Coating type cutting tool

By employing alternating (Ti, Si)N and (Ti, Al, Si)N nano-multilayer coatings on cutting tools, the problems of insufficient resistance to comb-like cracks and flank wear in metal machining are solved, thereby improving tool life and resistance to spalling when machining sticky materials.

CN119053728APending Publication Date: 2024-11-29SANDVIK COROMANT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380037118.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-01
Filing Date
2023-05-31
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing cutting tools have problems with insufficient resistance to comb-like cracks, flank wear, spalling resistance, and cutting edge toughness in metal processing, especially when milling and machining viscous materials.

Method used

By employing alternating (Ti, Si)N and (Ti, Al, Si)N nanolayer coatings, the coating's resistance to comb-like cracks and flank wear is improved, and its adhesion to the substrate is enhanced, through controlling the composition and structure of the nanolayers.

Benefits of technology

It significantly improves the cutting tool's resistance to comb-like cracks and flank wear, especially extending tool life in milling operations and reducing coating peeling when machining viscous materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053728A_ABST
    Figure CN119053728A_ABST
Patent Text Reader

Abstract

The present invention relates to a coated cutting tool (1) comprising a substrate (5) and a coating (6), where the coating (6) comprises a nanomultilayer (8) as alternating layers of a first nanolayer (9) and a second nanolayer (10), the first nanolayer (9) being Ti1-xAlxN, where 0.55 lt; the first nanolayer (9) is Ti < 1-y-z > Al < y > Si < z > N, x < = 0.70, and the second nanolayer (10) is Ti < 1-y-z > Al < y > Si < z > N with 0.20 < = y < = 0.50, 0.13 < = z < = 0.25, 0.46 < = y + z < = 0.65, the sequence of one first nanolayer (9) and one second nanolayer (10) forming a layer period, the average layer period thickness in the nanomultilayer (8) being < = 20 nm.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a coating type cutting tool comprising a nano multilayer of (Ti, Al)N and (Ti, Al, Si)N. Background Art

[0002] Typically, cutting tools for metal machining comprise a hard substrate material, such as cemented carbide with a thin hard, wear-resistant coating. The cutting tool typically has at least one rake face and at least one flank face. The cutting edge is located at the junction of the rake face and the flank face.

[0003] Nano-multilayer coatings are often used in the field of cutting tools for metal machining. In these coatings, at least two sub-layers that are different in some respects alternate to form a coating of a nano-layer stack. Various metal nitrides are often used in wear-resistant coatings for cutting tools.

[0004] Metal machining operations include, for example, turning, milling and drilling.

[0005] In order to provide long tool life, coated cutting tools such as inserts should have high resistance to different types of wear, such as flank wear resistance, crater wear resistance, chipping resistance and spalling resistance.

[0006] Different metal machining operations affect coated cutting tools in different ways. For example, turning is a continuous metal machining operation, while milling is more intermittent in nature. During milling, thermal and mechanical loads vary over time. Thermal tensions are induced in the coating, which can lead to so-called thermal cracks (referred to herein as "comb cracks"), which can cause fatigue of the cutting edge, resulting in chipping, where small pieces of the cutting edge are loosened from the rest of the substrate. As a result, common types of wear for coated cutting tools during milling are cracking and chipping. Therefore, improving the ability to resist comb cracks is critical to extending tool life.

[0007] A high level of toughness in the coating, especially at the cutting edge, ie high edge line toughness, also helps to reduce chipping.

[0008] Flank wear obviously occurs on the flank face of the cutting edge and is primarily derived from abrasive wear mechanisms. The flank face is subject to workpiece motion, and excessive flank wear can result in poor workpiece surface texture, inaccurate cutting, and increased friction during cutting. Providing better flank wear resistance provides longer tool life for specific metal machining operations.

