Electrode catalyst layer, membrane electrode assembly, and solid polymer fuel cell

By introducing nitrogen-containing fibrous materials into the electrode catalyst layer, optimizing the pore structure and polymer electrolyte distribution, the problems of insufficient proton conductivity and durability were solved, and high-performance operation of fuel cells was achieved over a wide current density range.

CN119054116APending Publication Date: 2024-11-29TOPPAN HOLDINGS INC
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202380034665.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-15
Filing Date
2023-04-17
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The electrode catalyst layers of existing solid polymer fuel cells have shortcomings in terms of proton conductivity and durability. In particular, the proton conduction resistance increases under low humidification conditions, which affects power generation performance and durability.

Method used

By introducing fibrous materials containing nitrogen atoms into the electrode catalyst layer, and by adjusting the fiber diameter and content, the distribution of polymer electrolytes is optimized, and an appropriate void structure is formed to improve proton conductivity and gas diffusion, thereby enhancing the bonding strength of the catalyst layer.

Benefits of technology

It achieves high power generation performance and good durability in the range of low to high current density, thus improving the overall performance of fuel cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119054116A_ABST
    Figure CN119054116A_ABST
Patent Text Reader

Abstract

An electrode catalyst layer (10) for use in a solid polymer fuel cell, the electrode catalyst layer comprising a catalyst substance (12), a conductive carrier (13) supporting the catalyst substance (12), a polymer electrolyte (14), and a fibrous substance (15) containing nitrogen atoms, the ratio of the number of atoms of nitrogen to the total number of atoms of carbon, nitrogen, oxygen, fluorine, sulfur, and platinum as determined by energy-dispersive X-ray spectroscopy in a specific region of a cross-section of the electrode catalyst layer is 2 at% to 20 at%. The specific region contains 50% by area or more of the fibrous material containing nitrogen atoms, and does not contain the catalyst material and the conductive carrier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an electrode catalyst layer, a membrane electrode assembly, and a solid polymer fuel cell. Background Art

[0002] Background 1

[0003] Fuel cells are power generation systems that generate electricity through a chemical reaction between hydrogen and oxygen. Compared to conventional power generation methods, fuel cells have the characteristics of high efficiency, low environmental impact, and low noise, and are attracting much attention as a clean energy source of the future. In particular, solid polymer fuel cells that can be used near room temperature are expected to be used as power sources for vehicles and household fixed power sources, and various research and development on solid polymer fuel cells have been carried out in recent years. Issues for their practical application include improving battery performance such as power generation characteristics and durability, infrastructure construction, and reducing manufacturing costs.

[0004] A solid polymer fuel cell is usually composed of multiple stacked cells. The cell has the following structure: a membrane electrode assembly in which a fuel electrode (anode) for supplying fuel gas and an oxygen electrode (cathode) for supplying oxidant are bonded to both sides of a polymer electrolyte membrane and sandwiched by a separator having a gas flow path and a cooling water flow path. The fuel electrode (anode) and the oxygen electrode (cathode) are mainly composed of an electrode catalyst layer containing at least a catalyst material such as a platinum-based precious metal, a conductive carrier and a polymer electrolyte, and a gas diffusion layer having both gas permeability and conductivity.

[0005] In a solid polymer fuel cell, electricity can be obtained via the electrochemical reaction described below. First, in the fuel electrode side electrode catalyst layer, the hydrogen contained in the fuel gas is oxidized by the catalyst substance to become protons and electrons. The generated protons pass through the polymer electrolyte in the electrode catalyst layer and the polymer electrolyte membrane in contact with the electrode catalyst layer to reach the oxygen electrode side electrode catalyst layer. In addition, the electrons generated at the same time pass through the conductive carrier in the fuel electrode side electrode catalyst layer, the gas diffusion layer in contact with the fuel electrode side electrode catalyst layer, the separator and the external circuit to reach the oxygen electrode side electrode catalyst layer. Then, in the oxygen electrode side electrode catalyst layer, the protons and electrons react with the oxygen contained in the oxidant gas such as air to generate water. In these series of reactions, the proton conduction resistance is larger than the electron conduction resistance, so in order to improve the reactivity and improve the performance as a fuel cell, it is important to effectively conduct protons.

