Ammonia separation membrane filled with pores with double functional sites and preparation method of ammonia separation membrane
By introducing Lewis acid groups and transition metal ions into the ammonia separation membrane, combined with high mechanical properties of membrane materials, the problems of poor performance and insufficient strength of the existing ammonia separation membrane are solved, and efficient ammonia separation is achieved and industrial Application potential.
Patent Information
- Application Number
- CN202411177853.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The selected separation performance and poor mechanical strength of existing ammonia separation membranes limit their use in industrial applications.
The ammonia separation membrane is used to fill the ammonia separation membrane with a dual-functional site pore-filled ammonia separation membrane. By introducing Lewis acid groups and transition metal ions into the membrane, it promotes rapid transmission of ammonia, improves separation performance, and uses materials such as PVDF or PTFE to improve mechanical strength.
High selectivity and high throughput ammonia separation, significantly improved ammonia/nitrogen and ammonia/hydrogen selectivity, and tensile strength exceeds 60MPa, making it suitable for industrial applications.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of new chemical materials, and in particular to an ammonia separation membrane with dual-functional site pore filling and a preparation method thereof. Background Art
[0002] Ammonia plays an extremely important role in the industrial field. It is not only a key raw material for the production of agricultural fertilizers, but also widely used in the synthesis of pharmaceuticals, organic compounds and polymer materials. As a hydrogen source, ammonia also has important applications in the field of hydrogen energy. In addition, ammonia is one of the chemicals with the largest output and the widest application in the global chemical industry. Its core role in many fields such as agriculture, energy and chemical industry has established ammonia's irreplaceable position in the global economic and technological development. The Haber-Bosch process is the most mature and widely used ammonia production method. Its basic principle is to generate ammonia (NH3) through the chemical reaction of nitrogen (N2) and hydrogen (H2) under high temperature and high pressure conditions. Despite this, it also has some significant disadvantages. In particular, since ammonia synthesis is an exothermic reaction, the equilibrium constant of the reaction is low at high temperature, which limits the conversion rate of ammonia. Generally, the ammonia synthesis conversion rate of the Haber-Bosch process is only 10-20%, and about 3% of the ammonia will remain in the circulating gas, greatly increasing the energy consumption of ammonia synthesis. Therefore, it is extremely important to develop efficient technology to recover the residual ammonia.
[0003] Ammonia separation technology is crucial in industrial production, and commonly used methods include liquid absorption and solid adsorption. Liquid absorption is a technology that achieves ammonia separation by utilizing the difference in solubility of ammonia in liquid solvents. This method usually utilizes the high solubility of ammonia in water, acidic solutions or other specific solvents to separate ammonia from a gas mixture. Solid adsorption is a technology that separates ammonia from a mixed gas by physically or chemically adsorbing ammonia through porous solid materials (such as activated carbon, zeolite or metal organic framework materials). It is worth noting that both liquid absorption and solid adsorption require regeneration of the adsorbent, and the process involves ammonia phase change, resulting in high energy consumption and difficulty in achieving continuous operation. Membrane separation technology has gradually attracted attention in the field of ammonia separation. Compared with traditional separation methods such as liquid absorption and solid adsorption, membrane separation technology relies on the difference in the transfer rate of ammonia and other gas components in the membrane material to achieve separation, and does not involve gas-liquid or gas-solid phase change processes. Therefore, the energy consumption is low. At the same time, membrane separation does not require the use of chemical solvents, and there are no problems with solvent regeneration, treatment and discharge. More importantly, membrane separation is suitable for continuous production and can achieve uninterrupted ammonia separation operation, greatly improving production efficiency. Compared with adsorption separation that requires periodic regeneration, the continuity of membrane separation significantly reduces operational complexity and downtime. However, the ammonia separation membrane in the prior art has poor selective separation performance and poor mechanical strength, which seriously affects its industrial application. Summary of the invention
[0004] In view of the problems of poor ammonia selective separation performance and poor mechanical strength of ammonia separation membranes in the prior art, the present invention provides an ammonia separation membrane with dual-functional site pore filling and a preparation method thereof. The prepared ammonia separation membrane has Lewis acid groups and transition metal ions, which can promote the preferential and rapid transmission of ammonia through their high affinity for ammonia, thereby giving the prepared pore filling membrane high ammonia selective permeability separation performance, thereby achieving high selectivity and high flux separation of ammonia.
