High purity iron-containing material and production system and method thereof
The high-purity iron oxide powder is extracted from low-purity iron ore through acid leaching and hydrolysis processes and reduced to high-purity iron metal, which solves the problem of battery pack performance reduction caused by impurities in low-purity iron materials and achieves high The production of low-purity iron materials, suitable for a variety of uses.
Patent Information
- Application Number
- CN202380035581.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-25
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-29
AI Technical Summary
When existing iron-based battery packs use low-purity iron materials, due to the presence of impurities such as silica, calcium oxide, magnesium oxide, etc., the performance of the battery pack is reduced, making it difficult to achieve high-purity and low-cost iron material production.
The iron-rich solution is produced by acid-lime low-purity iron ore. It is formed by purification and hydrolysis, and the high-purity iron oxide powder is reduced to high-purity iron metal, so that the apparent density is less than 3g/cc and the silica content is less than 0.5% iron material.
The production of high-purity iron materials is achieved at low cost, reducing battery pack performance losses, and meeting the needs of a variety of end-uses, including the supply of high-purity iron metals in the fields of battery packs and steelmaking.
Smart Images

Figure CN119054101A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of priority to U.S. Provisional Patent Application No. 63 / 363,556, filed on April 25, 2022, the entire contents of which are incorporated herein by reference. Background Art
[0003] Due to the low cost and high abundance of iron, iron-based batteries such as iron-air batteries, iron-nickel batteries and iron-manganese oxide batteries are promising candidates for long-term energy storage. Generally, the lowest-cost iron materials are those of low purity. This contradicts the general requirements of batteries, which generally require high-purity input materials to reduce efficiency losses and degradation caused by impurities (for example, impurities produced by catalyzing unwanted side reactions). That is, common impurities in low-cost iron materials such as silicon dioxide, calcium oxide, magnesium oxide, aluminum oxide, manganese oxide, titanium dioxide, etc. (collectively referred to as "gangue") can cause battery performance to decrease. Therefore, there is still a need for high-purity, low-cost iron materials that support the robust performance of iron-based batteries. Summary of the invention
[0004] The present disclosure relates to high purity iron materials and systems and methods for producing such high purity iron materials based on economically converting low cost iron raw materials. Generally, the production method using the system described herein may include acid leaching low purity iron ore to produce an iron-rich acid solution, which may be purified to remove residual soluble impurities and hydrolyzed to produce a high purity iron oxide powder. The high purity iron oxide powder may be reduced to form a high purity iron metal suitable for a variety of end uses including for batteries.
[0005] According to one aspect, the iron metal may have an apparent density of less than 3 g / cc and a silica content of less than 0.5 wt%.
[0006] According to another aspect, the iron oxide material can have a silica content of less than 0.5 wt%.
[0007] According to yet another aspect, a method of producing an iron-containing material may include directly reducing an iron oxide material having a silica content of less than 0.5 wt % to an iron material having an apparent density of less than 3 g / cc and a silica content of less than 0.5 wt %. In some embodiments, the iron oxide material may be a powder.
[0008] In certain embodiments, the method may further include hydrolyzing a solution of iron in an acidic leaching agent to form the iron oxide material. Hydrolyzing the solution to form the iron oxide material may include spray roasting the solution to form the iron oxide material. Further, or alternatively, hydrolyzing the solution to form the iron oxide material may include fluidized bed hydrolyzing the solution to form the iron oxide material. In some cases, hydrolyzing the solution may include adding steam. Further, or alternatively, hydrolyzing the solution may include adding water to the solution to maintain the concentration of the iron in the solution below the saturation level of iron in the acidic leaching agent.
[0009] In some embodiments, the method may further include dissolving the iron-containing material in the acidic leachant to form a solution of iron in the acidic leachant. In some cases, dissolving the iron-containing material in the acidic leachant may include recovering the acidic leachant separated from the iron in the solution of hydrolyzing the iron in the acidic leachant. Further, or alternatively, dissolving the iron-containing material may include heating the solution to at least 40°C. Additionally or alternatively, dissolving the iron-containing material may include directing energy into the solution, wherein the energy is one or more of ultrasound, mechanical microwave radiation, or UV light radiation. In some cases, the iron-containing material may be a granular raw material having an average particle size of 20 microns to 500 microns. Further, or alternatively, the acidic leachant may include hydrochloric acid. Additionally or alternatively, the iron-containing material may include one or more of iron ore, scrap metal, mining tailings, mineral processing tailings, waste battery electrodes, or waste batteries.