[0006] The gas diffusion layer has the function of diffusing the gas supplied from the separator and supplying it to the electrode catalyst layer. In addition, the pores in the electrode catalyst layer are located at the place where the gas diffusion layer passes through the separator, and serve as a passage for transporting various substances. The pores of the fuel electrode need to smoothly supply the hydrogen contained in the fuel gas to the three-phase interface that is the site of the redox reaction. In addition, the pores of the oxygen electrode need to smoothly supply the oxygen contained in the oxidant gas. Furthermore, the pores of the oxygen electrode need to smoothly discharge the generated water produced by the reaction. Here, in order to smoothly supply the gas and smoothly discharge the generated water, it is important to have sufficient gaps in the electrode catalyst layer to smoothly discharge the generated water and not to have a dense structure.

[0007] As a means of controlling the structure of the electrode catalyst layer to be less dense and thereby improving the power generation performance, for example, an electrode catalyst layer including carbon or carbon fibers having different particle sizes has been proposed (Patent Documents 1 and 2).

[0008] In Patent Document 1, by combining carbon particles having moderately different particle sizes, dense packing of carbon particles in the electrode catalyst layer is suppressed. In addition, in Patent Document 2, by including carbon fibers having different fiber lengths and setting their ratio within a certain range, appropriate pores account for the majority in the electrode catalyst layer. On the other hand, when large particles having a larger particle size and small particles having a smaller particle size are mixed, the small particles may enter the gaps between the large particles and fill them densely instead. In addition, in the case where the carbon material is only particles, cracks in the catalyst layer are easily induced, and the resulting reduction in durability may become a problem.

[0009] In addition, for example, when carbon fibers are used as in Patent Document 2, even if dense filling can be prevented, the ratio of electron conductors in the catalyst layer increases and the ratio of proton conductors decreases, so the resistance to proton movement increases, which becomes the main reason for the reduction in power generation performance. The power generation performance in a fuel cell also varies greatly depending on the material transportability / electron conductivity / proton conductivity. As a result, in a method such as using a combination of carbon particles or a combination of carbon fibers to improve only the electron conductivity, there is a limit to improving the power generation performance.

[0010] Background 2

[0011] As a countermeasure to the increasing environmental load on the earth, the demand for creating cleaner energy is increasing. Fuel cells are a power generation system that generates electricity through a chemical reaction between hydrogen and oxygen and only emits water. Fuel cells are highly expected to be a future energy source.

[0012] Fuel cells are classified into alkaline type, phosphoric acid type, solid polymer type, molten carbonate type, and solid oxide type according to the type of electrolyte. Since solid polymer fuel cells can be used at room temperature, they are expected to be widely used as power sources for vehicles and homes. Therefore, research and development on improving power generation performance and durability, and cost reduction measures are being carried out for the practical application of solid polymer fuel cells.

[0013] The solid polymer fuel cell has: a polymer electrolyte membrane with proton conductivity, a fuel electrode as an anode, and an air electrode as a cathode. In the thickness direction of the polymer electrolyte membrane, the fuel electrode and the air electrode sandwich the polymer electrolyte membrane. The fuel electrode has an electrode catalyst layer that separates the fuel gas into protons and electrons. The air electrode has an electrode catalyst layer that oxidizes the protons transported through the polymer electrolyte membrane with an oxygen-containing oxidant and receives electrons from an external circuit. The electrode catalyst layers of the fuel electrode and the air electrode contain catalyst substances such as platinum-based precious metals, carriers that support the catalyst substances, and polymer electrolytes.

[0014] The solid polymer fuel cell is a single cell with a structure in which a gas diffusion layer and a separator are arranged on the surface of each electrode catalyst layer of the fuel electrode and the air electrode on the opposite side of the polymer electrolyte membrane as the basic structure, and a plurality of such single cells are stacked. The gas diffusion layer is a layer with conductivity for uniform diffusion of the reaction gas. The separator is a component that has a gas flow path and a cooling water flow path and is responsible for taking out electrons to the external circuit, and is arranged on the outside of the gas diffusion layer. Hereinafter, the structure in which the fuel electrode and the air electrode are formed on both sides of the polymer electrolyte membrane is referred to as a membrane electrode assembly.

[0015] The polymer electrolyte fuel cell generates electricity by supplying a fuel gas containing hydrogen to a fuel electrode and an oxidant gas containing oxygen to an air electrode, and electrode reactions represented by the following formulas 1 and 2 occur in the fuel electrode and the air electrode.