[0009] During the machining operation, the coating must also maintain adhesion to the substrate, i.e. not flake off. Certain workpiece material types such as ISO-M (stainless steel) and ISO-S (heat-resistant super alloys, such as titanium) are so-called sticky materials and are more likely to cause flakes than other workpiece material types. These material types also have smearing behavior, which means that the workpiece material smears onto the cutting tool surface and can ultimately lead to the formation of built-up edge (BUE) of the workpiece material on the cutting edge. This BUE can cause the coating to flake off or even tear off part of the cutting tool edge.

[0010] In order to provide cutting tools with superior performance to those currently available on the market, there is a continuing need for coated cutting tools in which the coating has excellent properties in terms of flank wear resistance, comb crack resistance, spalling resistance, pit wear resistance, edge line toughness, etc. If one or more of the above properties is improved, longer tool life is provided.

[0011] An object of the present invention is to provide a coated cutting tool which exhibits a high resistance to flank wear at least during turning operations and a high resistance to comb cracks during milling operations.

[0012] Furthermore, another object of the present invention is to provide a coated cutting tool having high resistance to peeling when machining a coated material such as stainless steel.

[0013] definition

[0014] The term "average layer period thickness" refers to the average thickness of the combination AB in the nano-multilayer coating of the first nano-layer A and the second nano-layer B in the nano-multilayer ABABA. If the deposition process is known, it can be calculated by dividing the total thickness of the nano-multilayer by the number of times AB is deposited (which corresponds to the number of revolutions when the substrate is deposited in a rotating manner).

[0015] Alternatively, the calculation is performed by using TEM analysis on a cross section of the nanomultilayer to count the number of AB nanolayer combinations that are continuous over a length of at least 200 nm and calculate an average value.

[0016] If the total thickness of the nanomultilayer is only 0.5 µm, the measurement position is just below the outer surface of the nanomultilayer. Suitable analysis methods include transmission electron microscopy (TEM).

[0017] The term "FWHM" refers to "full width at half maximum", which is the width of an X-ray diffraction peak at half its peak intensity (for a particular (hkl) diffraction peak) and is measured in degrees (2θ). Summary of the invention

[0018] There is now provided a nanomultilayer coating of alternating (Ti, Si)N and (Ti, Al, Si)N layers, which has surprisingly high resistance to comb-shaped cracking and flank wear.

[0019] The present invention relates to a coated cutting tool comprising a substrate and a coating, wherein the coating comprises a nanomultilayer which is an alternating layer of a first nanolayer and a second nanolayer, the first nanolayer being Ti 1- x Al x N, where 0.55 < x ≤ 0.70, and the second nanolayer being Ti 1-y-z Al y Si z N, where 0.20 ≤ y ≤ 0.50, 0.13 ≤ z ≤ 0.25, 0.46 ≤ y + z ≤ 0.65, and the sequence of one first nanolayer and one second nanolayer forms a layer period, and the average layer period thickness in the nanomultilayer is ≤ 20 nm.

[0020] For the first nanolayer Ti 1-x Al x N, suitably 0.56 ≤ x ≤ 0.65, preferably 0.58 ≤ x ≤ 0.63, and most preferably 0.58 ≤ x ≤ 0.61.

[0021] For the second nanolayer Ti 1-y-z Al y Si z N, suitably 0.25 ≤ y ≤ 0.45 and 0.13 ≤ z ≤ 0.20, preferably 0.28 ≤ y ≤ 0.40 and 0.14 ≤ z ≤ 0.18, and most preferably 0.33 ≤ y ≤ 0.40 and 0.14 ≤ z ≤ 0.17.

[0022] For the second nanolayer Ti 1-y-z Al y Si z N, suitably 0.46 ≤ y + z ≤ 0.60, preferably 0.47 ≤ y + z ≤ 0.55.

[0023] The average layer period thickness of the nanomultilayer is suitably 2 to 15 nm, for example 3 to 10 nm or 3 to 7 nm.

[0024] In one embodiment, the nanomultilayer has a columnar microstructure. This means that there are columnar microcrystals or "grains" in the nanomultilayer, which are usually elongated in their growth direction.

[0025] In one embodiment, the nano-multilayer has 200 crystallographic preferred orientations. In this embodiment, the intensity ratio I(200) / I(111) in θ-2θ X-ray diffraction analysis is suitably >5, such as >10 or >20.

