Carbon coated nanowire network electrode

By preparing a nanowire network coated with a carbon-based coating in the electrode, using gas phase technology and carbon pyrolysis deposition steps, the problem of capacity and cyclic characteristics of the electrode under fast charging/discharge is solved, achieving high capacity and stability .

CN119054093APending Publication Date: 2024-11-29FUNDACION IMDEA MATERIALES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380022273.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-18
Filing Date
2023-02-17
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing electrodes have low capacity and poor cycle characteristics at fast charging/discharge rates, and the capacity retention rate is poor under repeated charging/discharge cycles, making it difficult to have good mechanical and electrochemical properties at the same time.

Method used

Nanowire network electrodes coated with carbon-based coatings are prepared by vapor phase technology, and a self-supported nanowire network is formed using aerosol and vapor phase deposition methods, and the conductivity and structural stability of the electrodes are improved by carbon pyrolysis deposition steps.

Benefits of technology

Capacity performance close to the theoretical value at low magnifications, and high specific capacity and cyclic characteristics are maintained at high magnifications, improving the mechanical flexibility and electrochemical performance of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004996577510000011
    Figure HDA0004996577510000011
  • Figure HDA0004996577510000021
    Figure HDA0004996577510000021
  • Figure HDA0004996577510000031
    Figure HDA0004996577510000031
Patent Text Reader

Abstract

The invention relates to a method for preparing an electrode. To an electrode obtained by said method; to a battery comprising the electrode; and to the use of said electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the preparation of electrodes. More specifically, the present invention relates to a method for preparing an electrode for a battery, and an electrode obtained by the method. Background Art

[0002] Electrochemical energy generation and storage are promising technologies for powering the electric vehicles and devices of our modern society. The development of novel electrodes is considered necessary to increase the energy density of batteries relative to conventional lithium-ion batteries.

[0003] Nanowire networks present advantages over materials made from larger building blocks. In general, nanowires are mechanically flexible due to their nanoscale size and have a reduced amount of defects compared to bulk materials. Nanowire networks also exhibit various properties due to their small size and one-dimensional morphology. Therefore, some properties of nanowire networks depend on the characteristics of the nanowires.

[0004] Document WO2021094485 discloses an electrode comprising a nanowire network and an optional electrical connection or current collector. According to the document, the mechanical properties imparted by the nanowire network eliminate the use of reinforcing additives (such as polymer binders) in the electrode, and provide a method for processing or integrating such electrodes without the need for solvents or other dispersion forms traditionally adopted. However, these types of electrodes have low conductivity values, and thus, as electrodes in batteries, they have low capacity, especially at fast charge / discharge rates, and poor capacity retention (commonly referred to as cycle characteristics) under repeated charge / discharge cycles.

[0005] Despite various proposals in the prior art, there is still a need to develop methods for synthesizing new electrodes that overcome the limitations of the prior art and new electrodes with good mechanical and electrochemical properties, such as capacity and cycling characteristics. Summary of the invention

[0006] The inventors of the present invention have discovered a method for manufacturing an electrode comprising a nanowire network coated with a carbon-based coating. The method for manufacturing the electrode manufactures a nanowire network that is self-supporting and has good mechanical properties, such as good flexibility when bent, and wherein the nanowires have a high aspect ratio. In addition, the method is capable of coating the nanowire network with a uniform carbon-based coating, capable of providing high conductivity values ​​resulting in high capacity and cycle characteristics. In addition, the method of the present invention is based on aerosol and gas phase technology and has the potential to be scaled up to produce a large number of products while maintaining a high level of control over the process. In addition, the carbon-based coating of the electrode of the present invention contains crystalline graphite domains that improve the electrochemical properties of the electrode, in particular its conductivity. In addition, the inventors have observed that the interface between the nanowires of the network and the carbon coating contains a majority of aligned crystalline graphite domains. This feature is a result of the carbon pyrolysis deposition step of the electrode synthesis method and improves the final performance of the electrode.

[0007] In addition, when tested in a battery, the electrode of the present invention comprising a nanowire network coated with a carbon-based coating exhibits a capacity value close to the theoretical value at low rates and even at high surface density. In addition, the electrode exhibits high specific capacity, high structural stability, and high capacity retention and cycle characteristics.

[0008] Thus, in a first aspect, the present invention relates to a method for preparing an electrode, comprising:

[0009] (a) preparing a nanowire network by a method comprising the following steps:

[0010] i. providing a first gas flow to the reaction vessel;

[0011] wherein the first gas stream comprises at least one precursor compound, the precursor compound comprising at least one element selected from Si, Ge, Al, Cu, Zn, Sb, Ni, Ti, Se, Ta, Pt, Mo, V, W, Co, Mn and Li; wherein at least one precursor compound is a metal hydride or an organometallic compound; and

[0012] ii. providing a second gas stream to the reaction vessel, the second gas stream comprising metal catalyst particles; allowing the first and second gas streams to mix in the reaction vessel to form a gas stream mixture; wherein the metal catalyst particles comprise one or more elements selected from Au, Ag, Cu, Fe, Ni, Ga, Co, Pt, In and Al;

[0013] wherein the at least one precursor compound is present in the gas stream mixture at a mole fraction (xi) of at least 0.010;

[0014] Wherein, the temperature inside the reaction container is 200°C to 3000°C;

[0015] wherein the at least one precursor compound decomposes at a temperature inside the reaction vessel and grows on the metal catalyst particles by vapor-liquid-solid (VLS) and / or chemical vapor deposition (CVD) to form a nanowire network; and

[0016] (b) coating the nanowire network obtained from step (a) by pyrolyzing a carbon precursor at a temperature of 500° C. to 1300° C. under an inert gas atmosphere to obtain a nanowire network coated with a carbon coating; and

[0017] (c) Optionally, contacting the carbon-coated nanowire network with an electrical connection or current collector.

[0018] In a second aspect, the present invention relates to an electrode obtainable by any specific embodiment of the method of the present invention, comprising:

[0019] - A nanowire network coated with a carbon coating;

[0020] wherein the aspect ratio of the nanowires of the nanowire network is at least 130;

[0021] wherein the carbon coating comprises graphite carbon;

[0022] wherein the amount of the carbon coating is greater than 3 weight % of the total weight of the nanowire network coated with the carbon coating; and

[0023] - Optional electrical connections and / or current collectors.

[0024] In another aspect, the invention relates to a battery comprising:

[0025] - electrodes, wherein at least one electrode is as described in any embodiment of the present invention;

[0026] - electrolytes; and

[0027] - Device for connection to a power / load source.

[0028] A further aspect of the present invention relates to the use of an electrode according to any specific embodiment of the present invention in a battery, preferably a lithium battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Images of a free-standing Si nanowire network before (a) and after (b) carbon coating are shown.

[0030] Figure 2 Shown is an electron micrograph of a Si nanowire network before carbon coating.

[0031] Figure 3HRTEM micrograph showing the interface between the carbon coating and the crystalline Si of the Si nanowire network after carbon coating.

[0032] Figure 4 Representative Raman spectra are shown, which illustrate the crystallinity of the Si nanowires and the graphitization of the coating on the C-coated Si nanowire network.

[0033] Figure 5 Shown is the XRD pattern of the Si nanowire network after carbon coating.

[0034] Figure 6 (a) The first 10 cyclic voltammograms at a scan rate of 0.025 mV / s and (b) the rate performance (specific capacity vs. number of cycles) at C rates from C / 20 to 2C obtained using Si nanowire networks coated with carbon coatings (with two different C contents: 27 wt% and 5 wt%, respectively) as electrodes in half-cells are shown. The results for the Si nanowire network coated with 27 wt% carbon coating are shown as black circles, and the results for the Si nanowire network coated with 5 wt% carbon coating are shown as triangles. Electrode mass loading: 1.2 mg / cm 2 And 1C = 3.6A / g.

[0035] Figure 7 Shown are (i) specific capacity vs cycle number and (ii) coulombic efficiency (1C = 3.6 A / g) of a carbon-coated Si nanowire network as an electrode at (a) a C-rate of C / 10 for 100 cycles and (b) a C-rate of C / 2 for 500 cycles.