[0016] Fuel electrode: H2→2H + +2e - ···(Formula 1)

[0017] Air electrode: 1 / 2O2 + 2H + +2e - → H2O···(Formula 2)

[0018] As shown in Formula 1, the fuel gas supplied to the fuel electrode is separated into protons and electrons by the catalyst material contained in the electrode catalyst layer of the fuel electrode. The separated protons pass through the humidified polymer electrolyte and polymer electrolyte membrane contained in the electrode catalyst layer of the fuel electrode and move to the air electrode. The separated electrons are taken out from the fuel electrode to the external circuit, pass through the external circuit and move to the air electrode. As shown in Formula 2, in the air electrode, the oxidant gas reacts with the protons and electrons moved from the fuel electrode to generate water. The electrons pass through the external circuit to generate current.

[0019] However, it can be cited that the electrode catalyst layer of the fuel cell is usually formed of a thin film with a thickness of less than 100 μm, and cracks in the electrode catalyst layer during manufacturing become a problem. Due to the generation of cracks, the proton conduction path and the electron conduction path in the electrode catalyst layer are cut off, and the power generation performance and durability are reduced. In order to solve this problem, as a technology for improving the bonding strength of the electrode catalyst layer, the technology disclosed in Patent Document 3 is known.

[0020] In Patent Document 3, a fibrous substance such as hydrophilic carbon whiskers is added to the electrode catalyst layer to improve the bonding strength of the electrode catalyst layer.

[0021] Prior art literature

[0022] Patent Literature

[0023] Patent Document 1: Japanese Patent No. 3617237

[0024] Patent Document 2: Japanese Patent No. 5537178

[0025] Patent Document 3: Japanese Patent No. 4065862 Summary of the invention

[0026] Problems to be solved by the invention

[0027] Lesson 1

[0028] The present disclosure is completed with a focus on aspects such as the above-mentioned first background, and the subject is to provide an electrode catalyst layer, a membrane electrode assembly and a solid polymer fuel cell that can improve the material transport and proton conductivity in the electrode catalyst layer, exert high power generation performance and have good durability.

[0029] Topic 2

[0030] In conventional fuel cells using the electrode catalyst layer disclosed in Patent Document 3, there is still room for improvement in terms of initial power generation performance.

[0031] When a fibrous substance is added to the electrode catalyst layer, since protons cannot be conducted on the fibrous substance, the proton conduction resistance in the electrode catalyst layer increases, and the power generation performance of the membrane electrode assembly sometimes decreases. In particular, under low humidification conditions, the proton conduction resistance sometimes increases significantly due to the decrease in the water content of the polymer electrolyte. On the other hand, when the ratio of the polymer electrolyte in the electrode catalyst layer is increased in order to improve the proton conductivity, the electronic conductivity in the electrode catalyst layer cannot be ensured, or the water discharged during power generation under high current density cannot be discharged outside the system due to the water retention of the polymer electrolyte, and the power generation performance is reduced. Therefore, it is necessary to exert the power generation performance while suppressing the amount of polymer electrolyte in the catalyst layer to a small amount. Therefore, it becomes very important to properly construct the proton conduction path in the electrode catalyst layer to which the fibrous substance is added.

[0032] The present inventors have conducted intensive research and found that by measuring the amount of polymer electrolyte around the fibrous material in the electrode catalyst layer and finding that a certain amount of polymer electrolyte exists around the fibrous material, the proton conduction path in the electrode catalyst layer can be appropriately constructed, thereby solving the above-mentioned problem.

[0033] One aspect of the present disclosure aims to provide an electrode catalyst layer, a membrane electrode assembly, and a solid polymer fuel cell having excellent initial power generation performance from a low current density region to a high current density region.

[0034] Means for solving problems

[0035] First Invention Group A

[0036] [1] An electrode catalyst layer for a solid polymer fuel cell, characterized in that:

[0037] The electrode catalyst layer comprises: a catalyst substance, a conductive carrier supporting the catalyst substance, a polymer electrolyte, and a fibrous substance containing nitrogen atoms.

[0038] The ratio of the number of nitrogen atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, sulfur and platinum elements obtained by energy dispersive X-ray spectroscopy in a specific area of ​​the cross-section of the electrode catalyst layer is greater than 2 at % and less than 20 at %, and the specific area is an area that contains more than 50 area % of the fibrous material containing nitrogen atoms and does not contain the catalyst substance and the conductive carrier.

[0039] [2] The electrode catalyst layer according to [1], wherein the average fiber diameter of the fibrous material containing nitrogen atoms is 50 nm to 400 nm.

[0040] [3] The electrode catalyst layer according to [1] or [2], wherein the fibrous substance containing nitrogen atoms is a polymer fiber.