[0026] In one embodiment, the FWHM value of the cubic (200) peak of the nano-multilayer in X-ray diffraction is 0.4 to 1° (2θ), such as 0.5 to 0.9° (2θ) or 0.6 to 0.8° (2θ).

[0027] The (200) peak in XRD for determining the FWHM value is the exfoliated Cu-K α2 。

[0028] The thickness of the nano-multilayer is suitably about 0.5 to about 15 μm, preferably about 1 to about 10 μm, more preferably about 1 to about 7 μm, and most preferably about 1.5 to about 4 μm.

[0029] The nano-multilayer is suitably a cathodic arc evaporation deposition layer.

[0030] In one embodiment, the coating comprises a TiN, (Ti, Al)N or (Cr, Al)N layer under the nano-multilayer film, which is suitably closest to the substrate.

[0031] Preferably, the innermost layer is (Ti, Al)N. If (Ti, Al)N is used, then (Ti, Al)N is suitably Ti 1-v Al v N, where 0.35 ≤ v ≤ 0.70, preferably 0.45 ≤ v ≤ 0.65, and most preferably 0.55 < v ≤ 0.65. In a preferred embodiment, the Ti-Al relationship in (Ti, Al)N is the same as the Ti-Al relationship in the first nano-layer of the nano-multilayer, i.e., in Ti 1-v Al v N, it is suitably 0.55 ≤ v ≤ 0.70, such as 0.56 ≤ v ≤ 0.65 or 0.58 < v ≤ 0.63 or 0.58 < v ≤ 0.61. The thickness of this innermost layer can be about 0.1 to about 3 μm, about 0.2 to about 2 μm, and most preferably about 0.5 to about 1.5 μm.

[0032] In a preferred embodiment, the coating comprises a nano-multilayer as an alternating layer of a first nano-layer and a second nano-layer, the first nano-layer being Ti 1-x Al x N, where 0.55 < x ≤ 0.65, and the second nano-layer being Ti 1-y-z Al y Si zN, where 0.25 ≤ y ≤ 0.45 and 0.13 ≤ z ≤ 0.20, 0.46 ≤ y + z ≤ 0.65, the average layer period thickness of the nano-multilayer is 3 to 10 nm, the thickness of the nano-multilayer is about 1 to about 7 μm, and there is an innermost layer (Ti, Al)N closest to the substrate below the nano-multilayer, and its thickness is about 0.5 to about 1.5 μm.

[0033] In a more preferred embodiment, the coating comprises a nano-multilayer that is an alternating layer of a first nano-layer and a second nano-layer, and the first nano-layer is Ti 1-x Al x N, where 0.55 < x ≤ 0.63, and the second nano-layer is Ti 1-y- z Al y Si z N, where 0.28 ≤ y ≤ 0.40 and 0.13 ≤ z ≤ 0.17, 0.47 ≤ y + z ≤ 0.55, the average layer period thickness of the nano-multilayer is 3 to 10 nm, the thickness of the nano-multilayer is about 1 to about 7 μm, and there is an innermost layer (Ti, Al)N closest to the substrate below the nano-multilayer, and its thickness is about 0.5 to about 1.5 μm.

[0034] The substrate of the coated cutting tool can be selected from cemented carbide, cermet, ceramic, cubic boron nitride, and high-speed steel. In one embodiment, the substrate is cemented carbide, and the cemented carbide contains 5 to 18% by weight of Co and 0 to 10% by weight of carbides, nitrides, or carbonitrides of Groups 4 to 5 in the Periodic Table.

[0035] Other components such as Cr may be present in the cemented carbide substrate.

[0036] The coated cutting tool is suitably a cutting tool blade, drill bit, or solid end-mill for metal machining. For example, the cutting tool blade is a turning blade or a milling blade. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 A schematic diagram showing an embodiment where the cutting tool is a milling blade is shown.

[0038] Figure 2 A schematic diagram showing an embodiment where the cutting tool is a turning blade is shown.