[0036] Figure 8 Rate performance (specific capacity vs. cycle number) at C rates from C / 20 to 2C using a carbon-coated Si nanowire network (black circles) and results for a Si nanowire network with interspersed carbon nanotubes (shown as squares). Electrode mass loading: 1.2 mg / cm 2 And 1C = 3.6A / g. DETAILED DESCRIPTION

[0037] The present invention relates to a method for preparing an electrode; to an electrode obtainable by the method; to a battery cell comprising the electrode; and to the use of the electrode.

[0038] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present disclosure belongs.As used herein, the singular forms "a", "an", and "the" include plural references unless the context clearly dictates otherwise.

[0039] In a first aspect, the present invention relates to a method for preparing an electrode, comprising:

[0040] (a) preparing a nanowire network by a method comprising the following steps:

[0041] i. providing a first gas flow to the reaction vessel;

[0042] wherein the first gas stream comprises at least one precursor compound comprising at least one element selected from the group consisting of Si, Ge, Al, Cu, Zn, Sb, Ni, Ti, Se, Ta, Pt, Mo, V, W, Co, Mn, and Li; wherein the at least one precursor compound is a metal hydride or an organometallic compound; and

[0043] ii. providing a second gas stream to the reaction vessel, the second gas stream comprising metal catalyst particles; allowing the first and second gas streams to mix in the reaction vessel to form a gas stream mixture;

[0044] Wherein, the metal catalyst particles include one or more elements selected from Au, Ag, Cu, Fe, Ni, Ga, Co, Pt, In and Al;

[0045] wherein at least one precursor compound is present in the gas stream mixture at a mole fraction (xi) of at least 0.010;

[0046] Wherein, the temperature inside the reaction vessel is 200°C to 3000°C;

[0047] wherein at least one precursor compound decomposes at a temperature inside the reaction vessel and grows on the metal catalyst particles by vapor-liquid-solid (VLS) and / or chemical vapor deposition (CVD) to form a nanowire network; and

[0048] (b) coating the nanowire network obtained from step (a) by pyrolyzing a carbon precursor at a temperature of 500° C. to 1300° C. under an inert gas atmosphere to obtain a nanowire network coated with a carbon coating; and

[0049] (c) Optionally, contacting the carbon-coated nanowire network with an electrical connection or current collector.

[0050] Step (a)

[0051] The method of preparing a nanowire network may include a further step of converting the nanowire network into a fiber, yarn or fabric. The step of converting the nanowire network into a fiber, yarn or fabric is optionally performed simultaneously with step (ii) of the method.

[0052] Step (i)

[0053] The method for preparing a nanowire network of step (a) comprises the step (i) of providing a first gas flow to a reaction vessel; wherein the first gas flow comprises at least one precursor compound comprising at least one element selected from Si, Ge, Al, Cu, Zn, Sb, Ni, Ti, Se, Ta, Pt, Mo, V, W, Co, Mn and Li; and wherein at least one precursor compound is a metal hydride or an organometallic compound.

[0054] In one embodiment, the first gas stream further comprises a sheath gas selected from nitrogen, hydrogen, noble gases and mixtures thereof; preferably H2 or an inert gas, in particular N2.

[0055] In one embodiment, the first gas flow consists of at least one precursor compound and a sheath gas selected from nitrogen, hydrogen, noble gases and mixtures thereof; preferably H2 or an inert gas, in particular N2.

[0056] Precursor

[0057] Step (i) of the method of the present invention provides a first gas stream to the reaction vessel, wherein the first gas stream comprises at least one precursor compound.

[0058] In a particular embodiment, at least one precursor compound is a compound that participates in a reaction (i.e., a chemical reaction) to produce a nanowire network of the invention, for example, SiH4 is a precursor compound that can produce a Si nanowire network when used in the method of the invention.

[0059] In a particular embodiment, at least one precursor compound of the process of the invention comprises at least one element selected from Si, Ge, Al, Cu, Zn, Pt, Mo, V, W, Co, Mn and Li; in particular Si, Ge, Al, Cu, Zn, Pt and Co; more particularly Si and Ge; still more particularly Si.

[0060] In one embodiment, the metal element of the metal hydride or organometallic compound of at least one precursor compound is at least one element selected from Si, Ge, Al, Cu, Zn, Sb, Ni, Ti, Se, Ta, Pt, Mo, V, W, Co, Mn and Li; preferably selected from Si, Ge, Al, Cu, Zn, Pt, Mo, W, Co, Mn and Li; in particular Si, Ge, Al, Cu, Zn, Pt and Co; more particularly Si, Ge and Al; still more particularly Si and Ge; even more particularly Si. In a preferred embodiment, the metal element of the metal hydride or organometallic compound of at least one precursor compound is an element selected from Si, Ge, Al, Cu, Zn, Sb, Ni, Ti, Se, Ta, Pt, Mo, V, W, Co, Mn and Li; preferably selected from Si, Ge, Al, Cu, Zn, Pt, Mo, W, Co, Mn and Li; in particular Si, Ge, Al, Cu, Zn, Pt and Co; more particularly Si, Ge and Al; still more particularly Si and Ge.

[0061] Precursors of the present invention include, but are not limited to, compounds such as: compounds containing Si, such as (3-aminopropyl)triethoxysilane, N-sec-butyl(trimethylsilyl)amine, chloropentamethyldisilane, tetramethylsilane, silicon tetrabromide, silicon tetrachloride, tri(tert-butoxy)silanol or SiH4; compounds containing Ge, such as tetramethylgermanium, triethylgermanium hydride, triphenylgermanium hydride, triphenylgermanium hydride, tetramethylgermanium, tributylgermanium hydride, triethylgermanium hydride, triphenylgermanium hydride; compounds containing Se, such as dimethylselenium; compounds containing Al, such as trimethylaluminum (TMAl) or triethylaluminum (TEAl).

[0062] The at least one precursor compound may be in solid or liquid form (ie atomized in the first gas stream of the process of the invention), or in gaseous form. In a particular embodiment, the at least one precursor compound is in gaseous form.

[0063] In a more particular embodiment, at least one precursor compound is a metal hydride, in particular SiH4.

[0064] In a particular embodiment, the at least one precursor compound is a precursor compound.

[0065] In a particular embodiment, the first gas stream comprises more than one precursor compound. In particular, the first gas stream may comprise a first precursor compound and an additional precursor compound. In a particular embodiment, the additional precursor compound may be used as a dopant for the nanowire network (in an amount less than the primary precursor compound). Suitable dopants depend on the nanowire material being doped.

[0066] In a particular embodiment, at least one precursor compound of the present invention is provided to the reaction vessel of the present invention at a rate of at least 0.01 mol / h; preferably at a rate of at least 0.05 mol / h; more preferably at least 0.10 mol / h; and still more preferably at a rate of about 0.03 mol / h.

[0067] Step (ii)

[0068] The method for preparing a nanowire network of step (a) comprises the step (ii) of providing a second gas flow containing metal catalyst particles to a reaction vessel; and mixing the first gas flow and the second gas flow in the reaction vessel to form a gas flow mixture.

[0069] In one embodiment, the second gas stream further comprises a sheath gas selected from nitrogen, hydrogen, noble gases and mixtures thereof; preferably H2 or an inert gas, in particular N2.

[0070] In one embodiment, the second gas stream consists of metal catalyst particles and a sheath gas selected from nitrogen, hydrogen, noble gases and mixtures thereof; preferably H2 or an inert gas, especially N2.

[0071] In a particular embodiment, only one type of gas is used in the present invention. In particular, the terms "first" and "second" refer to the number of streams used.

[0072] In a particular embodiment, step (a) of the method for preparing a nanowire network comprises the further step of collecting the nanowire network; in particular by spinning and winding the nanowire network (as a yarn or fabric) on a bobbin.