[0005] The present invention adopts the following technical solution:
[0006] A method for preparing ammonia separation membrane with dual-functional site pore filling, comprising the following steps:
[0007] S1, quaternizing a small N-heterocyclic molecule with a vinyl group with a functionalized alkane to obtain a quaternized product;
[0008] S2, dissolving the quaternized product, the crosslinking agent and the initiator together in a polar solvent to form a functional solution A;
[0009] S3, soaking the PTFE or PVDF porous base membrane in the functional solution A, taking it out after the membrane pores of the porous base membrane are fully infiltrated by the functional solution A, removing the residual liquid on the surface, and then thermally polymerizing it at 80-120° C. for 1-12 hours to obtain a thermally polymerized membrane;
[0010] S4. Immerse the polymer membrane in a functional solution B containing metal chloride to carry out a chelating reaction, take it out, wash it, and dry it to obtain the final pore-filled ammonia separation membrane with dual functional sites.
[0011] In the step S1, the N-heterocyclic small molecule with a vinyl group is one of vinyl imidazole, 4-methyl-5-vinylthiazole, 4-vinylpyridine, and N-vinylcarbazole.
[0012] The general chemical formula of the functionalized alkane in step S1 is X(CH2): n R, wherein X represents Cl or Br, and R represents a Lewis acid group, which is -OH, -NH3 + Cl - , -COOH, n=3-6.
[0013] In the step S2, the mass ratio of the quaternized product, the crosslinking agent and the initiator is 1:(0.04-0.2):(0.01-0.08).
[0014] The cross-linking agent in step S2 is a small molecule containing at least two double bonds, which can be selected from divinylbenzene, butadiene, N,N′-methylenebisacrylamide and tripropylene glycol diacrylate.
[0015] In the step S2, the initiator is one of azobisisobutyronitrile, azobisisoheptanenitrile, dibenzoyl peroxide, potassium persulfate and ammonium persulfate.
[0016] The polar solvent in step S2 is one of ethanol, ether, chloroform, benzene and acetone.
[0017] The mass concentration of the functional solution A in step S2 is 20%-60%.
[0018] The mass concentration of the functional solution B in step S4 is 1%-20%, wherein the solute is one of CoCl2, NiCl2, SnCl2, CuCl2, MnCl2 and FeCl2, and the solvent is one of ethanol, acetone and ether.
[0019] The temperature of the chelating reaction in step S4 is 30-80° C. and the time is 4-48 hours.
[0020] An ammonia separation membrane with dual-functional site pore filling prepared according to the preparation method.
[0021] The technical solution of the present invention has the following advantages:
[0022] A. The pore-filled ammonia separation membrane with dual functional sites prepared by the present invention has two active sites, one of which is -OH and the other is -NH3 + Cl - The first is a Lewis acid site such as -COOH, and the second is a chelated transition metal ion site. Both of these active sites have good ammonia affinity and can synergistically promote high selectivity and high-throughput separation of ammonia.
[0023] B. The pore-filled ammonia separation membrane with dual functional sites obtained by the present invention uses a membrane with excellent mechanical properties such as PVDF or PTFE as a substrate, which effectively improves the film strength and meets the actual application requirements.