[0010] In certain embodiments, the method may further include removing at least a portion of one or more soluble impurities from the solution of the iron in the acidic leachate, wherein the solution of the iron in the acidic leachate is hydrolyzed and the one or more soluble impurities are removed from the solution. The soluble impurities may include one or more of silicon, aluminum, calcium, magnesium, chromium, titanium, manganese, vanadium, or copper.
[0011] In some embodiments, the method may include fabricating a component of a battery, wherein the component includes the ferrous material.
[0012] In certain embodiments, the method may include producing a steel comprising the ferrous material. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1is a block diagram of a system for producing high purity iron material from iron raw materials, the system including a leaching reactor, a purifier, a spray roaster and a post-processing station. DETAILED DESCRIPTION
[0014] Embodiments will be described in detail with reference to the accompanying drawings, in which exemplary embodiments are shown. However, the foregoing may be embodied in many different forms and should not be construed as being limited to the exemplary embodiments set forth herein. Unless the context otherwise dictates or clearly indicates, all material flows described herein may flow through channels (e.g., pipes and / or headers) or other forms of material transport.
[0015] The multiple embodiments of the systems, devices, technologies, methods, activities and operations set forth in this specification can be used in multiple other activities and other fields beyond those set forth herein. In addition, for example, these embodiments can be used together with other devices or activities that may be developed in the future, and can be used together with existing devices or activities that can be partially modified based on the teachings of this specification. In addition, the multiple embodiments and examples set forth in this specification can be used together with each other in whole or in part, and can be used in different and multiple combinations. Therefore, the configurations provided in the multiple embodiments of this specification can be used together with each other. For example, according to the teachings of the present disclosure, the components of the embodiments with A, A' and B and the components of the embodiments with A ", C and D can be used together with each other in multiple combinations, such as A, C, D and A, A ", C and D, etc.
[0016] As used herein, unless the context dictates otherwise or clearly indicated, the term "apparent density" shall be understood to refer to the mass of a powder per unit volume, usually expressed as grams per cubic centimeter, as determined by a specified method such as ASTM B212-17 and / or ASTM B417-13, the entire contents of each of these test standards being incorporated herein by reference.
[0017] Reference now Figure 1, the system 100 may include a leaching reactor 102, a purifier 104, a hydrolyzer 106, and a post-processing station 108. The system 100 can be used to scalably and economically convert low-cost iron raw materials into high-purity iron metal suitable for a variety of end uses, including for batteries. Therefore, in certain embodiments, the system 100 may additionally or alternatively include a battery manufacturing plant 110. As described in more detail below, the system 100 can be used to implement a production method including acid leaching low-purity iron ore to produce an iron-rich acid solution, which can be purified to remove residual soluble impurities, and additionally, or alternatively, the iron-rich acid solution can be hydrolyzed to produce a high-purity iron oxide powder. The high-purity iron oxide powder can be reduced to form a high-purity iron metal suitable for a variety of end uses, such as in batteries, ironmaking, and / or steelmaking. Compared to conventional processes for producing iron metal using melt processing operations (e.g., in a blast furnace, direct reduction in a shaft furnace combined with electric arc furnace smelting, etc.), the system 100 can be used to implement an iron metal production technique that facilitates achieving lower costs in obtaining high purity iron metal. In other words, the techniques described herein facilitate the production of high purity iron metal at a given cost. For example, the system 100 can be used to upgrade blast furnace iron ore to a quality level exceeding that of direct reduction (DR) grade ore without the need for additional mechanical crushing, magnetic separation, or flotation.
[0018] When used, as described in more detail below, the system 100 can remove impurities in the iron material to low levels by using liquid phase purification, which is low cost, scalable, and a key requirement for end-uses such as battery manufacturing for multi-day energy storage. As an example, the system 100 can implement the following general process steps to produce high-purity iron metal with low apparent density: 1) Produce an iron-rich solution; 2) Remove soluble impurities; 3) Hydrolysis to produce iron oxide powder; and 4) Post-processing and end-use. The following sections describe each of these steps.
[0019] 1. Produce iron-rich solution
[0020] Iron material (e.g., natural ore and other forms such as oxides, hydroxides, metalliferous, metalliferous and / or sulfides) may be beneficiated (sorted) to form an iron material feedstock of a predetermined particle size (e.g., an average particle size of 20 microns to 500 microns).