[0041] [4] The electrode catalyst layer according to [3], wherein the fibrous substance containing nitrogen atoms has an azole structure.

[0042] [5] The electrode catalyst layer according to any one of [1] to [4], wherein the peak value of the fiber diameter distribution of the fibrous material containing nitrogen atoms is 150 nm or more and 250 nm or less.

[0043] [6] The electrode catalyst layer according to any one of [1] to [5], wherein the content of the fibrous material containing nitrogen atoms in the electrode catalyst layer is 1% by weight or more and 10% by weight or less.

[0044] [7] The electrode catalyst layer according to any one of [1] to [6], wherein the thickness of the electrode catalyst layer is 2 μm or more and 10 μm or less.

[0045] [8] A membrane electrode assembly comprising the electrode catalyst layer according to any one of [1] to [7] on at least one surface of a polymer electrolyte membrane.

[0046] [9] A polymer electrolyte fuel cell comprising the membrane electrode assembly described in [8].

[0047] Second Invention Group B

[0048] One aspect of the present disclosure is an electrode catalyst layer, which is an electrode catalyst layer bonded to a polymer electrolyte membrane, comprising: a catalyst, a fluorine-containing polymer electrolyte, and a fibrous substance, wherein the ratio of the number of fluorine atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, sulfur and platinum elements obtained by energy-dispersive X-ray spectroscopy in a specific area of ​​a cross-section of the electrode catalyst layer is greater than 0.2 at%, and the specific area is an area containing more than 50 area% of the fibrous substance and does not contain a catalyst.

[0049] In one embodiment, the fibrous substance may have an azole structure.

[0050] In one embodiment, the content of the fibrous substance may be 5 parts by mass to 20 parts by mass when the content of the carrier is 100 parts by mass, and the specific region is a region that does not contain the carrier.

[0051] In one embodiment, the polymer electrolyte may cover at least a portion of the surface of the fibrous substance. The thickness of the polymer electrolyte covering the fibrous substance may be 3 nm or more and 30 nm or less.

[0052] In one embodiment, the polymer electrolyte may contain a proton-donating group, and the dry weight of the polymer electrolyte per 1 mol of the proton-donating group may be 600 g / mol or more and 1200 g / mol or less.

[0053] In one embodiment, the average fiber length of the fibrous substance may be 0.7 μm or more and 40 μm or less. The average fiber diameter of the fibrous substance may be 10 nm or more and 500 nm or less.

[0054] In one embodiment, the fibrous material may have a capability of adsorbing a polymer electrolyte. The fibrous material may have an adsorption capacity of 10 mg / g or more for a polymer electrolyte.

[0055] Another aspect of the present disclosure is a membrane electrode assembly including a polymer electrolyte membrane and the electrode catalyst layer, wherein the electrode catalyst layer is bonded to the polymer electrolyte membrane.

[0056] Another aspect of the present disclosure is a solid polymer fuel cell comprising: the above-mentioned membrane electrode assembly, a pair of gas diffusion layers sandwiching the membrane electrode assembly in the thickness direction of the membrane electrode assembly, and a pair of separators sandwiching the membrane electrode assembly and the pair of gas diffusion layers in the thickness direction of the membrane electrode assembly.

[0057] Effects of the Invention

[0058] According to the first invention group A which is one embodiment of the present disclosure, it is possible to provide an electrode catalyst layer, a membrane electrode assembly, and a solid polymer fuel cell that can improve the mass transport property and proton conductivity in the electrode catalyst layer, exhibit high power generation performance, and have good durability.

[0059] According to the second invention group B as one aspect of the present disclosure, there are provided an electrode catalyst layer, a membrane electrode assembly, and a solid polymer fuel cell having excellent initial power generation performance from a low current density region to a high current density region. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] [ Figure 1 ] is a cross-sectional view schematically showing an example of the cross-sectional structure of the electrode catalyst layer of the first invention group of the present disclosure.

[0061] [ Figure 2 ] is a schematic diagram showing an example of a cross-section of an electrode catalyst layer of the first invention group and an example of a cross-section of the first electrode catalyst layer of the second invention group.

[0062] [ Figure 3 ] is an illustration of the fiber diameter distribution of the fibers of the first invention group.

[0063] [ Figure 4 ] is an illustration of the fiber diameter of the fibers of the first invention group.

[0064] [ Figure 5 ] shows an example of the structure of the membrane electrode assembly involved in this embodiment of the first invention group, Figure 5 (a) is a plan view of the membrane electrode assembly viewed from the oxygen electrode side of the electrode catalyst layer. Figure 5 (b) is Figure 5 (a) Cross-sectional view after fracture at line XX'.