[0024] C. The pore-filled ammonia separation membrane with dual functional sites obtained by the present invention has a high-efficiency ammonia separation effect. When separating the residual gas of synthetic ammonia, the ammonia permeability is as high as 2401.5 Barrer, the ammonia / nitrogen and ammonia / hydrogen selectivities are as high as 515.2 and 138.7 respectively, and the tensile strength is greater than 60 MPa, which has good potential for industrial application. DETAILED DESCRIPTION
[0025] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Embodiment 1:
[0027] Add vinyl imidazole (0.05 mol, 4.81 g) and 3-chloropropionic acid (0.075 mol, 8.22 g) into a flask, and then add 100 mL of acetonitrile. Under the protection of inert gas Ar, heat to 80 ° C and stir to react for 30 hours. After the reaction is completed, wash the resulting mixture 5 times with ethyl acetate to remove unreacted raw materials. Finally, place the washed product in a vacuum drying oven at 40 ° C for 24 hours to obtain a quaternized product containing a -COOH group.
[0028] The quaternized product, divinylbenzene and azobisisobutyronitrile were dissolved in ethanol at a mass ratio of 1:0.04:0.01 to form a functional solution A with a mass concentration of 20%. The PVDF porous base membrane was immersed in the functional solution A for 12 hours, taken out, and the surface solution was removed. Then, the polymerization reaction was carried out at 80°C for 24 hours. Finally, the polymerized membrane was immersed in a CoCl2 / ethanol solution with a mass concentration of 1% for a chelating reaction and immersed at 80°C for 4 hours to obtain the final pore-filled ammonia separation membrane with dual functional sites.
[0029] The tensile strength of the membrane was measured to be 63 MPa. Furthermore, a gas separation device was used to separate a mixed gas containing ammonia, nitrogen and hydrogen, and the permeability of the three was tested and the ammonia / nitrogen and ammonia / hydrogen selectivities were calculated. The results showed that the pure ammonia permeability of the membrane was 2895.2 Barrer, and the ammonia / nitrogen and ammonia / hydrogen selectivities were 138.4 and 48.9, respectively.
[0030] Embodiment 2:
[0031] The membrane was prepared by a method similar to that of Example 1, except that the mass ratio of the quaternized product, divinylbenzene and azobisisobutyronitrile was changed to 1:0.06:0.03.
[0032] The tensile strength of the membrane was measured to be 66 MPa. Furthermore, a gas separation device was used to separate a mixed gas containing ammonia, nitrogen and hydrogen, and the permeability of the three gases was tested and the ammonia / nitrogen and ammonia / hydrogen selectivities were calculated. The results showed that the pure ammonia permeability of the membrane was as high as 2401.5 Barrer, and the ammonia / nitrogen and ammonia / hydrogen selectivities were as high as 515.2 and 138.7, respectively.
[0033] Embodiment 3:
[0034] The membrane was prepared by a method similar to that of Example 1, except that the mass ratio of the quaternized product, divinylbenzene and azobisisobutyronitrile was changed to 1:0.2:0.08.
[0035] The tensile strength of the membrane was measured to be 72 MPa. Furthermore, a gas separation device was used to separate a mixed gas containing ammonia, nitrogen and hydrogen, and the permeability of the three gases was tested and the ammonia / nitrogen and ammonia / hydrogen selectivities were calculated. The results showed that the pure ammonia permeability of the membrane was as high as 1407.4 Barrer, and the ammonia / nitrogen and ammonia / hydrogen selectivities were as high as 624.2 and 179.6, respectively.
[0036] Combining Examples 1-3, it can be seen that the increase in the cross-linking agent content leads to a decrease in the ammonia permeability of the membrane and an increase in the selectivity, and vice versa. From the experimental results, the best effect is achieved when the mass of the cross-linking agent is 6% of the mass of the quaternary ammonium product.
[0037] Embodiment 4:
[0038] Add vinyl imidazole (0.05 mol, 4.81 g) and 3-chloropropylamine hydrochloride (0.06 mol, 7.96 g) into a flask, and then add 50 mL of N,N-dimethylformamide. Under the protection of inert gas Ar, heat to 70 ° C and stir to react for 48 hours. After the reaction is completed, wash the resulting mixture 5 times with ethyl acetate to remove unreacted raw materials. Finally, place the washed product in a vacuum drying oven at 40 ° C and dry it for 24 hours to obtain -NH3 + Cl- Quaternization product of the group.
