorganic pigments, surfactants and combinations thereof. These additives may be used in an amount ranging from 0.1 to 30% by weight, based on the total solid content of the aqueous adhesive composition.

[0144] The aqueous adhesive composition may include fillers or extenders, inorganic pigments and combinations thereof. Suitable examples of inorganic pigments, fillers or extenders include metal oxides, hydroxides, sulfides, carbonates, sulfates or silicate compounds of magnesium, calcium, zinc, barium, titanium, aluminum, antimony and lead; preferably calcium carbonate, kaolin, talc, titanium dioxide, aluminum hydroxide, silicon dioxide, gypsum, barium oxide powder, alumina white and satin white. The fillers or extenders, inorganic pigments and combinations thereof can be used in an amount ranging from 30 to 60% by weight, based on the total solid content of the aqueous adhesive composition.

[0145] According to the present invention, the aqueous adhesive composition can be a two-component adhesive composition. Typically, the first component comprises the polymer latex of the present invention, and the second component comprises the polyisocyanate compound. The first component may further comprise polyvinyl alcohol, vinyl alcohol-ethylene copolymer, polyvinyl alcohol modified by silanol; cellulose derivatives such as methyl cellulose, ethyl cellulose, hydroxy cellulose and carboxyl cellulose; chitin, chitosan, starch, polyethylene glycol, polypropylene glycol, polyvinyl ether, gelatin, casein, cyclodextrin and combinations thereof. Preferably, the first component further comprises polyvinyl alcohol. The first component may further comprise additives, fillers or extenders, inorganic pigments and combinations thereof.

[0146] The aqueous adhesive of the present invention may be in the form of a wood glue. As used herein, the term "wood glue" refers to an adhesive that firmly bonds wood pieces together. In particular, the aqueous adhesive is in the form of a D4 wood glue. As used herein, the term "D4 wood glue" refers to a wood glue suitable for use in interiors that are often exposed to tap water or condensation for a long period of time and / or in exteriors that are exposed to the weather. According to European Standard EN 204:2001, a D4 wood glue has a strength of more than 4 N / mm 2 of bonding strength.

[0147] The present invention further relates to a method for preparing an aqueous adhesive composition, comprising: providing (i) the polymer latex of the present invention or a polymer latex prepared by the method for preparing a polymer latex of the present invention; and mixing with (ii) a polyisocyanate compound.

[0148] All variations with respect to the compounds and their relative amounts used to prepare the aqueous adhesive composition of the present invention may be as described above.

[0149] The aqueous adhesive of the present invention may be in the form of wood glue. Preferably, the aqueous adhesive is in the form of D4 wood glue.

[0150] The present invention will be further illustrated with reference to the following examples.

[0151] Example:

[0152] In the following, all parts and percentages are by weight unless otherwise specifically specified.

[0153] Preparation of styrene butadiene polymer (XSBR) latex

[0154] The polymer latex compositions used in Examples and Comparative Examples were produced by free radical emulsion polymerization in a pressure-resistant stainless steel reactor connected to a cryostat capable of controlling the jacket temperature of the reactor.

[0155] The initial charge in the reactor consisted of 66 pphm (parts by weight, based on 100 parts of total monomer weight) of deionized water and polystyrene seeds having an average particle size of 35 nm (the amount of seeds for each example is tabulated in Tables 1 and 2). After heating the initial charge to 85° C. under continuous agitation using a three-layer beam stirrer, the polymerization reaction was initiated by starting to feed a 3.5% (w / w) sodium persulfate solution (1 pphm). The temperature was maintained constant at 85° C. for 2 minutes after the start of the persulfate feed, and the monomers (the amounts for each example are tabulated in Tables 1 and 2), the chain transfer agent tert-dodecyl mercaptan, and the anionic surfactant (0.5 pphm of sulfonic acid C 2+) were added at a constant feed rate over a period of five hours. 13 -C 15 An aqueous solution of 1,2-dihydro-1,4-dihydro-2-yl 4-(2-(2-alkyl aryl ester)) was added to the reactor. After that, a post-activation feed containing 0.25 pphm sodium persulfate was started to reduce residual monomers and continued for one hour at a batch temperature of 90°C. After completion of the sodium persulfate addition, the batch was kept at 90°C for a further 30 minutes with continuous stirring. The product was then allowed to cool down to ambient temperature, the pH was adjusted to 5 using a 10 wt. % aqueous sodium hydroxide solution and the total solids content of the final latex was adjusted to 47.5 wt. %. Finally, the latex was screened on a filter cloth with a mesh width of 50 μm.