[0039] Figure 3 A schematic cross-sectional view showing an embodiment of the coated cutting tool of the present invention is shown, and the schematic diagram shows the substrate and the coating including different layers. DETAILED DESCRIPTION

[0040] Figure 1A schematic diagram of an embodiment of a cutting tool (1) is shown having a rake face (2) and a flank face (3) and a cutting edge (4). The cutting tool (1) is a milling insert in this embodiment.

[0041] Figure 2 A schematic diagram of an embodiment of a cutting tool (1) is shown having a rake face (2) and a flank face (3) and a cutting edge (4). The cutting tool (1) is a turning insert in this embodiment.

[0042] Figure 3 A schematic diagram of a cross section of an embodiment of a coated cutting tool of the present invention having a substrate body (5) and a coating (6). The coating is composed of a first (Ti, Al) N innermost layer (7) and a nano-multilayer (8) of alternating nano-layers of Ti, Al, and Al. 1-x Al x N (9) and nano-layer Ti 1-y-z Al y Si z N (10).

[0043] Example

[0044] Embodiment 1:

[0045] Different nano-multilayers of (Ti, Al) N and (Ti, Al, Si) N were deposited on sintered carbide cutting tool insert blanks of geometry SNMA120408, CNMG120408MM and R390-11. The composition of the cemented carbide is 10 wt % Co, 0.4 wt % Cr and the remaining WC. The cemented carbide blanks were coated by cathodic arc evaporation in a vacuum chamber comprising four arc flanges. The Ti-Al-Si target was mounted on two flanges opposite to each other. The Ti-Al target was mounted on the remaining two flanges opposite to each other. The target was a circular plane with a diameter of 100 mm available on the open market. Target technology packages suitable for arc evaporation can be obtained from suppliers on the market such as IHI Hauzer Techno Coating BV, Kobelco (Kobe Steel Ltd.) and Oerlikon Balzers.

[0046] The uncoated blanks were mounted on pins that were triple rotated in the PVD chamber.

[0047] Samples 1-4:

[0048] Evacuate the chamber to a high vacuum (less than 10 -2 Pa) and heated to 450-550° C. by a heater located inside the chamber. The blank was then etched in Ar plasma for 60 minutes.

[0049] First, a Ti layer with a thickness of about 1 µm was deposited using only a Ti-Al target. 0.40 Al 0.60 N innermost layer, the Ti-Al target is Ti 0.40 Al 0.60 The process conditions for depositing the innermost (Ti,Al)N layer were as follows: the chamber pressure (reaction pressure) was 4 Pa ​​N2 gas, and the DC bias voltage applied to the blank assembly was -70 V (relative to the chamber wall). The cathodes were operated in arc discharge mode at a current of 150 A (each).

[0050] Then, Ti-Al target and Ti-Al-Si target were used. The chamber pressure (reaction pressure) was set to 4 Pa ​​of N2 gas, and a DC bias voltage of -70 V (relative to the chamber wall) was applied to the blank assembly. The cathode was operated in arc discharge mode at 150 A current (each) for 75 minutes (4 flanges). A nano-multilayer coating with a thickness of about 3 µm was deposited on the blank.

[0051] Deposition was performed using a combination of a Ti-Al-Si target and a Ti-Al target, wherein the Ti-Al-Si target is Ti 0.50 Al 0.35 Si 0.15 、Ti 0.50 Al 0.30 Si 0.20 、Ti 0.35 Al 0.55 Si 0.10 and Ti 0.30 Al 0.60 Si 0.10 , and the Ti-Al target is Ti 0.40 Al 0.60 The total thickness of the deposited nano-multilayer was about 3 μm (as measured on the flank surface). The rotation speed is related to the specific period thickness. In the specific equipment used, the rotation speed of 5 rpm used corresponds to a nano-layer period thickness of about 5 nm.

[0052] The prepared samples are respectively referred to as “Sample 1 (Invention)”, “Sample 2 (Invention)”, “Sample 3 (Comparative)”, and “Sample 4 (Comparative)”.