[0073] catalyst

[0074] In a particular embodiment, the metal catalyst particles of the method of the present invention comprise one or more elements selected from Au, Ag, Cu, Fe, Ni, Ga, Co, Pt, In and Al; particularly one or more elements selected from Au, Ni, Ag and Cu; more particularly one or more elements selected from Au and Ag; still more particularly Au. The metal catalyst particles may consist of a single element, or a combination of two or more elements (e.g., an alloy). The metal catalyst particles may be in the second gas stream as solid particles or as liquid particles; preferably as solid particles.

[0075] In another specific embodiment, the metal catalyst particles of the method of the present invention further comprise one or more additional elements selected from Group 16 elements to control and / or enhance the growth of nanowires. The additional elements are particularly selected from oxygen, sulfur, selenium, tellurium and polonium; more particularly selected from S, Se, Te and O.

[0076] In a particular embodiment, the metal catalyst particles consist of an element selected from Au, Ag, Cu, Fe, Ni, Ga, Co, Pt, In and Al; particularly consist of an element selected from Au, Ag and Cu; more particularly consist of an element selected from Au and Ag; even more particularly consist of Au.

[0077] In a particular embodiment, the metal catalyst particles have an average diameter of 0.1 nm to 100 nm; preferably 1 nm to 30 nm. The average diameter of the metal catalyst particles of the present invention can be calculated by the average of the values ​​obtained by measuring the diameters of more than 100 metal catalyst particles using electron microscope micrographs, or by the size distribution obtained from different aerosol measurement techniques, such as obtained from a differential mobility particle sizer (DMA).

[0078] Furthermore, the metal catalyst particles may be provided without an electric charge, or the metal catalyst particles may be charged.

[0079] The metal catalyst particles may be provided to the reaction vessel in the form of an aerosol generated by an upstream aerosol generator. Alternatively, the metal catalyst particles may be formed in situ by providing a precursor compound; preferably a gaseous precursor compound. In a preferred embodiment, the metal catalyst particles are provided in the form of an aerosol.

[0080] In a particular embodiment, the metal catalyst particles are present in an amount of at least 1×10 -5 g / h; preferably at least 1×10 - 4 g / h; more preferably at least 2×10 -4 g / h; more preferably at least 2.7×10 -4 g / h enters the reaction vessel.

[0081] Gas Flow Mixture

[0082] In a particular embodiment, a gas stream mixture is generated when the first and second gas streams are contacted in the reaction vessel. A mixing device can be used to mix the streams to form a gas stream mixture. As needed, the pressure and flow rate can be adjusted to ensure proper mixing of the first and second streams to form a gas stream mixture.

[0083] In a particular embodiment, the gas stream mixture circulates in the reaction vessel at a rate of at least 60 l / h; preferably at least 120 l / h.

[0084] In another specific embodiment, the residence time of the gas stream mixture in the reaction vessel is less than 100 seconds; specifically 0.1 seconds to 80 seconds; more specifically 1 second to 60 seconds; still more specifically 2 seconds to 30 seconds; preferably 4 seconds to 16 seconds.

[0085] In addition to the gas stream mixture, one or more sheath gas streams may be introduced into the reaction vessel of the present invention. Sheath gas streams include, but are not limited to, nitrogen, hydrogen, and noble gases such as helium and argon.

[0086] In the process of the present invention, the mole fraction (xi) of the at least one precursor compound in the gas stream mixture is at least 0.010.

[0087] In a particular embodiment, the mole fraction of at least one precursor compound in the gas stream mixture is at least 0.012; preferably at least 0.015; more particularly still 0.01 to 0.5; preferably 0.015 to 0.400; more preferably 0.016 to 0.100; more preferably about 0.02. In the context of the present invention, the mole fraction is expressed as the amount of one component (in moles) divided by the total amount of all components (also expressed in moles).

[0088] In a particular embodiment, at least one precursor compound according to the invention is present in an amount of at least 0.1*10 -4 mol / l; in particular at a concentration of at least 1*10 -4 mol / l; more particularly at a concentration of at least 1.5*10 -4 mol / l; more particularly at a concentration of at least 2*10 -4 mol / l concentration in the gas stream mixture.

[0089] In a particular embodiment, the gas stream mixture comprises H2.

[0090] In one embodiment, the gas stream mixture of the process of the present invention comprises:

[0091] - at least one precursor compound;

[0092] - at least one sheath gas, such as nitrogen, hydrogen and / or a noble gas; and

[0093] -Metal catalyst particles.

[0094] In one embodiment, the gas stream mixture of the process of the present invention consists of:

[0095] - at least one precursor compound;

[0096] - at least one sheath gas, such as nitrogen, hydrogen and / or a noble gas; and

[0097] -Metal catalyst particles.

[0098] In a preferred embodiment, the gas stream mixture of the process of the present invention consists of:

[0099] - as a precursor compound of a metal hydride or an organometallic compound; wherein the metal element of the metal hydride or the organometallic compound is at least one element selected from Si, Ge, Al, Cu, Zn, Sb, Ni, Ti, Se, Ta, Pt, Mo, V, W, Co, Mn and Li; preferably selected from Si, Ge, Al, Cu, Zn, Pt, Mo, V, W, Co, Mn and Li; in particular Si, Ge, Al, Cu, Zn, Pt and Co; more particularly Si, Ge and Al; still more particularly Si and Ge; even more particularly Si;

[0100] - a sheath gas or gas mixture selected from nitrogen, hydrogen, a noble gas or a combination thereof; and

[0101] - Metal catalyst particles consisting of an element selected from Au, Ag, Cu, Fe, Ni, Ga, Co, Pt, In and Al; in particular consisting of an element selected from Au, Ag and Cu; in particular consisting of an element selected from Au and Ag; even more particularly consisting of Au.

[0102] Reaction vessel

[0103] In a specific embodiment, the reaction vessel used in the method of step (a) is a gas reaction vessel; preferably a cylindrical reaction vessel; more preferably a ceramic or metal cylindrical reaction vessel; still more preferably a stainless steel cylindrical reaction vessel, such as a tube.

[0104] According to the method of the invention, the first and second gas streams are mixed inside the reaction vessel.

[0105] In a particular embodiment, the temperature inside the reaction vessel is uniform; particularly uniform within 50 degrees along the reactor tube, more particularly uniform over 80 cm from the hot zone; particularly uniform between 30 cm and 50 cm of the hot zone.

[0106] In the method of step (a) of the method of the present invention, the temperature inside the reaction vessel is in the range of 200°C to 3000°C; preferably in the range of 300°C to 2800°C; more preferably in the range of 400°C to 2000°C; still more preferably in the range of 500°C to 1800°C.

[0107] In a particular embodiment, the pressure inside the reaction vessel is from 500 mbar to 20,000 mbar (50,000 Pa to 2,000,000 Pa); preferably from 900 mbar to 3,000 mbar (90,000 Pa to 300,000 Pa).

[0108] In a particular embodiment, the temperature inside the reaction vessel is achieved by any suitable heating means known in the art; preferably by plasma, arc discharge, resistance heating, hot wire heating, torch heating or flame heating means; more preferably by resistance heating, hot wire heating, torch heating or flame heating means.

[0109] Nanowire network growth

[0110] In step (a) of the method of the present invention, at least one precursor compound decomposes under the temperature conditions inside the reaction vessel and grows on the metal catalyst particles by gas-liquid-solid (VLS) and / or chemical vapor deposition (CVD) to form a nanowire network. In a specific embodiment, the nanowires grow while in the gas stream mixture (i.e. they are atomized). In a specific embodiment, at least one precursor compound decomposes under the temperature conditions inside the reaction vessel and grows on the metal catalyst particles by floating catalyst chemical vapor deposition (CVD) to form a nanowire network.

[0111] As required, one or more sheath gas streams can be introduced into the reaction vessel. In particular, the one or more sheath gas streams can be introduced between the gas stream mixture and the reaction vessel wall.

[0112] By selecting appropriate precursor compounds, gas flow, temperature, pressure and metal catalyst particles, nanowires can be grown in the axial or radial direction, or in a combination of the two growth modes; preferably, growth occurs in the axial direction; more preferably, growth occurs in the 110 direction; especially for Si nanowires.