[0156] The particle size of the latex was measured by dynamic light scattering according to ISO 22412:2017 using a dynamic light scattering device Mastersizer 2000 (Malvern Panalyt ical (UK)).

[0157] Table 1: Examples 1 to 6

[0158]

[0159]

[0160] Table 2: Examples 7 to 12

[0161]

[0162] Wood glue preparation

[0163] A wood glue comprising the polymer latex obtained as described above is prepared. The wood glue consists of component (i) (wood glue compound) and a hardener component (ii).

[0164] Preparation of component (i)

[0165] Step 1: Prepare the polyvinyl alcohol solution:

[0166] A glass beaker was placed on a magnetic stirrer and 800 ml of cold deionized water was added to the beaker. 200 grams of polyvinyl alcohol (PVA) powder (Poval PVA-CST, commercially available from Kuraray) was slowly added to the gently stirred water and allowed to swell for 20 minutes. The PVA dissolved when heated to a maximum of 95°C. After maintaining the temperature for a further 45 minutes, the solution was cooled down to 50°C, 2 grams of sodium metabisulfite was added and dissolved. The solution was filtered. The 20 wt% PVA solution was cooled down to room temperature and maintained overnight.

[0167] Step 2: Preparation of the wood glue compound (component (i))

[0168] To obtain the component A, 350 g of XSBR latex, 4 g of dispersant Dispex AA4140 (commercially available from BASF SE (Germany)), 4 g of wetting agent Lumiten I-SC (commercially available from BASF SE (Germany)), 1.5 g of defoamer Foamaster 111 (commercially available from BASF SE (Germany)), 300 g of the PVA solution from step 1 and 250 g of 325 mesh calcium carbonate powder (ExCal 325, commercially available from RE Carrol l, Inc. (USA)) were mixed and adjusted to a solid content of 47.5 wt% with 90.5 g of water. The pH was about 8 to 9 and the Brookfield viscosity of spindle 7 was in the range of 15,000 to 30,000 centipoise at RVT 20 rpm.

[0169] Step 3: Mix components (i) and (ii)

[0170] The final wood glue formulation was obtained by homogenizing 85 wt % of component (i) with 15 wt % of a diphenylmethane diisocyanate polymer (Desmodur 44V20L, commercially available from Covestro (Germany)).

[0171] Determination of storage period

[0172] As explained above, wood glue of the present invention is a 2K system and begins to solidify when mixing these two wood glue components (i) and (ii). The solidification in this progress causes the wood glue viscosity to increase steadily over time. On a certain limit, this viscosity no longer allows the application of suitable wood glue. This critical viscosity threshold is defined as a value with 150,000 centipoise. Due to practical reasons (for example, not intending to stop the line), from the viewpoint of laminated wood manufacturing, particularly using the automated processing of a robot dispenser, a storage period of 60 minutes is a minimum requirement. Any value greater than 60 minutes is useful.

[0173] One minute after components (i) and (ii) have been mixed, the Brookfield viscosity of the wood glue is measured at RVT 20 rpm, spindle 7. The viscosity increases steadily over time. The viscosity increase is monitored in 5 minute intervals until a threshold of 150,000 centipoise is reached. The result is the period from the first measurement one minute after mixing until the first result greater than 150,000 centipoise is reached.

[0174] Determination of wood joint strength

[0175] This test is carried out according to European standard EN 205:2003. This European standard describes a test for the evaluation of the resistance of adhesives to hot and cold water. Bonds with thin bond lines are evaluated here. With the aid of wood glue, beech wood panels of dimensions according to EN 205:2003 are glued together, firmly pressed, conditioned for 7 days in a standard environment (23±2°C and 50±5% relative humidity) and finally cut to obtain test pieces suitable for the tensile shear test. 10 test pieces are prepared for each glue and the average value of the valid results is calculated. Before determining the bond strength with a tensile shear tester, the wood test pieces are subjected to resistance conditions according to European standard EN 204:2001 grade D4. The wood test pieces are subjected to 7 days in a standard environment (23±2°C and 50±5% relative humidity), followed by 6 hours in boiling water and then 2 hours in water at 20±2°C.