[0039] The quaternized product, butadiene, and azobisisoheptonitrile were dissolved in ether at a mass ratio of 1:0.06:0.03 to form a functional solution A with a mass concentration of 40%. The PTFE porous base membrane was immersed in the functional solution A for 12 hours, taken out, and the surface solution was removed. Then, the polymerization reaction was carried out at 120°C for 1 hour. Finally, the polymerized membrane was immersed in a NiCl2 / acetone solution with a mass concentration of 20% for chelation reaction, and immersed at 30°C for 48 hours to obtain the final pore-filled ammonia separation membrane with dual functional sites.
[0040] The tensile strength of the membrane was measured to be 63 MPa. Furthermore, a gas separation device was used to separate a mixed gas containing ammonia, nitrogen and hydrogen, and the permeability of the three gases was tested and the ammonia / nitrogen and ammonia / hydrogen selectivities were calculated. The results showed that the pure ammonia permeability of the membrane was 2048.3 Barrer, and the ammonia / nitrogen and ammonia / hydrogen selectivities were 404.3 and 88.2, respectively.
[0041] Embodiment 5:
[0042] Add vinyl imidazole (0.05 mol, 4.81 g) and 6-bromo-1-hexanol (0.06 mol, 10.86 g) into a flask, and then add 50 mL of N,N-dimethylformamide. Under the protection of inert gas Ar, heat to 70 ° C and stir to react for 48 hours. After the reaction is completed, wash the resulting mixture 5 times with ethyl acetate to remove unreacted raw materials. Finally, place the washed product in a vacuum drying oven at 40 ° C for 24 hours to obtain -NH3 + Cl - Quaternization product of the group.
[0043] The quaternized product, N,N′-methylenebisacrylamide, and dibenzoyl peroxide were dissolved in chloroform at a mass ratio of 1:0.06:0.03 to form a functional solution A with a mass concentration of 60%. The PTFE porous base membrane was immersed in the functional solution A for 12 hours, taken out, and the surface solution was removed. Then, the polymerization reaction was carried out at 120°C for 1 hour. Finally, the polymerized membrane was immersed in a SnCl2 / ether solution with a mass concentration of 20% for chelation reaction and immersed at 30°C for 48 hours to obtain the final pore-filled ammonia separation membrane with dual functional sites.
[0044] The tensile strength of the membrane was measured to be 63 MPa. Furthermore, a gas separation device was used to separate a mixed gas containing ammonia, nitrogen and hydrogen, and the permeability of the three gases was tested and the ammonia / nitrogen and ammonia / hydrogen selectivities were calculated. The results showed that the pure ammonia permeability of the membrane was 2002.5 Barrer, and the ammonia / nitrogen and ammonia / hydrogen selectivities were 385.3 and 87.9, respectively.
[0045] Embodiment 6:
[0046] A membrane was prepared by a method similar to that of Example 2, except that the vinyl-containing N-heterocyclic molecule was replaced with 4-methyl-5-vinylthiazole, the cross-linking agent was changed to tripropylene glycol diacrylate, the initiator was changed to potassium persulfate, the solvent of functional solution A was changed to benzene, and the solute of functional solution B was changed to CuCl2. The resulting membrane had similar performance to that of Example 2.
[0047] Embodiment 7:
[0048] The membrane was prepared by a method similar to that of Example 2, except that the solute of functional solution B was changed to FeCl2, and the resulting membrane had performance similar to that of Example 2.
[0049] In summary, the pore-filled ammonia separation membrane with dual functional sites prepared by the present invention has two active sites, one of which is -OH and the other is -NH3 + Cl - The first is a Lewis acid site such as -COOH, and the second is a chelated transition metal ion site. Both of these active sites have good ammonia affinity and can synergistically promote high selectivity and high-throughput separation of ammonia.