[0113] Nanowire growth can be initiated by catalytic decomposition of at least one precursor compound on the surface of a metal catalyst particle and nucleation of the nanowire on the surface of the metal catalyst particle. After nucleation, the nanowire can grow in a directional manner and form an elongated object, i.e., a nanowire. Growth can occur by gas-liquid-solid (VLS) and / or chemical vapor deposition (CVD). At the same time, the nanowires reach a critical concentration and aggregate to form a nanowire network in a reaction vessel. Thus, the method of the present invention is a continuous aggregation method. Preferably, a gas mixture carrying metal catalyst particles flows through a reactor, and a nanowire network flows through the length of the reaction vessel. In one embodiment, the nanowire network comprises hollow nanowires, such as nanotubes. In one embodiment, the nanowire network comprises hollow and non-hollow nanowires, such as solid nanowires. In another embodiment, the nanowire network consists of hollow nanowires such as nanotubes.

[0114] In the context of the present invention, the expression chemical vapor deposition (CVD) is understood as a process in which one or more volatile precursor compounds react and / or decompose on the catalyst surface to produce a one-dimensional structure, such as a nanowire. The catalyst particles may be suspended in the gas phase, often referred to as floating catalysts. The particles may be in a molten or solid state and, as described above, may include additional elements to control and / or enhance the growth of the nanowires. Such additional elements include Group 16 elements, such as S, Se, Te or oxygen. The precursor may also be partially decomposed on the surface of the reactor.

[0115] In a specific embodiment, the method of the present invention for preparing a nanowire network is at least 1*10 -7 aerogel parameters; in particular, at least 1*10 -6 aerogel parameters; more particularly at least 2*10 -6 The aerogelation parameters were as follows.

[0116] In the context of the present invention, the expression "aerogelation parameter" is understood to be the product of the average aspect ratio (length / diameter) of the nanowires and the volume concentration (vc (volume of nanowires / volume of the reactor)).

[0117] In the context of the present invention, the expression "vapor-liquid-solid" (VLS) is a mechanism for growing one-dimensional structures such as nanowires by chemical vapor deposition through the direct adsorption of a gas (i.e., at least one precursor compound on the gas phase) onto liquid catalyst particles, which can rapidly adsorb the vapor to a supersaturation level and can initiate crystal growth from nucleated seeds at the gas-liquid-solid interface.

[0118] In a particular embodiment, the nanowire network is formed while being in the gas flow mixture (in the reaction vessel), in particular, a nanowire network in which the nanowires are aggregated (i.e., the nanowires are coupled, entangled, connected or fused therebetween) is obtained at the outlet of the reaction vessel of the present invention.

[0119] In a particular embodiment, the nanowire network is generated as a continuous process. Alternatively, the nanowire network can be generated discretely. In a preferred embodiment, the nanowire network is generated continuously.

[0120] In a particular embodiment, the method of step (a) further comprises the step of collecting the nanowire network on a substrate; preferably, wherein the substrate is a filter; more preferably a vacuum filter. In a more particular embodiment, the method further comprises the step of densifying the nanowire network; preferably by using a solvent or a mixture of solvents; more preferably an organic solvent or a mixture of organic solvents; still more preferably a solvent or a mixture of solvents comprising an alcohol group; even more preferably using isopropanol.

[0121] In a particular embodiment, the nanowire network is generated at a rate of at least 0.01 g / h; preferably at a rate of at least 0.02 g / h; more preferably at a rate of at least 0.05 g / h; and even more preferably at a rate of about 0.1 g / h.

[0122] In another specific embodiment, the nanowire network is generated at a rate of 0.01 g / h to 10 g / h; preferably at a rate of 0.02 g / h to 5 g / h; more preferably at a rate of 0.05 g / h to 1 g / h; and even more preferably at a rate of 0.09 g / h to 1 g / h.

[0123] Step (b)

[0124] Step (b) of the method for preparing an electrode of the present invention involves coating the nanowire network obtained from step (a) with a carbon coating by pyrolyzing a carbon precursor at a temperature of 500° C. to 1300° C. under an inert gas atmosphere.

[0125] The coating of step (b) is formed when the carbon precursor decomposes at a temperature of 500° C. to 1300° C. under an inert gas atmosphere to produce pyrolytic carbon, which is deposited on the nanowire network to produce a carbon coating.

[0126] The carbon precursor of step (b) may be any compound known in the art which decomposes at a temperature of 500° C. to 1300° C. under an inert gas atmosphere to produce pyrolytic carbon. Non-limiting examples of carbon precursors are organic molecules such as hydrocarbons, for example acetylene.

[0127] In a particular embodiment, step (b) of the method for preparing an electrode of the present invention is carried out at a temperature of 550°C to 1200°C; preferably 600°C to 1100°C; preferably 620°C to 1000°C; more preferably 650°C to 900°C; still more preferably 660°C to 850°C; even more preferably about 700°C.

[0128] Step (b) of the method for preparing an electrode of the present invention is carried out under an inert gas atmosphere, which means that it can be carried out under a rare gas atmosphere or under N2; for example, using a gas flow containing a sheath gas, wherein the sheath gas is selected from any rare gas or N2; preferably Ar or N2; more preferably Ar.

[0129] In a more specific embodiment, the carbon precursor is a hydrocarbon or a mixture of hydrocarbons; preferably, wherein the hydrocarbon or the mixture of hydrocarbons contains hydrocarbons having a carbon atom number equal to or less than 10; more preferably equal to or less than 9, equal to or less than 8, equal to or less than 7, equal to or less than 6, equal to or less than 5, equal to or less than 4 or equal to or less than 3.

[0130] Non-limiting examples of hydrocarbons suitable as carbon precursors are methane, ethane, ethylene, acetylene, propane, propylene, methylacetylene, cyclopropane, propadiene, butane, butane, butyne, cyclobutane, butadiene, pentane, pentene, pentyne, cyclopentane, pentadiene, hexane, hexane, hexyne, cyclohexane, hexadiene or mixtures thereof; preferably methane, ethane, ethylene, acetylene, propane, propylene, methylacetylene, cyclopropane, propadiene, butane, butane, butyne, cyclobutane, butadiene, pentane, pentene, pentyne, cyclopentane, pentadiene and mixtures thereof; more preferably methane, ethane, ethylene, acetylene, propane, propylene, methylacetylene, cyclopropane, propadiene, butane, butane, butyne, cyclobutane, butadiene and mixtures thereof.

[0131] In a more particular embodiment, the carbon precursor is in a gas or vapor phase; preferably a gas.

[0132] In one embodiment, step (b) is carried out in the same reaction vessel as step (a).

[0133] In a more particular embodiment, the carbon precursor is part of an additional gas stream introduced into the reaction vessel of step (a); preferably further comprising an inert gas.

[0134] In a particular embodiment, the volume of the carbon precursor is at least 1% of the total volume of the gas stream; preferably at least 2%; more preferably at least 3%; and even more preferably about 5%.

[0135] While not being bound by theory, the inventors have observed that, as a result of the carbon pyrolytic deposition step of the electrode synthesis process, the carbon coating of the electrode of the present invention comprises crystalline graphite domains that improve the electrochemical properties of the electrode, in particular its electrical conductivity. In addition, the interface between the nanowires of the network and the carbon coating comprises a majority of aligned crystalline graphite domains, improving the final performance of the electrode.

[0136] In a particular embodiment, step (b) further comprises the step of drying the nanowires coated with the carbon coating; preferably at a temperature of 80°C to 150°C; more preferably at a temperature of 90°C to 140°C; and even more preferably at a temperature of about 120°C.

[0137] In one embodiment, the drying step is performed under vacuum.

[0138] In another embodiment, the drying step is performed for at least 4 hours; preferably at least 6 hours.

[0139] In a particular embodiment, step (b) further comprises the step of pressing the nanowires coated with the carbon coating; preferably, mechanically pressing the nanowires coated with the carbon coating; more preferably, applying 10 5 Pa to 10 10 Pa, preferably 10 6 Pa to 10 9 Pa, more preferably about 10 8 Pa's pressure.

[0140] Step (c)

[0141] The method of the present invention optionally comprises the further step (c) of contacting the carbon coated nanowire network with an electrical connection or current collector.