[0053] Sample 5:

[0054] As a further comparison, a nano-multilayer coating comprising (Ti, Al)N and (Ti, Si)N was deposited on sintered cemented carbide cutting tool insert blanks of geometry SNMA120408, CNMG120408MM and R390-11. The composition of the cemented carbide was the same as that of samples 1 to 4. The cemented carbide blanks were coated by cathodic arc evaporation in a vacuum chamber comprising four arc flanges. The Ti-Si target was mounted on two flanges facing each other. The Ti-Al target was mounted on the remaining two flanges facing each other. The target was a circular flat surface with a diameter of 100 mm available on the open market. Target technology packages suitable for arc evaporation are available from suppliers on the market such as IHI Hauzer Techno Coating BV, Kobelco (KobeSteel Ltd.) and Oerlikon Balzers.

[0055] The uncoated blanks were mounted on pins that were triple rotated in the PVD chamber.

[0056] Evacuate the chamber to a high vacuum (less than 10 -2 Pa) and heated to 450-550° C. by a heater located inside the chamber. The blank was then etched in Ar plasma for 60 minutes.

[0057] First, a Ti layer with a thickness of about 1 µm was deposited using only a Ti-Al target. 0.40 Al 0.60 N innermost layer, the Ti-Al target is Ti 0.40 Al 0.60 The process conditions for depositing the innermost (Ti,Al)N layer were as follows: the chamber pressure (reaction pressure) was 4 Pa ​​N2 gas, and the DC bias voltage applied to the blank assembly was -70 V (relative to the chamber wall). The cathodes were operated in arc discharge mode at a current of 150 A (each).

[0058] Then, Ti-Al target and Ti-Al-Si target were used. The chamber pressure (reaction pressure) was set to 4 Pa ​​of N2 gas, and a DC bias voltage of -70 V (relative to the chamber wall) was applied to the blank assembly. The cathode was operated in arc discharge mode at 150 A current (each) for 75 minutes (4 flanges). A nano-multilayer coating with a thickness of about 3 µm was deposited on the blank.

[0059] The rotation speed is related to the specific period thickness. In the specific device used, the rotation speed of 5 rpm used corresponds to a nanolayer period thickness of about 5 nm.

[0060] The prepared sample is referred to as "Sample 5 (comparative)".

[0061] The prepared samples 1 to 5 are listed in Table 1.

[0062]

[0063] The results of the measurement of the actual elemental composition in the (Ti, Al) N and (Ti, Al, Si) N coatings using energy dispersive X-ray spectroscopy (EDS) showed that deviations of only 1 to 2 percentage points were found compared to the theoretical composition based on the target composition. These small deviations are within the accuracy of the EDS method. It was therefore concluded that the actual elemental composition of Ti, Al and Si in the layers deposited here corresponds essentially well to the corresponding target composition used.

[0064] Example 2 (Analysis):

[0065] The SEM images of samples 1 to 5 show that the nano-multilayer films have a columnar structure.

[0066] In addition, X-ray diffraction (XRD) analysis of the flank face of the coated inserts was performed using a PANalytical CubiX3 diffractometer equipped with a PIXcel detector. The coated cutting tool inserts were mounted in a sample holder to ensure that the flank face of the sample was parallel to the reference surface of the sample holder and also to ensure that the flank face was at an appropriate height. α Radiation was used for the measurement with a voltage of 45 kV and a current of 40 mA. An anti-scatter slit of 1 / 2° and a divergence slit of 1 / 4° were used. The diffraction intensity from the coated cutting tool was measured near the 2θ angle where the relevant peak appeared.

[0067] Data analysis, including background subtraction and Cu-K α2 Peeling. The peak analysis adopts the Pseudo-Voigt-Fit function. No film correction is applied to the peak intensity obtained. When determining the peak intensity and peak width, the software (deconvolution of the combined peak) compensates for the possible peak overlap of the (111) or (200) peak with any diffraction peak that does not belong to the PVD layer, such as the reflection of the substrate such as WC. The XRD of the nano multilayer of the present invention shows a 200 crystallographic preferred orientation. There is no obvious (111) peak at all, so the intensity ratio I (200) / I (111) is much higher than 20. The half-maximum full width (FWHM) value of the sample (200) peak was calculated. The results are shown in Table 2.