[0176] The test pieces were tested in a tensile testing machine (zwickiLine Z5.0 TS, commercially available from Zwick Roell (Germany)) capable of achieving a constant traverse rate of 50 mm / min.

[0177] According to European standard EN 204:2001, the minimum bond strength for D4 durability class is greater than 4N / mm 2 .

[0178] The results of the shelf life and wood joint strength of the wood glues containing XSBR latex in Examples 1 to 12 are shown in Tables 3 and 4.

[0179] Table 3: Examples 1-6

[0180] Example 1(CE) 2 3 4 5 6 Storage period [minutes] 35 70 80 100 120 105 <![CDATA[Wood joint strength [N / mm 2 > 4.8 5.8 6.0 6.2 6.8 6.5

[0181] Table 4: Examples 7-12

[0182] Example 7(CE) 8 9 10 11 12 Storage period [minutes] 85 105 110 110 100 115 <![CDATA[Wood joint strength [N / mm 2 > 3.7 5.6 6.2 6.4 5.5 6.4 .

Claims

1. A polymer latex for an adhesive composition, obtainable by free radical emulsion polymerization of a mixture of ethylenically unsaturated monomers, wherein the mixture comprises: (a) vinyl aromatic monomers; (b) a conjugated diene monomer; and (c) ethylenically unsaturated monomers having acid and / or hydroxyl functionality; wherein the weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) is in the range of 1.60 to 2.30, and wherein the polymer latex has a median particle size of at least 220 nanometers.

2. The polymer latex according to claim 1, wherein the sum of the vinyl aromatic monomer (a) and the conjugated diene monomer (b) is in the range of 85.0 to 99.0 wt %, preferably 90.0 to 98.0 wt %, based on the total weight of the monomers in the monomer mixture.

3. The polymer latex according to claim 1 or 2, wherein the mixture of ethylenically unsaturated monomers comprises: (a) 40 to 80 wt %, preferably 50 to 75 wt %, more preferably 55 to 70 wt % of a vinyl aromatic monomer, based on the total weight of the monomers in the monomer mixture; The vinyl aromatic monomer (a) is preferably selected from styrene, α-methylstyrene, vinyltoluene and combinations thereof, more preferably styrene.

4. The polymer latex according to any one of the preceding claims, wherein the mixture of ethylenically unsaturated monomers comprises: (b) 15 to 50 wt %, preferably 20 to 45 wt %, more preferably 25 to 40 wt % of a conjugated diene monomer, based on the total weight of the monomers in the monomer mixture; The conjugated diene monomer (b) is preferably selected from 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2,4-hexadiene, 1,3-octadiene, 2-methyl-1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 3,4-dimethyl-1,3-hexadiene, 2,3-diethyl-1,3-butadiene, 4,5-diethyl-1,3-octadiene, 3-butyl-1,3-octadiene, 3,7-dimethyl-1,3,6-octatriene, 2-methyl-6-methylene-1,7-octadiene, 7-methyl-3-methylene-1,6-octadiene, 1,3,7-octatriene, 2-ethyl-1,3-butadiene, 2-pentyl-1,3-butadiene, 3,7-dimethyl-1,3,7-octatriene, 3,7-dimethyl-1,3,6-octatriene, 3,7,11-trimethyl-1,3,6,10-dodecatetraene, 7,11-dimethyl-3-methylene-1,6,10-dodecatriene, 2,6-dimethyl-2,4,6-octatriene, 2-phenyl-1,3-butadiene, 2-methyl-3-isopropyl-1,3-butadiene, 1,3-cyclohexadiene, myrcene, ocimene, farnesene and combinations thereof, more preferably selected from 1,3-butadiene, isoprene and combinations thereof, even more preferably 1,3-butadiene.