[0142] In one embodiment, the electrical connection or current collector comprises a conductive material, such as a metallic material, for example a metal wire. The electrical connection of the foregoing embodiments may be accomplished by any method known in the art.

[0143] electrode

[0144] As mentioned above, in a second aspect, the present invention relates to an electrode obtained by any specific embodiment of the method according to the present invention, said electrode comprising:

[0145] - A nanowire network coated with a carbon coating;

[0146] wherein the nanowires of the nanowire network have an aspect ratio of at least 130;

[0147] wherein the carbon coating comprises graphitic carbon;

[0148] wherein the amount of the carbon coating is greater than 3 weight % of the total weight of the nanowire network coated with the carbon coating; and

[0149] - Optional electrical connections and / or current collectors.

[0150] In a particular embodiment, the nanowires of the nanowire network of the electrode of the invention form a mesh; preferably, the nanowires of the nanowire network are joined, entangled, connected, fused or interlocked between them; preferably joined, entangled, connected or fused; more preferably form joints between them. In one embodiment, the mesh comprises aggregates of nanowires. In a particular embodiment, the mesh is self-supporting.

[0151] In a particular embodiment, the nanowire network is self-supporting. In the context of the present invention, the term "self-supporting" refers to a structure that is not supported by other objects or structures (such as a substrate). In one embodiment, the nanowire network does not contain additional phases such as additional matrix or binder. In an alternative embodiment, the nanowire network consists of nanowires.

[0152] In a particular embodiment, the nanowires of the network of the electrode of the invention are aggregated; in particular strongly aggregated; in particular, they are strongly aggregated by secondary forces such as van der Waals forces, permanent dipoles, hydrogen bonds and / or covalent bonds, entanglements and other forms of mechanical interlocking. In the context of the present invention, strongly aggregated means that the material forms a solid object and the nanowires comprising the network cannot be easily dispersed without resorting to ultrasonic treatment, stirring, cutting or similar methods.

[0153] In a particular embodiment, the nanowire network of the electrode of the invention is a continuous network. In the context of the present invention, a continuous network is understood as a percolating, non-discrete network.

[0154] In a particular embodiment, the nanowire network of the invention is an aerogel, i.e., a solid material of low density; preferably with a density of less than 10 -2 g / cm 3 ; preferably less than 10 -3 g / cm 3 ; More preferably less than 10 -4 g / cm 3 ; More preferably less than 10 -5 g / cm 3 In one specific embodiment, the nanowire network of the present invention has a molecular weight of at least 0.001 g / cm 3 ; especially at least 0.01g / cm 3 density.

[0155] In a more particular embodiment, the nanowire network of the electrode of the invention is densified; in particular by mechanical methods, solvent addition methods, electromagnetic methods or the like.

[0156] In a particular embodiment, the nanowires of the network of the invention have an average aspect ratio (length / diameter) of at least 135; more preferably at least 140; more preferably at least 150; still more preferably at least 200; even more preferably at least 250.

[0157] In a more specific embodiment, the average aspect ratio (length / diameter) of the nanowires of the network of the present invention is from 135 to 1000; specifically, from 140 to 800; more specifically, from 150 to 700. The average aspect ratio of the nanowires of the network of the present invention can be calculated by averaging the values ​​obtained by measuring the size of a large number of nanowires (e.g., more than 100) using an electron microscope.

[0158] In a particular embodiment, the average length of the nanowires of the network of the present invention is at least 1 micron; in particular at least 2 microns; preferably at least 3, 4 or 5 microns; more preferably at least 10 microns. In a particular embodiment, the average length of the nanowires of the network of the present invention is 1 to 30 microns; preferably 2 to 20 microns; more preferably 3 to 15 microns. The average length of the nanowires of the network of the present invention can be calculated by the average of the values ​​obtained by measuring the length of more than 100 nanowires using an electron microscope.

[0159] In a particular embodiment, the nanowires of the nanowire network of the electrode of the present invention comprise at least one material selected from the group consisting of: Al x Ga 1-x As y P 1-y 、AlN、Al z Ga x In 1-x-z N, Si, SiC, Ge or Si x Ge 1-x 、SiO x 、TiO x 、ZnO x 、 x 、MoS y , WS y 、MoTe y 、TaSe y 、NbSe y 、NiTe y , BN, Cu, Pt, CoO x 、MnO x , CuO x , VO x , Lix Mn y O. Li x Ni y Mn z O and Ni x , wherein 0≤x≥1, 0≤y≥1 and 0≤z≥1; preferably comprising Si, SiC, Ge or Si x Ge 1-x and SiO x , wherein 0≤x≥1; more preferably Si, Ge or Si x Ge 1-x and SiO x , wherein 0≤x≥1; more preferably comprising Si or Ge; and even more preferably comprising Si.

[0160] In another specific embodiment, the nanowires of the nanowire network of the electrode of the present invention are composed of at least one material selected from the group consisting of: Al x Ga 1-x As y P 1-y 、AlN、Al z Ga x In 1-x-z N, Si, SiC, Ge or Si x Ge 1-x 、SiO x 、TiO x 、ZnO x 、 x 、MoS y , WS y 、MoTe y 、TaSe y 、NbSe y 、NiTe y , BN, Cu, Pt, CoO x 、MnO x , CuO x , VO x , Li x Mn y O. Li x Ni y Mn z O and Ni x , wherein 0≤x≥1, 0≤y≥1 and 0≤z≥1; preferably comprising Si, SiC, Ge or Si x Ge 1-x and SiO x , wherein 0≤x≥1; more preferably Si, Ge or Si x Ge 1-x and SiO x, wherein 0≤x≥1; more preferably comprising Si or Ge; and even more preferably comprising Si.

[0161] In a particular embodiment, the nanowires of the nanowire network of the electrode of the present invention comprise at least one material selected from the group consisting of: Al x Ga 1-x As y P 1-y 、AlN、Al z Ga x In 1-x-z N, Si, SiC, Ge or Si x Ge 1-x 、SiO x 、TiO x 、ZnO x 、 x 、MoS y , WS y 、MoTe y 、TaSe y 、NbSe y 、NiTe y , BN, Cu, Pt, CoO x 、MnO x , CuO x , VO x , Li x Mn y O. Li x Ni y Mn z O and Ni x , wherein 0≤x≤2, 0≤y≤2 and 0≤z≤2; preferably comprising Si, SiC, Ge or Si x Ge 1-x and SiO x , wherein 0≤x≤2; more preferably Si, Ge or Si x Ge 1-x and SiO x , wherein 0≤x≤2; more preferably comprising Si or Ge; and even more preferably comprising Si.

[0162] In a particular embodiment, the nanowires of the nanowire network of the electrode of the present invention comprise at least one material selected from the group consisting of: Al x Ga 1-x As y P 1-y 、AlN、Al z Ga x In 1-x-z N, Si, SiC, Ge or Si x Ge 1-x 、SiOx 、TiO x 、ZnO x 、 x 、MoS y , WS y 、MoTe y 、TaSe y 、NbSe y 、NiTe y , BN, Cu, Pt, CoO x 、MnO x , CuO x , VO x , Li x Mn y O. Li x Ni y Mn z O and Ni x , wherein 0≤x≤2, 0≤y≤2 and 0≤z≤2; preferably comprising Si, SiC, Ge or Si x Ge 1-x and SiO x , wherein 0≤x≤2; more preferably Si, Ge or Si x Ge 1-x and SiO x , wherein 0≤x≤2; more preferably comprising Si or Ge; and even more preferably comprising Si.

[0163] In a particular embodiment, the volume density of the nanowire network of the electrode of the present invention is at least 0.01 g / cm 3 ; especially at least 0.05 g / cm 3 ; more particularly at least 0.075 g / cm 3 ; more particularly at least 0.080 g / cm 3 ; preferably at least 0.015 g / cm 3 More preferably at least 0.020 g / cm 3 ; Still more preferably about 0.128 g / cm 3 .