[0068]

[0069] The FWHM value reflects both the grain size of the crystallites in the coating and the point defect density, since the smaller the grain size and / or the greater the point defect density, the greater the FWHM value. In this case, the coating of the present invention exhibits a rather small FWHM value.

[0070] Embodiment 3:

[0071] Cutting tests were conducted to determine the properties of the prepared samples.

[0072] Explanation of terms used:

[0073] The following expressions / terms are commonly used in metal cutting, but are explained in the table below:

[0074] Vc (m / min): cutting speed, in meters per minute

[0075] fz (mm / tooth): feed rate in millimeters / tooth (milling)

[0076] fn (mm / rev): Feed rate per revolution (turning)

[0077] z (number): number of milling cutter teeth

[0078] a e (mm): Radial cutting depth, in millimeters

[0079] a p (mm): Axial cutting depth, in millimeters

[0080] Comb crack resistance:

[0081] Operation: Shoulder milling

[0082] Tool holder: R245-080027-12M, Dc=80 mm

[0083] Workpiece material: Toolox 33 (tool steel), L=600 mm, I=200 mm, h=100 mm,

[0084] Blade type: R390-11

[0085] Cutting speed V c =320 m / min

[0086] Feed speed f z =0.3 mm / rev

[0087] z=1

[0088] Cutting depth a p =2 mm

[0089] Radial toothinge =15 mm

[0090] Using cutting fluid

[0091] The criterion for tool life termination is maximum chipping height VB>0.3 mm.

[0092] Flank wear test:

[0093] Longitudinal turning

[0094] Workpiece material: Sverker 21 (tool steel), hardness ~210HB, D=180, L=700 mm,

[0095] V c =125 m / min

[0096] f n =0.072 mm / rev

[0097] a p =2 mm

[0098] No cutting fluid

[0099] The cut-off criterion for tool life is that the flank wear VB is 0.15 mm.

[0100] Anti-peeling:

[0101] The evaluation was carried out by turning tests on austenitic steel. In order to induce adhesive wear and coating peeling, the cutting depth a p Varies between 4 to 0 and 0 to 4 mm (in one run during radial facing). The inserts were evaluated by SEM analysis.

[0102] Operation: facing (turning)

[0103] Workpiece material: Austenitic stainless steel Sanmac 316L bar, L=200 mm, D=100 mm, ~215 HB

[0104] Blade type: CNMG 120408-MM

[0105] Cooling: Yes

[0106] Cutting depth a p =4 to 0, 0 to 4 mm

[0107] Cutting speed V c =140 m / min

[0108] Feed rate f z =0.36 mm / rev

[0109] Edge toughness:

[0110] Workpiece material: Unhardened Dievar, P3.0.Z.AN,

[0111] z=1

[0112] V c =200 m / min

[0113] F z =0.20 mm

[0114] a e =12 mm

[0115] a p =3.0

[0116] Cutting length = 12 mm

[0117] No cutting fluid

[0118] The cut-off criteria are a minimum chipping of 0.5 mm at the edge line or a depth of 0.2 mm measured at the flank or rake face. Tool life is expressed as the number of cuts that achieve these criteria.

[0119] The results of the cutting tests are shown in Tables 3 to 5.

[0120]

[0121] *: Sample of the present invention

[0122] **:Compare

[0123] In terms of comb crack resistance, all samples 1 to 4 performed well, but sample 1 performed best, and the performance decreased in the order of sample 1 > sample 2 > sample 3 > sample 4. Regarding flank wear resistance, samples 1 and 2 performed well, while samples 3 and 4 performed much worse.