5. The polymer latex according to any one of the preceding claims, wherein the mixture of ethylenically unsaturated monomers comprises: (c) 0.2 to 6.0 wt. %, preferably 0.3 to 5.0 wt. %, more preferably 0.5 to 4.0 wt. % of ethylenically unsaturated monomers having acid and / or hydroxy functionality, based on the total weight of the monomers in the monomer mixture; The ethylenically unsaturated monomer (c) having an acid functional group is preferably selected from ethylenically unsaturated carboxylic acid monomers, ethylenically unsaturated sulfonic acid monomers, and ethylenically unsaturated phosphorus-containing acid monomers; more preferably selected from (meth)acrylic acid, crotonic acid, fumaric acid, itaconic acid, maleic acid, maleic anhydride, vinyl acetic acid, vinyl lactic acid, vinyl sulfonic acid, styrene sulfonic acid, 2-carboxyethyl (meth)acrylate, vinyl sulfonate, phenyl vinyl ester, sodium 4-vinylbenzenesulfonate, 2-methyl-2-propylene-1-sulfonic acid, 2-propylene-1-sulfonic acid, 4-styrenesulfonic acid, 2-acrylamido-2-methyl-1-propanesulfonic acid, vinylphosphonic acid, dimethyl vinylphosphonate, diethyl vinylphosphonate, diethyl allylphosphonate, allylphosphonic acid, and combinations thereof; even more preferably selected from (meth)acrylic acid, itaconic acid, and combinations thereof; The ethylenically unsaturated monomer (c) having a hydroxyl functional group is preferably selected from allyl alcohol, vinyl alcohol, N-hydroxymethyl (meth) acrylamide, 1-penten-3-ol; hydroxyalkyl esters of ethylenically unsaturated acids, such as hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl (meth) acrylate, and hydroxyethyl caprolactone acrylate, and combinations thereof; more preferably selected from hydroxyalkyl esters of ethylenically unsaturated acids, such as hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl (meth) acrylate, and hydroxyethyl caprolactone acrylate; even more preferably selected from hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl methacrylate, and combinations thereof; and The ethylenically unsaturated monomers having acid and hydroxyl functions (c) are preferably selected from 3-allyloxy-2-hydroxy-1-propanesulfonic acid.

6. The polymer latex according to any one of the preceding claims, wherein the weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) is in the range of 1.70 to 2.10; and / or The polymer latex has a median particle size of at least 230 nanometers, preferably at least 250 nanometers.

7. The polymer latex according to any one of the preceding claims, wherein the mixture of ethylenically unsaturated monomers comprises 0.05 to 3.0 wt%, preferably 0.10 to 2.0 wt%, more preferably 0.15 to 1.5 wt% of a chain transfer agent, wherein the weight percentage is based on the total amount of monomers in the monomer mixture; wherein the chain transfer agent is preferably selected from n-dodecyl mercaptan, carbon tetrachloride, carbon tetrabromide, bromotrichloromethane, 4-methylbenzenethiol, isooctyl 3-mercaptopropionate, tert-nonyl mercaptan, 4,4′-thiobisbenzenethiol, tert-dodecyl mercaptan, α-methylstyrene dimer, thioglycolic acid, 2-ethylhexyl thioglycolate, butyl 3-mercaptopropionate, 1,8-dimercapto-3,6-dioxaoctane and combinations thereof; more preferably tert-dodecyl mercaptan.

8. The polymer latex according to any one of the preceding claims, wherein the mixture of ethylenically unsaturated monomers comprises (d) 0 to 20 weight percent of an ethylenically unsaturated monomer different from (a) to (c), based on the total weight of monomers in the monomer mixture; wherein the ethylenically unsaturated monomer different from (a) to (c) is preferably selected from: (d1) an ethylenically unsaturated nitrile compound, which is preferably selected from (meth)acrylonitrile, α-cyanoethylacrylonitrile, fumaronitrile, α-chloronitrile and combinations thereof; (d2) alkyl esters of ethylenically unsaturated acids, which are preferably selected from methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and combinations thereof; (d3) ethylenically unsaturated compounds having a primary or secondary amino group, which are preferably selected from (meth)acrylamide, 2-aminoethyl (meth)acrylate hydrochloride, 2-aminoethyl (meth)acrylamide hydrochloride, N-ethyl (meth)acrylamide, N-(3-aminopropyl) (meth)acrylamide hydrochloride, N-hydroxyethyl (meth)acrylamide, N-3-(dimethylamino)propyl (meth)acrylamide, [3-(methacryloylamino)propyl]trimethylammonium, N-[tris (hydroxymethyl)methyl] (meth)acrylamide, N-phenylacrylamide, alkyl acrylamide, methacrylamide poly (ethylene glycol) amine hydrochloride and combinations thereof; and combinations thereof.