[0164] In a specific embodiment, the volume density of the nanowire network of the electrode of the present invention is 0.01 g / cm 3 Up to 0.2g / cm 3 ; especially 0.07g / cm 3 Up to 0.30g / cm 3 The volume density of the nanowire network of the present invention can be calculated by any experimental technique known in the art, and in particular it is determined from the area density and thickness of a sample of the nanowire network.

[0165] In a particular embodiment, the nanowires of the nanowire network are entangled; preferably physically entangled.

[0166] In a particular embodiment, the nanowire network is a network comprising nanowires. In a particular embodiment, the nanowires forming the network can have the same or different properties. In a more specific embodiment, the nanowires contained in the network have different compositions and / or aspect ratios.

[0167] In a particular embodiment, the nanowires of the nanowire network are hollow (i.e., they are nanotubes); preferably, they are nanotubes. In a more particular embodiment, the hollow nanowires comprise Si, SiC, Ge, or Si x Ge 1-x and SiO x , wherein 0≤x≤2; more preferably consisting of at least one material selected from Si and Ge; and even more preferably consisting of Si.

[0168] In a particular embodiment, the nanowire network further comprises metal catalyst particles; in particular, metal catalyst particles of the method of the present invention.

[0169] In a specific embodiment, the nanowire network of the present invention further comprises particles; preferably quasi-spherical particles; more preferably quasi-spherical amorphous particles.

[0170] In a particular embodiment, the nanowire network consists of nanowires and catalyst particles and optional particles; in particular quasi-spherical or spherical particles, for example, wherein the quasi-spherical particles are the result of pyrolysis of the precursor compound of the method of step (a).

[0171] In a particular embodiment, the nanowires of the nanowire network further comprise an identification or labeling element or compound; wherein the labeling element or compound enables traceability. In a particular embodiment, the identification or labeling of the nanowires is performed during the synthesis process, or in an additional step after the synthesis.

[0172] In a particular embodiment, the nanowires of the nanowire network are majority aligned.

[0173] In a particular embodiment, the nanowires of the nanowire network are aligned by electromagnetic methods, electrochemical methods, fluid-based methods, or other methods.

[0174] In one embodiment, the nanowire network of the electrode of the present invention comprises a crystalline phase and an amorphous phase; preferably, the crystalline phase is at least 50 weight % of the total weight of the network; more preferably at least 75 weight %; still more preferably at least 90 weight %; even more preferably, the crystalline phase comprises crystalline nanowires and the amorphous phase comprises amorphous particles; preferably amorphous spherical particles.

[0175] In one embodiment, the nanowire networks of the invention comprise at least 50 wt%; preferably at least 75 wt%; more preferably at least 80 wt%; even more preferably at least 90 wt% crystalline nanowires, based on the total weight of the network.

[0176] In one embodiment, the nanowires of the nanowire network are crystalline.

[0177] In one embodiment, the nanowire network has a fracture energy value of at least 0.05 J / g; preferably 0.1 to 0.5 J / g. The fracture energy value is measured by mechanical tensile testing of a nanowire network sample using conventional mechanical testing equipment known in the art.

[0178] In one embodiment, the nanowire network has a specific tensile strength of more than 0.5 MPa / SG; preferably more than 0.8 MPa / SG, more preferably more than 1 MPa / SG. In particular, the specific tensile strength value is in units of MPa / SG, where SG stands for specific gravity, which is numerically equal to g / cm 3 The specific tensile strength can be measured by any tensile testing technique known in the art, for example, by mechanical tensile measurement of a nanowire network sample using a Textechno Favimat tensile tester at a strain rate of 10% / min and preferably at a gauge length of 5 mm.

[0179] Carbon coating

[0180] In the context of the present invention, the expression "carbon coating" relates to a carbon-based coating; in particular, the carbon coating is obtained after step (b) of the method of the present invention by pyrolyzing a carbon precursor at a temperature of 500°C to 1300°C under an inert gas atmosphere to obtain a nanowire network coated with a carbon coating.

[0181] In one embodiment, the amount of carbon coating is greater than 3 wt %; preferably greater than 5 wt %; preferably greater than 6, 7 or 8 wt %; more preferably greater than 10 wt %; more preferably greater than 12 wt %; still more preferably greater than 15 wt % of the total weight of the nanowire network coated with the carbon coating.

[0182] In one embodiment, the amount of carbon coating is greater than 3 wt% and less than 50 wt%; preferably greater than 5 wt% and less than 49 wt%; preferably greater than 5, 6, 7 or 8 wt% and less than 45, 46 or 47 wt%; more preferably greater than 10 wt% and less than 40 wt%; more preferably greater than 12 wt% and less than 38 wt%; still more preferably greater than 15 wt% and less than 35 wt% of the total weight of the nanowire network coated with the carbon coating.

[0183] In one embodiment, the amount of the carbon coating is about 27 weight percent of the total weight of the nanowire network coated with the carbon coating.

[0184] The carbon coating comprises graphitic carbon.

[0185] In one embodiment, the carbon coating consists of graphitic carbon and non-graphitic carbon (eg, amorphous carbon).

[0186] In a particular embodiment, the graphitic carbon of the carbon coating includes graphitic planes of carbon aligned with crystal planes of the nanowires at the interface between the carbon coating and the nanowires.

[0187] In a more specific embodiment, when the nanowire is a Si nanowire, the graphitic (002) basal planes of the graphitic carbon of the carbon coating are oriented parallel to the Si (111) planes of the Si nanowire at the interface between the carbon coating and the nanowire.

[0188] In the context of the present invention, the expression "graphitic carbon" is understood to be all kinds of substances consisting of elemental carbon in the allotropes of graphite, regardless of the presence of structural defects or packing disorder. The presence of graphitic carbon on a sample can be detected by diffraction methods known in the art.

[0189] In one embodiment, the electrode of the present invention has a porosity of 60% to 90%; specifically 65% ​​to 85%; more specifically 70% to 80%; and more specifically about 78%. The porosity of the electrode is measured using methods known in the art, such as determining the volume of a conventional sample by optical and / or electron microscopy and measuring its weight by gravimetric analysis.

[0190] In one embodiment, the electrode of the present invention has a thickness of 0.05 to 0.70 g / cm 3 ; preferably 0.10 to 0.65 g / cm 3 , more preferably 0.40 to 0.60 g / cm 3 More preferably about 0.51g / cm 3 The bulk density of the electrode is measured by gravimetrically determining the mass and dividing it by the volume of the electrode.

[0191] In one embodiment, the electrodes of the present invention are electrically conductive. In a more specific embodiment, the in-plane and out-of-plane conductivity of the electrodes of the present invention are in the range of 1-1.5 S / m and 0.1 to 0.6 S / m, respectively. The conductivity of the electrodes is measured by two-probe resistance measurement using flat metal tape contacts as known in the art.

[0192] Battery

[0193] In another aspect, the invention relates to a battery comprising:

[0194] - electrodes, wherein at least one electrode of the present invention is as described in any embodiment;

[0195] - electrolytes; and

[0196] - Device for connection to a power / load source.

[0197] In one embodiment, the electrolyte of the battery of the present invention comprises lithium. In a particular embodiment, the battery is a lithium battery; preferably a lithium ion battery.

[0198] In one embodiment, at least one electrode is a working electrode. In another embodiment, at least one electrode is an anode.

[0199] In another embodiment, the electrolyte of the battery is a gel electrolyte. In another embodiment, the electrolyte of the battery is a solid.

[0200] use

[0201] Another aspect of the present invention relates to the use of the electrode in any specific embodiment of the present invention in a battery; preferably in a lithium battery; more preferably in a lithium ion battery.

[0202] An additional aspect of the invention relates to a method for storing or delivering electricity comprising the steps of using an electrode according to any specific embodiment of the invention in a battery; preferably a lithium battery; more preferably a lithium ion battery.

[0203] It should be understood that the scope of the present disclosure includes all possible combinations of the embodiments disclosed herein.

[0204] Example

[0205] The invention is illustrated by the following examples, which in no way limit the scope of the invention.

[0206] Example 1: Electrode

[0207] The electrodes were fabricated by coating a nanowire network comprising silicon (Si) nanowires with a uniform carbon coating.