[0065] [ Figure 6 ] is a decomposed perspective view showing an example of the structure of a solid polymer fuel cell of the first invention group.

[0066] [ Figure 7 ] is a cross-sectional view showing the structure of a membrane electrode assembly in one embodiment of the second invention group.

[0067] [ Figure 8 ] is a schematic diagram schematically showing the structure of the first electrode catalyst layer in one embodiment of the second invention group.

[0068] [ Fig. 9 ] is a cross-sectional view showing the structure of catalyst-supported particles contained in the first electrode catalyst layer in one embodiment of the second invention group.

[0069] [ Fig.10 ] is a decomposed perspective view showing the structure of a solid polymer fuel cell in one embodiment of the second invention group. DETAILED DESCRIPTION

[0070] First invention group

[0071] Hereinafter, the embodiments of the present disclosure will be described with reference to the accompanying drawings. It should be noted that the present disclosure is not limited to the embodiments described below, and the design can be modified according to the knowledge of those skilled in the art, and the embodiments with such modifications are also included in the scope of the present disclosure. In addition, for ease of understanding, the drawings are appropriately exaggerated.

[0072] The inventors of the present disclosure have conducted in-depth research on the initial power generation performance and the durable power generation performance of solid polymer fuel cells, and found that the gas diffusivity and proton conductivity in the electrode catalyst layer have a great influence on these performances. In addition, by using a fibrous material containing nitrogen atoms in the electrode catalyst layer, a wide gap is formed to improve the gas diffusivity and reduce the proton conduction resistance. In addition, by making the ratio of the number of nitrogen atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, sulfur and platinum elements obtained by energy dispersive X-ray spectroscopy in a specific area of ​​the cross section of the electrode catalyst layer 2at% or more and 20at% or less, a solid polymer fuel cell with high power generation performance and excellent durability is successfully obtained.

[0073] It was also found that when the peak value of the fiber diameter distribution of the fibrous material was set to be between 150 nm and 250 nm, the proton conduction resistance was reduced without damaging the conductivity, and the gas diffusivity was improved. As a result, a solid polymer fuel cell was successfully obtained that suppressed the reduction of output power and the degradation of the electrode catalyst layer and exerted high power generation performance for a long time.

[0074] [Constitution of Electrode Catalyst Layer]

[0075] Hereinafter, the specific configuration of the electrode catalyst layer according to the present embodiment will be described with reference to the drawings.

[0076] like Figure 1 As shown in the schematic diagram, the electrode catalyst layer 10 involved in this embodiment is configured to be bonded to the surface of the polymer electrolyte membrane 11, and includes a catalyst substance 12, a conductive carrier 13 supporting the catalyst substance 12, a polymer electrolyte 14, and a fibrous substance 15 containing nitrogen atoms. In addition, the portion where any of the above components are not present becomes a gap 4.

[0077] The fibrous material 15 contained in the electrode catalyst layer 10 according to the present embodiment is a fibrous material containing nitrogen atoms. An example of the fiber containing nitrogen atoms is a polymer fiber containing nitrogen atoms. The nitrogen atoms in the fibrous material preferably constitute Lewis basic groups having unshared electron pairs.

[0078] The fibrous material containing nitrogen atoms preferably has an azole structure. An azole structure refers to a five-membered heterocyclic structure containing one or more nitrogen atoms, such as an imidazole structure, an oxazole structure, and a thiazole structure. In addition, the fibrous material containing nitrogen atoms preferably has a benzoxazole structure such as a benzimidazole structure and a benzoxazole structure. As specific examples of the fibrous material containing nitrogen atoms, polyazole-based polymers such as polybenzimidazole and polybenzoxazole can be cited.

[0079] Furthermore, the fibrous substance containing nitrogen atoms may be a polymer having a pyrrole ring structure or a pyridine ring structure.

[0080] When the fibrous material contains nitrogen atoms, the interaction between the unshared electron pairs of the nitrogen atoms and the protons of the polymer electrolyte can be generated. Thus, the proton conductivity in the electrode catalyst layer 10 can be improved, and the output power characteristics can be improved. For example, the fibrous material can be covered with a polymer electrolyte film, and the material transportability and proton conductivity in the electrode catalyst layer 10 can also be improved at the same time.

[0081] By making the fibrous substance a polymer, the flexibility is improved, and the strength of the electrode catalyst layer 10 is improved. In addition, the thermal stability of the electrode catalyst layer 10 is improved by introducing nitrogen.