[0050] The pore-filled ammonia separation membrane with dual functional sites obtained by the present invention adopts a membrane with excellent mechanical properties such as PVDF or PTFE as a substrate, which effectively improves the film strength and meets the actual application requirements.
[0051] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. However, the obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.
Claims
1. A method for preparing ammonia separation membrane with dual-functional site pore filling, characterized in that: The following steps are involved: S1, quaternizing a small N-heterocyclic molecule with a vinyl group with a functionalized alkane to obtain a quaternized product; S2, dissolving the quaternized product, the crosslinking agent and the initiator together in a polar solvent to form a functional solution A; S3, soaking the PTFE or PVDF porous base membrane in the functional solution A, taking it out after the membrane pores of the porous base membrane are fully infiltrated by the functional solution A, removing the residual liquid on the surface, and then thermally polymerizing it at 80-120° C. for 1-12 hours to obtain a thermally polymerized membrane; S4, immersing the polymer membrane in a functional solution B containing metal chloride to carry out a chelating reaction, taking it out, washing it, and drying it to obtain a final pore-filled ammonia separation membrane with dual functional sites.
2. The preparation method according to claim 1, characterized in that: The N-heterocyclic small molecule with a vinyl group in step S1 is one of vinyl imidazole, 4-methyl-5-vinylthiazole, 4-vinylpyridine, and N-vinylcarbazole; The general chemical formula of the functionalized alkane in step S1 is X(CH2): n R, wherein X represents Cl or Br, and R represents a Lewis acid group, which is -OH, -NH3 + Cl - , -COOH, n=3-6.
3. The preparation method according to claim 1, characterized in that: In the step S2, the mass ratio of the quaternized product, the crosslinking agent and the initiator is 1:(0.04-0.2):(0.01-0.08).
4. The preparation method according to claim 1, characterized in that: The cross-linking agent in step S2 is a small molecule containing at least two double bonds, which can be selected from divinylbenzene, butadiene, N,N′-methylenebisacrylamide and tripropylene glycol diacrylate.
5. The preparation method according to claim 1, characterized in that: In the step S2, the initiator is one of azobisisobutyronitrile, azobisisoheptanenitrile, dibenzoyl peroxide, potassium persulfate and ammonium persulfate.
6. The preparation method according to claim 1, characterized in that: The polar solvent in step S2 is one of ethanol, ether, chloroform, benzene and acetone.
7. The preparation method according to claim 1, characterized in that: The mass concentration of the functional solution A in step S2 is 20%-60%.
8. The preparation method according to claim 1, characterized in that: The mass concentration of the functional solution B in step S4 is 1%-20%, wherein the solute is one of CoCl2, NiCl2, SnCl2, CuCl2, MnCl2 and FeCl2, and the solvent is one of ethanol, acetone and ether.
9. The preparation method according to claim 1, characterized in that: The temperature of the chelating reaction in step S4 is 30-80° C. and the time is 4-48 hours.
10. An ammonia separation membrane having dual-functional site pore filling obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of composite separating film filled by interpenetrating polymer network hydrogel
CN105289316A
Difunctional polymer-based ammonia gas adsorbent and preparation method thereof
CN117732444A
Membrane gas separation processes
EP0099868A1
Method for producing substance-selective separating membranes and their use
EP3290101A1
Cited By
Ammonia-hydrogen separation membrane based on self-contained microporous polymer and preparation method of ammonia-hydrogen separation membrane
CN119565408A
An ammonia-hydrogen separation membrane based on a self-microporous polymer and a preparation method thereof
CN119565408B
Brominated self-microporous polymer ammonia-hydrogen separation membrane and preparation method thereof
CN119565409A
Brominated self-microporous polymer ammonia-hydrogen separation membrane and preparation method thereof
CN119565409B
MOFs composite membrane for ammonia separation and preparation method thereof
CN119588188A