9. A method for preparing a polymer latex for an adhesive, comprising: A mixture of ethylenically unsaturated monomers is polymerized by free radical emulsion polymerization, wherein the mixture comprises: (a) vinyl aromatic monomers; (b) a conjugated diene monomer; and (c) ethylenically unsaturated monomers having acid and / or hydroxyl functionality; wherein the weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) is in the range of 1.60 to 2.30; and Wherein the polymer latex has a median particle size of at least 220 nanometers.

10. The method according to claim 9, wherein the weight ratio of the vinyl aromatic monomer (a) to the conjugated diene monomer (b) is in the range of 1.70 to 2.10; and / or The sum of the vinyl aromatic monomer (a) and the conjugated diene monomer (b) is in the range of 85.0 to 99.0 wt %, preferably 90.0 to 98.0 wt %, based on the total weight of the monomers in the monomer mixture.

11. The method according to claim 9 or 10, wherein the mixture of ethylenically unsaturated monomers comprises at least one, more than one or all of the following: (a) 40 to 80 wt %, preferably 50 to 75 wt %, more preferably 55 to 70 wt % of a vinyl aromatic monomer; The vinyl aromatic monomer (a) is preferably selected from styrene, α-methylstyrene, vinyltoluene and combinations thereof, more preferably styrene; (b) 15 to 50 wt %, preferably 20 to 45 wt %, more preferably 25 to 40 wt % of a conjugated diene monomer; The conjugated diene monomer (b) is preferably selected from 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2,4-hexadiene, 1,3-octadiene, 2-methyl-1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 3,4-dimethyl-1,3-hexadiene, 2,3-diethyl-1,3-butadiene, 4,5-diethyl-1,3-octadiene, 3-butyl-1,3-octadiene, 3,7-dimethyl-1,3,6-octatriene, 2-methyl-6-methylene-1,7-octadiene, 7-methyl-3-methylene-1,6-octadiene, 1 , 3,7-octatriene, 2-ethyl-1,3-butadiene, 2-pentyl-1,3-butadiene, 3,7-dimethyl-1,3,7-octatriene, 3,7-dimethyl-1,3,6-octatriene, 3,7,11-trimethyl-1,3,6,10-dodecatetraene, 7,11-dimethyl-3-methylene-1,6,10-dodecatriene, 2,6-dimethyl-2,4,6-octatriene, 2-phenyl-1,3-butadiene, 2-methyl-3-isopropyl-1,3-butadiene, 1,3-cyclohexadiene, myrcene, ocimene, farnesene and combinations thereof; more preferably selected from 1,3-butadiene, isoprene and combinations thereof; even more preferably 1,3-butadiene; and (c) 0.5 to 5.0% by weight, preferably 1.0 to 4.0% by weight, more preferably 1.0 to 3.0% by weight of ethylenically unsaturated monomers having acid and / or hydroxyl functionality; The ethylenically unsaturated monomer (c) having an acid functional group is preferably selected from ethylenically unsaturated carboxylic acid monomers, ethylenically unsaturated sulfonic acid monomers, and ethylenically unsaturated phosphorus-containing acid monomers; more preferably selected from (meth)acrylic acid, crotonic acid, fumaric acid, itaconic acid, maleic acid, maleic anhydride, vinyl acetic acid, vinyl lactic acid, vinyl sulfonic acid, styrene sulfonic acid, 2-carboxyethyl (meth)acrylate, vinyl sulfonate, phenyl vinyl ester, sodium 4-vinylbenzenesulfonate, 2-methyl-2-propylene-1-sulfonic acid, 2-propylene-1-sulfonic acid, 4-styrenesulfonic acid, 2-acrylamido-2-methyl-1-propanesulfonic acid, vinylphosphonic acid, dimethyl vinylphosphonate, diethyl vinylphosphonate, diethyl allylphosphonate, allylphosphonic acid, and combinations thereof; even more preferably selected from (meth)acrylic acid, itaconic acid, and combinations thereof; The ethylenically unsaturated monomer (c) having a hydroxyl functional group is preferably selected from allyl alcohol, vinyl alcohol, N-hydroxymethyl (meth) acrylamide, 1-penten-3-ol; hydroxyalkyl esters of ethylenically unsaturated acids, such as hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl (meth) acrylate and hydroxyethyl caprolactone acrylate, and combinations thereof; more preferably selected from hydroxyalkyl esters of ethylenically unsaturated acids, such as hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl (meth) acrylate and hydroxyethyl caprolactone acrylate; even more preferably selected from hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl methacrylate and combinations thereof; and The ethylenically unsaturated monomer (c) having acid and hydroxyl functional groups is preferably selected from 3-allyloxy-2-hydroxy-1-propanesulfonic acid; The weight percentages are based on the total weight of the monomers in the monomer mixture.