[0082] In addition, in the electrode catalyst layer 10, it is preferred that the content of the fibrous substance 15 in the electrode catalyst layer 10 is 1% by weight or more and 10% by weight or less. When the content of the fibrous substance 15 is less than the above range, the gap 4 becomes narrower and sufficient drainage and gas diffusion may not be ensured. In addition, cracks may be generated in the electrode catalyst layer 10, and durability may be reduced. When the content of the fibrous substance 15 is greater than the above range, the proton conduction path of the polymer electrolyte 14 may be cut off, thereby increasing resistance.

[0083] In this embodiment, the ratio of the number of nitrogen atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, sulfur and platinum elements obtained by energy dispersive X-ray spectroscopy (EDX) in a specific area of ​​the cross section of the electrode catalyst layer is 2 at% or more and 20 at% or less. The specific area refers to the cross section of the electrode catalyst layer, and is an area that contains more than 50% by area of ​​fibrous substances containing nitrogen atoms and does not contain catalyst substances and conductive carriers. The shape of the area (observation area) can be a rectangle (including a square), for example, a square of 150nm×150nm. The fibrous substance containing nitrogen atoms in the specific area can account for 100% of the area. The specific area only needs to be one in the cross section.

[0084] Figure 2 : is a schematic diagram showing an example of a cross section of an electrode catalyst layer. The cross section of the electrode catalyst layer is composed of a region R1 containing a catalyst substance and a conductive carrier and a region R2 not containing a catalyst substance and a conductive carrier. The region R2 is composed of a fibrous substance 23 containing nitrogen atoms and a region n not containing the fibrous substance 23 containing nitrogen atoms. Figure 2 In the above-mentioned specific region (observation region) is represented by A, which only includes region R2 and does not include region R1. The shape of the region (observation region) can be a rectangle (including a square), for example, a square of 150nm×150nm. The fibrous material 23 containing nitrogen atoms in the specific region can occupy 100% of the area. The specific region only needs to be one in the cross section.

[0085] The composition ratio of the elements in a specific region can be measured, for example, by performing element mapping using a transmission electron microscope (TEM-EDX) equipped with an energy dispersive X-ray spectrometer. It is appropriate to set the acceleration voltage of the X-rays in EDX to 200 kV. With such an acceleration voltage, the electron beam can be made to penetrate a thickness of about nm in a specific region, and information on the elements of the fiber and the surrounding of the fiber can be obtained.

[0086] A nitrogen atomic ratio of less than 2 at% in the EDX analysis of a specific region means that the density level of the fiber is too low. A nitrogen atomic ratio of more than 20 at% in the EDX analysis of a specific region means that the density level of the fiber is too high. A nitrogen atomic ratio of 2 at% to 20 at% in the EDX analysis of a specific region means that the density level of the fiber is appropriate.

[0087] When the density of the fibers is too low, the interaction between the nitrogen-containing fibers and the sulfonic acid group plasma of the polymer electrolyte is weakened, the proton conduction path is insufficient, and the resistance tends to increase. In addition, when the density of the fibers is too high, the gaps may be blocked due to entanglement and aggregation of the fibers, and sufficient drainage and gas diffusion cannot be ensured.

[0088] By appropriately setting the density of the fibers, the unshared electron pairs of the nitrogen atoms interact with the protons of the polymer electrolyte, thereby improving the proton conductivity in the electrode catalyst layer and improving the output characteristics.

[0089] The method of exposing the cross section is the same as the method of observing the thickness of the electrode catalyst layer 10 described below.

[0090] The weight ratio of the fibrous substance 15 contained in the electrode catalyst layer 10 can be obtained by the ratio of the weight after the substance other than the substance is removed by chemical method and electrochemical method to the weight before removal. For example, the catalyst substance is dissolved by an acid such as aqua regia containing a strong oxidant, and the conductive carrier can be burned by a high potential. In addition, the polymer electrolyte or polymer electrolyte membrane can be decomposed by hydrogen peroxide or the like.