[0208] Nanowire networks comprising silicon (Si) nanowires are produced by decomposing Si precursors in the presence of catalyst nanoparticles suspended in a gas stream inside a reaction vessel. In particular, the Si nanowire network is synthesized by floating catalyst chemical vapor deposition (FCCVD) at 650°C using a continuous flow of an aerosol of gold nanoparticles as a catalyst, silane as a precursor, and a mixture of nitrogen and hydrogen as a carrier gas. The mole fraction of the gas is maintained at 18:31:1 (N2:H2:SiH4). The reaction vessel used is a metal reaction tube inside a tube furnace.

[0209] After the synthesis of the Si nanowire network, the network was coated with carbon by pyrolyzing acetylene gas (5 vol% in Ar) at 700°C to form an electrode. The mass fraction of carbon in the electrode (nanowire network and carbon coating) was determined gravimetrically using a 5-digit high-precision weighing balance. The Si nanowire network coated with carbon was then dried at 120°C under vacuum overnight and heated to 100°C using a simple press at ambient temperature. 8 The result is a fully formed electrode.

[0210] Figure 1 Images of a free-standing Si nanowire network before (a) and after (b) carbon coating are shown.

[0211] Mechanical test results (not shown in this article) show that the network structure of the electrodes makes them flexible when bent and gives them mechanical properties similar to other fibrillar solids (such as paper), with a fracture strain above 10% and an average specific strength of 1.2 MPa / SG. Due to its mechanical robustness, the carbon-coated Si nanowire network is directly combined with a copper current collector without the need for polymer binders or other forms of mechanical reinforcement as in other granular electrodes.

[0212] Figure 2 Shown is an electron micrograph of a Si nanowire network before carbon coating. Figure 3 HRTEM micrograph showing the interface between the carbon coating and the crystalline Si nanowires of the Si nanowire network after carbon coating. Figure 3 The results indicate a preferred alignment of carbon graphite planes at the interface between the carbon coating and the Si nanowires. In addition, Figure 4 Representative Raman spectra are shown, illustrating the crystallinity of the Si nanowires and the graphitization of the coating on the carbon-coated Si nanowire network. Figure 5 An XRD pattern is shown which shows the absence of crystalline SiO2 on the nanowires.

[0213] The nanowires of the obtained nanowire network have an average length of at least 2 microns. The average diameter and aspect ratio of the nanowires are obtained by a large number of measurements performed by image analysis of scanning electron micrographs at high magnification. The nanowire length is calculated by the product of the diameter and the aspect ratio. In addition, the nanowires of the nanowire network are crystalline. Relative to the total weight of the nanowire network coated with carbon (i.e., the electrode excluding the current collector), the sample contains greater than 66.5% crystalline Si nanowires by weight.

[0214] The results of analyzing the samples by electron microscopy showed a C coating with an average thickness of 3.8 ± 1.3 nm, which was uniform throughout the electrode. The carbon coating of the Si network was a combination of graphitic and amorphous domains. Small stacks of graphitic planes could be directly observed by high-resolution transmission electron microscopy ( Figure 3 ). Raman spectroscopy ( Figure 4 ) also confirms that the sp 2 The carbonization process was performed on the silicon nanowires in the presence of a high fraction of hybridization. Furthermore, no passivating SiO2 layer was found on the silicon nanowires after the carbonization process, either by electron microscopy or in the XRD diffraction patterns. Instead, the interface between the silicon nanowires of the network and the carbon coating contained a majority of aligned crystalline silicon and crystalline graphite domains. Furthermore, it was observed that the graphite (002) basal planes of the coating were oriented parallel to the Si (111) planes of the nanowires and were thus tilted relative to the longitudinal axis of the silicon nanowires, as shown in Figure 2. Figure 3 The inventors believe that the carbon pyrolysis step of the electrode synthesis method is responsible for the chemical reduction of the silicon nanowire surface and the deposition of graphitic carbon planes assisted by nucleation on the crystalline silicon nanowires.

[0215] The mass fraction of the carbon coating, measured by gravity, averaged about 27 wt % of the total mass of the silicon nanowire network and the carbon coating. The electrode volume density was 0.51 g / cm 3 , which corresponds to a porosity of 78%. For different samples of Si nanowire networks coated with carbon, the in-plane conductivity (σ IP ) and the out-of-plane conductivity (σ OOP ) are in the range of 1-1.5 S / m and 0.1 to 0.6 S / m, respectively. Two-probe resistance measurements were performed on the electrode samples using flat copper tape contacts. The high conductivity values ​​obtained are a result of the high uniformity and high graphitization of the carbon coating.

[0216] Thus, the results indicate that the ongoing pyrolysis reaction effectively coats the Si nanowire network with a thin (eg, low mass fraction), uniform carbon layer that can provide high electrical conductivity values.

[0217] In contrast, the conductivity values ​​of electrodes containing only the nanowire network and electrical connections or current collectors (without the carbon coating) were much lower.

[0218] By comparison with other carbon materials such as carbon black, graphene or carbon nanotubes, the inventors observed that in order to reach conductivity values ​​similar to those of the coated electrodes of the invention, larger amounts of those materials in denser samples are required.

[0219] Sample characterization

[0220] The samples were characterized using field effect scanning electron microscopy (FESEM, FEI Helios NanoLab 600i, using TLD and CBS detectors to acquire images simultaneously), transmission electron microscopy (TEM, Talos F200X FEG, 200 kV), Raman spectroscopy (Ranishaw, using a 532 nm laser source), and 2D wide angle X-ray scattering (WAXS) and small angle X-ray scattering (SAXS). A microfocus with a diameter of ~10 μm and WAXS / SAXS data were collected at a radiation wavelength of . The collected pattern shown was corrected for background scattering and obtained after azimuthal integration.

[0221] Electrochemical performance

[0222] The performance of the electrodes was investigated in two-electrode and three-electrode cell configurations using a bioelectrochemical workstation (VMP300) and a Neware battery tester (CT-4008-5V10mA-164).

[0223] Button cells (CR 2032) were assembled as follows: the above-mentioned Si network coated with carbon nanowires as the working electrode, a circular lithium foil as the counter electrode, a Whatman GF / D disk facing the working electrode and a PP film (25 μm) as a separator, and 1 M LiPF6 and 10 wt% fluoroethylene carbonate (FEC) in ethylene carbonate / diethyl carbonate (1:1 v / v, Solvionic) as the electrolyte.

[0224] By galvanostatic cycling at C-rates from C / 20 to 2C, the + The battery was characterized by cyclic voltammetry at a scan rate of 0.1-10 mV / s in the voltage window of 1.5-0.01 V. For the galvanostatic measurement, 1C was considered to be 3579 mAh / g, corresponding to Li 15 The formation of Si4 phase was also investigated using electrochemical impedance spectroscopy at 10 MHz. -2 The cells were characterized in a frequency window of 1 MHz with an AC amplitude of 10 mV. The specific capacity values ​​were normalized by the mass of silicon.

[0225] Figure 6(a) The first 10 cyclic voltammograms at a scan rate of 0.025 mV / s and (b) the rate performance (specific capacity vs. cycle number) at C rates from C / 20 to 2C obtained using a carbon-coated Si nanowire network as an electrode in a half-cell. Electrode mass loading: 1.2 mg / cm 2 .

[0226] In particular, Figure 6 b shows a comparison of the rate performance of a carbon-coated Si nanowire network as an electrode in a half-cell at C rates ranging from C / 20 (≈0.179 mA / g) to 2C (≈7.2 mA / g) for two different C contents, i.e., 5 wt.% (triangles) and 27 wt.% (circles) carbon relative to the total weight of the nanowire network and carbon coating.

[0227] The results showed (see Figure 6 (b) For the two Si nanowire network electrodes with different amounts of C coating, the first discharge (lithiation) capacity including the solid electrolyte interface (SEI) formation exceeds 4200 mAh / g (close to Li 4.4 Theoretical capacity of silicon when Si is formed). Figure 6 It can be seen that after SEI formation, a reversible capacity of up to 3310 mAh / g of the optimized electrode (with 27 wt % carbon coating) was obtained at C / 20 (1C is 3.6 A / g) and remained stable, while the capacity of the electrode with 5 wt % carbon coating decreased to 2500 mAh / g in the second cycle and to 1280 mAh / g after 5 cycles. The specific capacity of the optimized electrode with 27 wt % carbon coating is significantly higher at all C-rates.