12. The method according to any one of claims 9 to 11, wherein the mixture of ethylenically unsaturated monomers comprises 0.05 to 3.0 wt. %, preferably 0.10 to 2.0 wt. %, more preferably 0.15 to 1.5 wt. % of a chain transfer agent, wherein the weight percentage is based on the total amount of monomers in the monomer mixture; wherein the chain transfer agent is preferably selected from n-dodecyl mercaptan, carbon tetrachloride, carbon tetrabromide, bromotrichloromethane, 4-methylbenzenethiol, isooctyl 3-mercaptopropionate, tert-nonyl mercaptan, 4,4′-thiobisbenzenethiol, tert-dodecyl mercaptan, α-methylstyrene dimer, thioglycolic acid, 2-ethylhexyl thioglycolate, butyl 3-mercaptopropionate, 1,8-dimercapto-3,6-dioxaoctane and combinations thereof; more preferably tert-dodecyl mercaptan.

13. The method according to any one of claims 9 to 12, wherein the polymer latex has a median particle size of at least 230 nanometers, preferably at least 250 nanometers.

14. Use of the polymer latex according to any one of claims 1 to 8 or the polymer latex prepared by the method according to any one of claims 9 to 13 for preparing an aqueous adhesive composition, preferably a two-component aqueous adhesive composition. 15 . An aqueous adhesive composition comprising (i) the polymer latex according to claim 1 or the polymer latex prepared by the method according to claim 9 , and (ii) a polyisocyanate compound.

16. The aqueous adhesive composition according to claim 15, wherein the (ii) polyisocyanate compound comprises toluene diisocyanate, hydrogenated toluene diisocyanate, methylene diphenyl diisocyanate, hydrogenated methylene diphenyl diisocyanate, triphenylmethane triisocyanate, 1,2,4-benzene triisocyanate, polymethylene polyphenyl polyisocyanate, xylene diisocyanate, tetramethylxylylene diisocyanate, 1,6-hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, isophorone diisocyanate, and 4,4′-methylene-bis(cyclohexyl isocyanate); and / or It further includes polyvinyl alcohol, vinyl alcohol-ethylene copolymers, polyvinyl alcohol modified by silanol, cellulose derivatives such as methyl cellulose, ethyl cellulose, hydroxy cellulose and carboxy cellulose; chitin, chitosan, starch, polyethylene glycol, polypropylene glycol, polyvinyl ether, gelatin, casein, cyclodextrin and combinations thereof, preferably polyvinyl alcohol.

17. The aqueous adhesive composition according to claim 15 or 16, which is a two-component adhesive composition, wherein the first component comprises the polymer latex and optionally polyvinyl alcohol, vinyl alcohol-ethylene copolymer, polyvinyl alcohol modified with silanol; cellulose derivatives such as methyl cellulose, ethyl cellulose, hydroxy cellulose and carboxy cellulose; chitin, chitosan, starch, polyethylene glycol, polypropylene glycol, polyvinyl ether, gelatin, casein, cyclodextrin and combinations thereof, preferably polyvinyl alcohol; and the second component comprises the polyisocyanate compound.

18. The aqueous adhesive composition according to any one of claims 15 to 17, comprising 1 to 50 wt%, preferably 2 to 45 wt%, more preferably 5 to 40 wt% of the polyisocyanate compound (ii), based on the total solid content of the aqueous adhesive composition.

19. An aqueous adhesive according to any one of claims 15 to 18 in the form of a wood glue.

20. A method for preparing an aqueous adhesive composition, comprising: Providing (i) a polymer latex according to any one of claims 1 to 8 or a polymer latex prepared by the method according to any one of claims 9 to 13; and mixing with (ii) a polyisocyanate compound, wherein the aqueous adhesive composition is preferably a wood glue.

Citation Information