[0091] The average fiber diameter of the fibrous material 15 contained in the electrode catalyst layer 10 involved in this embodiment is preferably 50 nm or more and 400 nm or less. By making the fiber diameter within this range, the voids 4 in the electrode catalyst layer 10 can be increased, and the reduction of proton conductivity can be suppressed, and high output power can be achieved. In the case where the average fiber diameter of the fibrous material 15 is less than the above range, the fibrous material may block the voids, thereby failing to ensure sufficient drainage and gas diffusivity. Since the fibrous material does not have electronic conductivity, the more the amount added, the lower the electronic conductivity. The finer the fiber diameter, the more the number of roots increases under the same added weight, and the surface area also increases, so it can bring the above-mentioned effect to a wider range of catalyst layers. Therefore, the fibrous material is preferably finer. On the other hand, the size of the voids naturally generated when the aggregates of the catalyst-loaded particles condense to form agglomerates is about 50 nm. Therefore, when the fiber diameter is less than 50 nm, the voids are blocked instead, which may lead to a reduction in drainage. On the other hand, when the average fiber diameter of the fibrous substance 15 is larger than the above range, the conduction of electrons or protons between the conductive support 13 and the polymer electrolyte 14 may be hindered, thereby increasing the resistance.

[0092] The fiber length of the fibrous material 15 is preferably 1 μm to 80 μm, more preferably 5 μm to 70 μm. By setting the fiber length within the above range, the strength of the electrode catalyst layer 10 can be increased, and cracks can be suppressed when the electrode catalyst layer 10 is formed.

[0093] The fiber diameter of the fibrous substance 15 can be obtained, for example, by measuring the diameter of the fibrous substance 15 exposed in the cross section when observing the cross section of the electrode catalyst layer 10 using a scanning electron microscope (SEM). When the fibrous substance 15 is cut obliquely, the shape of the exposed cross section sometimes becomes an ellipse. In this case, the fiber diameter of the fibrous substance 15 can be obtained by measuring the diameter of the true circle obtained by fitting along the minor axis. The average fiber diameter can be obtained by measuring the fiber diameter of the fibrous substance 15 at multiple locations, for example 20, and taking the arithmetic average.

[0094] In the present embodiment, the peak value of the fiber diameter distribution of the nitrogen-containing fibrous substance 15 contained in the electrode catalyst layer 10 is preferably greater than 150 nm and less than 250 nm. When the fiber diameter of the fibrous substance is smaller than the above range, the gap may become narrower, thereby failing to ensure sufficient drainage and gas diffusivity. In this case, water is retained in the electrode catalyst layer 10, sometimes promoting a decrease in output power and degradation of the electrode catalyst layer. When the fiber diameter of the fibrous substance is greater than the above range, the proton conduction path of the polymer electrolyte 14 and the electron conduction path of the conductive carrier 13 may be cut off, thereby increasing resistance.

[0095] Here, the peak value of the fiber diameter distribution of the fibrous substance will be described. Figure 3 This is an explanatory diagram of the fiber diameter distribution of the fibrous material. The curve graph is a histogram showing the frequency of each fiber diameter of the fibrous material contained in the electrode catalyst layer 10, and shows the distribution of the fiber diameter. Generally, a histogram is used to observe the data distribution of a quantity. After the data is divided into several levels and a frequency distribution table is prepared, the horizontal axis takes the level of the data and the vertical axis takes the number of data contained in the level to prepare a curve graph, which is a histogram.

[0096] In the present embodiment, the level width of the histogram is set to 10nm. For example, when the maximum value of the obtained fiber diameter is 298nm and the minimum value is 102nm, when the level width of the histogram is set to 10nm, the minimum level is "100nm or more and less than 110nm", and the maximum level is "290nm or more and less than 300nm". The number of levels (the number of columns of the histogram) is 20. In this case, each level of the histogram is represented by "100+(n-1)×10nm or more and less than 100+n×10nm" (n=1~20). By determining the levels in this way and preparing a frequency distribution table of the measured fiber diameters, a histogram representing the fiber diameter distribution can be obtained. In addition, the peak value of the fiber diameter distribution refers to the central value of the level with the highest frequency in the frequency distribution table and the histogram. For example, in the histogram of the fiber diameters of the fibrous substance included in the electrode catalyst layer 10 , when the frequency of the class of 200 nm or more and less than 210 nm is the largest, the peak of the fiber diameter distribution of the fibrous substance is 205 nm.