[0228] The initial Coulombic efficiency (ICE, e.g., the ratio of charge capacity to discharge capacity in the first cycle) of a Si nanowire network coated with 27 wt% carbon and acting as an electrode was estimated to be ~72%, while for a Si nanowire network with only 5 wt% C coating, it was about ~55%.

[0229] The Si nanowire network anode of the present invention coated with 27 wt % carbon coating tested in a half-cell demonstrated a capacity close to the theoretical value (3041 mAh / g) at low rates, even at 3.1 mg / cm 2 (9.3mAh / cm 2 ) is also true at high surface density.

[0230] Test the electrochemical stability of the electrode. Figure 7The specific capacity (i) and coulombic efficiency (ii) of the carbon-coated Si nanowire network as an electrode at C-rate vs. (a) 100 cycles at C / 10 and (b) 500 cycles at C / 2 are shown. The results show that at C / 10 rate, after 100 charge-discharge cycles, the material retains 75% of its initial capacity, while the coulombic efficiency increases from 97.6% to 99.1%. At a faster charge-discharge rate of C / 2, it retains about 60% of the initial capacity, and the coulombic efficiency increases from 98.8% to 99.9%. Therefore, it can be concluded that the optimized electrode of the present invention exhibits high stability and high initial specific capacity.

[0231] Example 2: Comparative Example

[0232] In a comparative example, an electrode consisting of a nanowire network comprising silicon (Si) nanowires synthesized as described in Example 1 but without a carbon coating and interspersed carbon nanotubes was fabricated. The carbon nanotubes acted as a conductive additive.

[0233] For this example, electrodes were prepared by drop casting an aqueous dispersion of carbon nanotubes onto a Si nanowire network. The aqueous dispersion consisted of a standard commercial mixture of single-walled carbon nanotubes in water. After casting the carbon nanotube dispersion, the electrodes were dried in an electric vacuum oven at 120 °C overnight and immediately transferred to a glove box to assemble a coin cell similar to that described in Example 1. The mass fraction of SWCNTs in the electrode was estimated based on the drop cast volume, yielding a value of 2.5 wt % of the total electrode weight.

[0234] Figure 8 A comparison of the rate performance of a carbon-coated Si nanowire network (circles) and a Si nanowire network with interspersed carbon nanotubes (squares) as electrodes at C-rates from C / 20 (≈0.179 mA / g) to 2C (≈7.2 mA / g) in a half-cell is shown.

[0235] Figure 8 The results in show that the Si nanowire network with interspersed carbon nanotubes has a much lower specific capacity at all rates compared to the Si nanowire network anode with carbon coating.

Claims

1. A method for preparing an electrode, comprising: (a) preparing a nanowire network by a method comprising the following steps: i. providing a first gas flow to the reaction vessel; wherein the first gas stream comprises at least one precursor compound, the precursor compound comprising at least one element selected from Si, Ge, Al, Cu, Zn, Sb, Ni, Ti, Se, Ta, Pt, Mo, V, W, Co, Mn and Li; wherein the at least one precursor compound is a metal hydride or an organometallic compound; and ii. providing a second gas flow to the reaction vessel, the second gas flow comprising metal catalyst particles; so that the first gas flow and the second gas flow are mixed in the reaction vessel to form a gas flow mixture; wherein the metal catalyst particles comprise one or more elements selected from Au, Ag, Cu, Fe, Ni, Ga, Co, Pt, In and Al; wherein the mole fraction (xi) of the at least one precursor compound in the gas stream mixture is at least 0.010; Wherein, the temperature inside the reaction container is in the range of 200°C to 3000°C; wherein the at least one precursor compound decomposes at a temperature inside the reaction vessel and grows on the metal catalyst particles by vapor-liquid-solid (VLS) and / or chemical vapor deposition (CVD) to form a nanowire network; and (b) coating the nanowire network obtained from step (a) by pyrolyzing a carbon precursor at a temperature of 500° C. to 1300° C. under an inert gas atmosphere to obtain a nanowire network coated with a carbon coating; (c) Optionally, contacting the carbon-coated nanowire network with an electrical connection or current collector.

2. The method according to claim 1, wherein: The at least one precursor compound of step (a) comprises an element selected from Si and Ge.

3. A method according to any preceding claim, wherein: The at least one precursor compound of step (a) is selected from (3-aminopropyl)triethoxysilane, N-sec-butyl(trimethylsilyl)amine, chloropentamethyldisilane, tetramethylsilane, silicon tetrabromide, silicon tetrachloride, tri(tert-butoxy)silanol, SiHH4, tetramethylgermanium, triethylgermanium hydride, triphenylgermanium hydride, triphenylgermanium hydride, tetramethylgermanium, tributylgermanium hydride, triethylgermanium hydride and triphenylgermanium hydride.

4. A method according to any preceding claim, wherein: The metal catalyst particles of step (a) are gold particles; preferably having a diameter of 0.1 to 100 nm.

5. A method according to any preceding claim, wherein: The gas flow mixture of step (a) comprises H2; and / or wherein the inert atmosphere of step (b) comprises argon or nitrogen.

6. A method according to any preceding claim, wherein: The carbon precursor of step (b) is an organic molecule; preferably a hydrocarbon.

7. An electrode obtained by a method according to any preceding claim, comprising: - A nanowire network coated with a carbon coating; wherein the aspect ratio of the nanowires of the nanowire network is at least 130; wherein the carbon coating comprises graphite carbon; wherein the amount of the carbon coating is greater than 3 weight % of the total weight of the nanowire network coated with the carbon coating; - Optionally, electrical connections and / or current collectors.

8. The electrode according to claim 7, wherein The nanowire composition is selected from Si, SiC, Ge, Si x Ge 1-x 、SiO x 、Al x Ga 1-x As y P 1-y 、Al z Ga x In 1-x-z N, AlN, Cu, CuO x 、ZnO x , GaSb, Ga x In 1-x As y Sb 1-y 、NiTe y , Li x Ni y Mn z O、Ni x 、TiO x 、NbSe y 、 x 、TaSe y 、Pt、MoTe y 、MoS y , VO x , WS y 、CoO x 、MnO x , Li x Mn y O and Li x Ni y Mn z O; wherein 0≤x≥1, 0≤y≥1 and 0≤z≥1; preferably, wherein the nanowire is made of Si, SiC, Ge or Si x Ge 1-x and SiO x Composition, where 0≤x≥1.

9. The electrode according to any one of claims 7 or 8, in, The nanowires of the nanowire network are crystalline; wherein the amount of the carbon coating is at least 5 weight % of the total weight of the nanowire network coated with the carbon coating.

10. The electrode according to claim 9, wherein The graphitic carbon of the carbon coating comprises carbon graphitic planes aligned with crystallographic planes of the nanowires at an interface between the carbon coating and the nanowires.

11. The electrode according to any one of claims 7 to 10, wherein The carbon coating has a thickness of 1 to 10 nm; and / or Wherein, the carbon coating has a carbon content of 0.05 to 0.70 g / cm 3 The bulk density of the electrode is measured by gravimetrically determining the mass and dividing it by the volume of the electrode.

12. An electrode according to any one of claims 7 to 11, consisting of a nanowire network coated with a carbon coating and optionally an electrical connection or current collector; and / or in, The carbon coating layer consists of graphite carbon and amorphous carbon.

13. A battery comprising: - electrodes, wherein at least one electrode is as claimed in any one of claims 7 to 12; - electrolytes; and - Device for connection to a power / load source.

14. The battery according to claim 13, wherein The electrode as claimed in any one of claims 7 to 12 is a working electrode.

15. The battery according to any one of claims 12 or 14, wherein The electrolyte includes lithium.

16. Use of the electrode according to any one of claims 7 to 12 in a battery, preferably a lithium battery.