[0021] The iron material feedstock may be fed into a leaching reactor 102, where the iron material feedstock may be combined with an acidic leaching agent (e.g., a solvent such as hydrochloric acid (HCl)) to produce an iron-rich solution. Advantageously, compared to other iron ore purification processes, many impurity phases such as silicon dioxide (e.g., SiO2, primarily in the form of quartz, aluminosilicates (kaolin)) are insoluble in acid, so acid dissolution (leaching) performed in the leaching reactor 102 easily separates iron and impurities. Further, or alternatively, relatively impure (e.g., high gangue content) iron material feedstock may be effectively upgraded from the leaching reactor 102 to a higher purity output.
[0022] The concentration of the acidic leachant fed into the leaching reactor 102 may be 1 mol / L (M) to 15 mol / L (M), and the iron concentration of the iron-rich solution produced by the leaching reactor 102 may be 0.01 M to 10 M. The acidic leachant regenerated by the hydrolyzer 106 may be fed back into the leaching reactor 102. Additionally or alternatively, the replenishment amount of the replenishment acidic leachant (referred to herein as "replenishment acidic leachant") offsets the material loss in the closed-loop process. In certain embodiments, the acidic leachant regenerated from the hydrolyzer 106 is not fed back into the leaching reactor 102, and only new acidic leachant is provided to the leaching reactor 102. Increasing the ionic strength of ions (e.g., chloride ions) in the acidic leachant - for example, using a combination of an acid (e.g., hydrochloric acid) and other leachants (e.g., other chloride leachants) - can increase the dissolution of the iron material feedstock in the iron-rich solution.
[0023] Although the iron-rich solution may be formed in the leaching reactor 102, the iron-rich solution may additionally or alternatively be provided directly by another chemical process. For example, byproducts of titanium refining (ilmenite processing), such as iron chloride and / or iron sulfate, may be provided directly to the purifier 104 and used in the remaining steps of the process implemented by the system 100. More generally, the system 100 may be flexible to use a variety of iron material feedstocks, and the system 100 may further or alternatively include the ability to switch between acid leaching iron ore and other iron feedstocks.
[0024] In certain embodiments, the iron material raw material fed into the leaching reactor 102 may additionally or alternatively include scrap metal. For example, the iron material raw material fed into the leaching reactor 102 may include waste battery electrodes or discarded battery electrodes and / or discarded batteries as a source of iron. Further, or alternatively, the iron material raw material may include discarded electronic waste as a source of iron. Additionally or alternatively, the iron material raw material fed into the leaching reactor 102 may include mining tailings (e.g., red mud, pyrite ore from base metal processing, jarosite and goethite residues from zinc extraction processes, etc.) in addition to iron ore, or may include mining tailings (e.g., red mud, pyrite ore from base metal processing, jarosite and goethite residues from zinc extraction processes, etc.) instead of iron ore.
[0025] In some embodiments, acid leaching in the leaching reactor 102 can be accelerated by adding energy to the leaching reactor 102. For example, acid leaching in the leaching reactor 102 can be accelerated by adding heat (e.g., heating the acid solution to at least 40° C.), pressure (e.g., high pressure treatment at above one atmosphere), sound (ultrasound), mechanical agitation (stirring), microwave irradiation, UV light irradiation, or a combination thereof. Additionally or alternatively, acid leaching in the leaching reactor 102 can be accelerated by adding an oxidant such as oxygen (O2), chlorine (Cl2) and / or hydrogen peroxide (H2O2). This may be particularly useful for acid leaching in the case where the iron material feedstock includes high levels of sulfur and / or organic matter. In some cases, further, or alternatively, refractory iron ores that are difficult to dissolve (e.g., pyrite ores, high sulfide ores, high carbonaceous iron ores, etc.) can be subjected to an electrochemical oxidation process. That is, the refractory iron ore may be coupled to a conductive electrode maintained at an oxidizing (anodic) potential, and a counter electrode may be maintained at a lower oxidizing (more cathodic) potential to accelerate the leaching rate.
[0026] In some cases, multiple acids may be used to increase the dissolution (leaching) rate of the iron material feedstock in the leaching reactor 102. For example, hydrochloric acid and oxalic acid may be used together to increase the rate at which iron dissolves into the iron-rich solution produced by the leaching reactor 102.