[0124]

[0125] *: Sample of the present invention

[0126] **:Compare

[0127] In terms of spalling resistance, Samples 1 and 2 performed well, although Sample 2 showed differences in the 100 m / min and 140 m / min spalling test runs. In this spalling test for stainless steel machining, 100 m / min is the most severe test because it produces more smearing than when 140 m / min is used. Samples 3 and 4, which contain nano-multilayers of (Ti, Al)N and (Ti, Al, Si)N with a higher content of Al in the (Ti, Al, Si)N nanolayers, performed much worse in both the 100 m / min and 140 m / min spalling resistance tests.

[0128]

[0129] *: Sample of the present invention

[0130] With regard to edge line toughness, the samples according to the invention performed very well.

Claims

1. A coated cutting tool (1), said coated cutting tool (1) comprising a substrate (5) and a coating (6), wherein said coating (6) comprises a nanomultilayer (8) which is an alternating layer of a first nanolayer (9) and a second nanolayer (10), said first nanolayer (9) being Ti 1-x Al x N, where 0.55 < x ≤ 0.70, and said second nanolayer (10) being Ti 1-y-z Al y Si z N, where 0.20 ≤ y ≤ 0.50, 0.13 ≤ z ≤ 0.25, 0.46 ≤ y + z ≤ 0.65, A sequence of one first nanolayer (9) and one second nanolayer (10) forms a layer period, the average layer period thickness in said nanomultilayer (8) ≤ 20 nm.

2. The coated cutting tool (1) according to claim 1, wherein for said first nanolayer (9) Ti 1-x Al x N, 0.56 ≤ x ≤ 0.

63.

3. The coated cutting tool (1) according to any one of claims 1 to 2, wherein for said second nanolayer (10) Ti 1-y-z Al y Si z N, 0.25 ≤ y ≤ 0.45, 0.13 ≤ z ≤ 0.

20.

4. The coated cutting tool (1) according to any one of claims 1 to 3, wherein for said second nanolayer (10) Ti 1-y-z Al y Si z N, 0.46 ≤ y + z ≤ 0.

60.

5. The coated cutting tool (1) according to any one of claims 1 to 3, wherein for said second nanolayer (10) Ti 1-y-z Al y Si z N, 0.33 ≤ y ≤ 0.40, 0.14 ≤ z ≤ 0.

17.

6. The coated cutting tool (1) according to any one of claims 1 to 5, wherein for said second nanolayer (10) Ti 1-y-z Al y Si z N, 0.47 ≤ y + z ≤ 0.

55.

7. The coated cutting tool (1) according to any one of claims 1 to 6, wherein an average layer period thickness in the nano-multilayer (8) is 2 nm to 15 nm.

8. The coated cutting tool (1) according to any one of claims 1 to 7, wherein the nano-multilayer (8) has a columnar microstructure.

9. The coated cutting tool (1) according to any one of claims 1 to 8, wherein the FWHM value of the cubic (200) peak in X-ray diffraction is 0.4° to 1° (2θ).

10. The coated cutting tool (1) according to any one of claims 1 to 9, wherein the thickness of the nano-multilayer (8) is about 0.5 μm to about 15 μm.

11. The coated cutting tool (1) according to any one of claims 1 to 10, wherein the coating (6) comprises an innermost layer (7) of TiN, (Ti, Al)N or (Cr, Al)N located closest to the substrate below the nano-multilayer (8), and the thickness of the innermost layer (7) is about 0.1 μm to about 3 μm.

12. The coated cutting tool (1) according to claim 11, wherein the innermost layer (7) is Ti 1-v Al v N, 0.35≤v≤0.

70.

13. The coated cutting tool (1) according to any one of claims 1 to 12, wherein the nano-multilayer (8) is a cathode arc evaporation deposition layer.

14. The coated cutting tool (1) according to any one of claims 1 to 13, wherein the substrate (5) of the coated cutting tool (1) is selected from cemented carbide, cermet, ceramic, cubic boron nitride and high speed steel.

15. The coated cutting tool (1) according to any one of claims 1 to 14, wherein the coated cutting tool (1) is a cutting tool insert, a drill or an integral end mill for metal machining.