[0027] 2. Remove soluble impurities
[0028] In the iron-rich solution (also referred to as the pregnenous leaching solution (PLS)) produced by the leaching reactor 102, additional soluble impurities (e.g., silicon, aluminum, calcium, magnesium, chromium, titanium, manganese, vanadium, copper, etc.) may remain in the solution phase. Therefore, in some cases, the iron-rich solution from the leaching reactor 102 may be fed to a purifier 104 to remove the soluble impurities in the iron-rich solution to produce a purified iron-rich solution. As used in this context, the purified iron-rich solution discharged from the purifier 104 is understood to differ from the iron-rich solution fed to the purifier 104 in that the purified iron-rich solution has a lower volume concentration of at least one soluble impurity in the iron-rich solution.
[0029] For example, in the purifier 104, the soluble impurities in the iron-rich solution from the leaching reactor 102 may be removed using one or more of the following: selective adsorption (e.g., ion exchange and activated carbon adsorption); solvent extraction (e.g., using a solvating extractant, a cation exchange extractant, a chelating extractant, and / or an anion exchange extractant); chemical oxidation (e.g., adding H2O2, O2, and / or Cl2); adding alkaline chemicals (e.g., sodium carbonate, sodium hydroxide, and / or a combination of alkaline solutions) to increase pH and selectively precipitate impurities; adding a sulfide source to precipitate impurities; electrochemical oxidation; or heating and / or cooling to achieve a precipitation (crystallization) reaction. Further, or alternatively, sulfide ions (e.g., sodium sulfide and / or hydrogen sulfide gas) may be added to selectively precipitate impurities in the form of metal sulfides. In some embodiments, removing soluble impurities from the iron-rich solution in purifier 104 can include cementation in which metallic iron, scrap iron, and / or scrap steel are added to the iron-rich solution to reduce ferric chloride III to ferric chloride II and precipitate elements more noble than iron (e.g., elements such as copper and nickel). Further, or alternatively, in purifier 104, adding scrap metal to the iron-rich solution can facilitate increasing the pH of the iron-rich solution and, when combined with pH adjustment, can facilitate precipitation and removal of dissolved silica, titanium, aluminum, chromium, and / or copper impurities from the iron-rich solution when the pH of the iron-rich solution is about 4 to 6.5. In the case where removing dissolved impurities from the iron-rich solution in purifier 104 includes cooling and / or heating (crystallization), the iron-rich solution can be heated to evaporate excess water, and the resulting iron chloride-saturated solution can be placed into a crystallizer in which ferric chloride II crystals can be formed.
[0030] In some embodiments, the purification process implemented in the purifier 104 may be a single unit operation, while in other embodiments, the purification process implemented in the purifier 104 may include multiple unit operations. Various aspects of the purification process implemented in the purifier 104 may be greatly affected by the composition and mineralogy of the iron material feedstock, and further, or alternatively, various aspects of the purification process implemented in the purifier 104 may be adjusted to adjust the quality of the high purity iron oxide material output. Additionally, or alternatively, because the composition of the iron material feedstock changes over time, the purification process implemented in the purifier 104 may be adjusted to facilitate the stable production of the output high purity iron oxide material.
[0031] 3. Hydrolysis to produce iron oxide powder
[0032] Typically, the purified iron-rich solution from the purifier 104 may be subjected to iron chloride decomposition and acid regeneration. For example, the purified iron-rich solution may be subjected to a spray roasting process in the spray roaster 106. Additionally or alternatively, the iron chloride decomposition and acid regeneration may be performed in a fluidized bed reactor.
[0033] In some embodiments, the hydrolysis reaction in the hydrolyzer 106 can include mixing the purified iron-rich solution with air (e.g., at a high temperature greater than 150°C, such as greater than about 500°C and less than about 800°C). In some cases, additional water (steam) can be added to promote rapid hydrolysis. For example, water can be added to the purified iron-rich solution to keep the iron concentration in the solution below saturation levels. Further, or alternatively, additional oxygen (O2) can be added to the purified iron-rich solution in the hydrolyzer 106. Further, or alternatively, in the case where high-temperature hydrolysis such as spray roasting is used to hydrolyze the purified iron-rich solution in the hydrolyzer 106, the exhaust gas can be rich in HCl-water vapor mixture, and, for example, the HCl-water vapor mixture can be absorbed into a packed bed absorber, where water can be used to remove (wash out) the absorbed HCl to produce regenerated hydrochloric acid that can be returned to the leaching reactor 102. In cases where the hydrolysis in hydrolyzer 106 includes spray roasting, the iron oxides produced by the spray roasting may be rinsed or washed, which may be useful to adjust the chemistry of the iron oxides.
[0034] 4. Post-processing and final use
[0035] While in some cases, the iron oxide produced by the hydrolyzer 106 can be used directly in an end-use application (e.g., directly in a battery manufacturing plant 110 - skipping the post-processing station 108 - for manufacturing a battery in which a negative electrode is formed in a discharged state), the iron oxide can undergo one or more post-processing steps in the post-processing station 108 to make the iron oxide into an iron-containing material suitable for a particular end-use, or in some cases more suitable for a particular end-use. As used in this context, the iron-containing material formed by one or more post-processing operations performed in the post-processing station 108 can include changing one or more chemical properties and / or physical properties of the iron oxide fed from the hydrolyzer 106 to the post-processing station 108. For example, in the post-processing station 108, the iron oxide from the hydrolyzer 106 can be blended with other iron-containing materials and then incorporated into a battery in the battery manufacturing plant 110. Further, or alternatively, in the post-processing station 108, the iron oxide from the hydrolyzer 106 can be reduced to iron metal and then used in a battery in the battery manufacturing plant 110. Additionally, or alternatively, the iron oxide from the hydrolyzer 106 can be partially reduced to an intermediate oxidation state between iron oxide and iron metal and then used in a battery in which a negative electrode is formed at an intermediate state of charge in a battery manufacturing plant 110. In some cases, the partially reduced material produced from the iron oxide can be blended with other iron-containing materials such that the combination of the iron oxide and the other iron-containing materials is incorporated into a battery at the battery manufacturing plant 110.
[0036] In certain embodiments, the iron oxides from the hydrolyzer 106 may be used directly as feedstock for a “fines-based” direct reduction process performed in the post-processing station 108 .
[0037] In some cases, in the post-processing station 108, the iron oxides from the hydrolyzer 106 can be agglomerated into iron oxide pellets by adding a binder such as bentonite or sodium alginate or other organic binders such as carboxymethyl cellulose, followed by granulation or pelletization according to methods known in the art such as disk granulation or drum granulation. In some cases, the resulting pellets can be used as input to a direct reduction process such as a shaft furnace process or a fluidized bed process implemented in the post-processing station 108. Further, or alternatively, the reducing gas for the direct reduction process implemented in the post-processing station 108 can include natural gas (methane), reformed natural gas, hydrogen (including but not limited to hydrogen obtained by methane steam reforming, in-situ reforming, methane pyrolysis, water electrolysis, and / or other methods).
[0038] In certain embodiments, the iron oxides from the hydrolyzer 106 may be directly reduced by a coal-based process or a coking coal-based process implemented in the post-processing station 108. In some embodiments, the iron oxides from the hydrolyzer 106 may be directly reduced in a rotary kiln or a tunnel kiln of the post-processing station 108. Further, or alternatively, the high-purity iron directly reduced by the iron oxides in the post-processing station 108 may be advantageously used in steelmaking. That is, the high-purity iron directly reduced by the iron oxides in the post-processing station 108 may contain a small amount of SiO2, CaO, MgO, MnO, Al2O3, etc., and thus may be advantageous in generating less slag in the steelmaking process. In some cases, the high-purity iron directly reduced by the iron oxides in the post-processing station 108 may be used in a blast furnace, an electric arc furnace, or other steelmaking operations.
[0039] In some cases, the high purity iron directly reduced by the iron oxide in the post-processing station 108 can be used in batteries such as iron-air batteries, iron-nickel batteries, or iron-manganese oxide batteries. For example, the high purity iron directly reduced in the post-processing station 108 can be prepared into battery electrodes by a variety of methods known in the art, such as sintering, coating and drying, or by incorporating pocket plate electrodes. Additionally or alternatively, the high purity iron directly reduced by the iron oxide in the post-processing station 108 can be formed into battery electrodes by a hot press forming process, such as the hot press forming process described in U.S. Patent Application Publication No. 2022 / 0149359A1, entitled “METHOD OF IRON ELECTRODE MANUFACTURE AND ARTICLES AND SYSTEMS THEREFROM” published on May 12, 2022 (the entire contents of which are incorporated herein by reference). U.S. patent application publication 2022 / 0149359A1 also describes multiple embodiments and provides specific examples of aspects of electrochemical cells, such as rechargeable battery packs using iron electrodes (e.g., iron negative electrodes), and design, manufacturing, and processing features of electrochemical cells, such as methods for manufacturing iron electrodes that can be at least partially made using high-purity iron that is directly reduced from the iron oxide in a post-processing station 108.
[0040] Although the foregoing description focuses on hydrochloric acid, it should be understood that this is for the sake of clarity and effective description. Unless otherwise specified or clearly stated in the context, the acidic leaching agent may include any one or more of a variety of acids and combinations thereof, including hydrochloric acid (HCl), sulfuric acid (H2SO4), nitric acid (HNO3), hydrofluoric acid (HF), oxalic acid (C2H2O4) and combinations and arrangements thereof.
[0041] The above method description and process flow chart are provided only as illustrative examples, and are not intended to require or imply that the steps of multiple embodiments should be performed in the order shown. As will be appreciated by those skilled in the art, the order of steps in the above embodiments can be performed in any order. Words such as "thereafter", "then", "next", etc. are not intended to limit the order of steps, and these words are only used to guide the reader to understand the description of the method. In addition, any reference to a claim element in the singular form, such as the use of the article "a", "an" or "the", should not be interpreted as limiting the element to the singular form. In this article, "about" can refer to a range of + / -5%.
[0042] In addition, any step of any embodiment described herein can be used in any other embodiment. The above description of the disclosed embodiment is provided to enable those skilled in the art to make or use the claims. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be applied to other embodiments without departing from the scope of the claims. Therefore, the present disclosure is not intended to be limited to the embodiments shown herein, but should be given the widest scope consistent with the following claims and the principles and new features disclosed herein.
Claims
1. A ferrous metal having an apparent density of less than 3 g / cc and a silica content of less than 0.5 wt. %.
2. An iron oxide material having a silicon dioxide content of less than 0.5 wt. %.
3. A method for producing an iron-containing material, the method comprising: An iron oxide material having a silica content of less than 0.5 wt % is directly reduced to an iron material having an apparent density of less than 3 g / cc and a silica content of less than 0.5 wt %.
4. The method of claim 3, wherein the iron oxide material is a powder.
5. The method of claim 3, further comprising hydrolyzing a solution of iron in an acidic leaching agent to form the iron oxide material.
6. The method of claim 5, wherein hydrolyzing the solution to form the iron oxide material comprises spray calcining the solution to form the iron oxide material.
7. The method of claim 5, wherein hydrolyzing the solution to form the iron oxide material comprises fluidized bed hydrolyzing the solution to form the iron oxide material.
8. The method of claim 5, wherein hydrolyzing the solution comprises adding steam.
9. The method of claim 5, wherein hydrolyzing the solution comprises adding water to the solution to maintain the concentration of the iron in the solution below a saturation level of iron in the acidic leaching agent.
10. The method of claim 5, further comprising dissolving an iron-containing material in the acidic leachant to form a solution of iron in the acidic leachant.
11. The method of claim 10, wherein dissolving the iron-containing material in the acidic leachant comprises recovering the acidic leachant separated from the iron in a solution that hydrolyzes the iron in the acidic leachant.
12. The method of claim 10, wherein dissolving the iron-containing material comprises heating the solution to at least 40°C.
13. The method of claim 10, wherein dissolving the iron-containing material comprises directing energy into the solution, wherein the energy is one or more of ultrasound, mechanical microwave radiation, or UV light radiation.
14. The method of claim 10, wherein the iron-containing material is a particulate feedstock having an average particle size of 20 microns to 500 microns.
15. The method of claim 10, wherein the acidic leaching agent comprises hydrochloric acid.
16. The method of claim 10, wherein the iron-containing material comprises one or more of iron ore, scrap metal, mining tailings, beneficiation tailings, spent battery electrodes, or spent batteries.
17. The method of claim 10, further comprising removing at least a portion of one or more soluble impurities from the solution of the iron in the acidic leachate, wherein the solution of the iron in the acidic leachate is hydrolyzed and the one or more soluble impurities are removed from the solution.
18. The method of claim 17, wherein the soluble impurities include one or more of silicon, aluminum, calcium, magnesium, chromium, titanium, manganese, vanadium, or copper.
19. The method of claim 5, further comprising manufacturing a component of a battery pack, wherein the component includes the ferrous material.
20. The method of claim 5, further comprising manufacturing a steel comprising the ferrous material.