[0097] For example Figure 4As shown, the fiber diameter of the fibrous material can be obtained by measuring the diameter of the exposed fibrous material when observing the cross section of the electrode catalyst layer 10 using a scanning electron microscope (SEM). When the fibrous material is beveled, the shape of the exposed cross section sometimes becomes an ellipse. In this case, the fiber diameter can be obtained by measuring the diameter of the true circle obtained by fitting along the minor axis. In addition, sometimes it is not the cross section of the fibrous material but the surface of the fibrous material that is exposed. In this case, the fiber diameter can be obtained by measuring the width of the fiber orthogonal to the major axis of the exposed fibrous material. By measuring the fiber diameters of multiple fibrous materials, a histogram representing the frequency of each fiber diameter can be obtained. The more locations where the fiber diameter is measured, the more clearly the peak value of the fiber diameter can be grasped. In order to grasp the fiber diameter distribution of the fibrous material without deviation in the electrode catalyst layer 10, it is preferred to measure at least 20 or more observation points in the same manner. From the point of view of being able to clearly confirm the outline of the fibrous material and correctly measure the fiber diameter, the observation magnification of the scanning electron microscope (SEM) is preferably set to about 50,000 times or more.

[0098] As a method for exposing the cross section of the electrode catalyst layer 10, for example, known methods such as ion milling and ultramicrotomy can be used. When performing the process of exposing the cross section, in order to reduce damage to the polymer electrolyte 14 constituting the polymer electrolyte membrane 11 and the electrode catalyst layer 10, it is particularly preferred to use cryo-ion milling (cryo-ion milling) while cooling the electrode catalyst layer 10.

[0099] The thickness of the electrode catalyst layer 10 is preferably 30 μm or less. If the thickness is greater than 30 μm, cracks are easily generated, and when used in a fuel cell, the diffusibility and conductivity of the gas and generated water are reduced, thereby reducing the output power. The thickness may be 10 μm or less.

[0100] The thickness of the electrode catalyst layer 10 is preferably 2 μm or more. When the thickness is greater than 10 μm, cracks are easily generated, and when used in a fuel cell, the diffusivity and conductivity of the gas and generated water are reduced, thereby reducing the output power. The thickness of the electrode catalyst layer 10 may be 5 μm or more.

[0101] The thickness of the electrode catalyst layer 10 can be measured, for example, by observing the cross section of the electrode catalyst layer 10 using a scanning electron microscope (SEM). As a method for exposing the cross section of the electrode catalyst layer 10, for example, known methods such as ion milling and ultramicrotomy can be used. When performing processing to expose the cross section, in order to reduce damage to the polymer electrolyte 14 constituting the polymer electrolyte membrane 11 and the electrode catalyst layer 10, it is particularly preferred to use cryogenic ion milling (cryo ion milling) while processing the electrode catalyst layer 10. For example, in a visual field that accommodates the entire electrode catalyst layer at an observation magnification of about 1000 to 10000 times, the thickness of the electrode catalyst layer can be measured. In order to grasp the thickness without deviation in the catalyst layer, it is preferred to measure at least 20 or more observation points in the same way.

[0102] The catalyst material 12 may be, for example, a metal included in the platinum group, a metal other than the platinum group, and an alloy, oxide, composite oxide, carbide, etc. of these metals. The metals included in the platinum group are platinum, palladium, ruthenium, iridium, rhodium, and osmium. The metals other than the platinum group may be iron, lead, copper, chromium, cobalt, nickel, manganese, vanadium, molybdenum, gallium, aluminum, etc.

[0103] The conductive carrier 13 can use a carrier that has conductivity and can load the catalyst substance 12 without being corroded by the catalyst substance 12. The conductive carrier 13 can use carbon particles. Carbon particles can use carbon black, graphite, black lead, activated carbon, carbon nanotubes, carbon nanofibers and fullerenes, for example. The particle size of the carbon particles is preferably about 10nm or more and about 1000nm or less, and more preferably about 10nm or more and about 100nm or less. By making the particle size greater than 10nm, the carbon particles will not be too densely packed in the electrode catalyst layer 10, thereby suppressing the reduction of the gas diffusion property of the electrode catalyst layer 10. By making the particle size less than 1000nm, the generation of cracks in the electrode catalyst layer 10 can be suppressed. It should be noted that the particle size of the carbon particles is the volume average diameter using the laser diffraction / scattering method.

[0104] The polymer electrolyte 14 contained in the polymer electrolyte membrane 11 and the electrode catalyst layer 10 can use an electrolyte having proton conductivity. The polymer electrolyte can use, for example, a fluorine-based polymer electrolyte and a hydrocarbon-based polymer electrolyte. The fluorine-based polymer electrolyte can use a polymer electrolyte having a tetrafluoroethylene skeleton. It should be noted that the polymer electrolyte having a tetrafluoroethylene skeleton can be exemplified by Nafion (registered trademark) manufactured by DuPont. The hydrocarbon-based polymer electrolyte can use, for example, sulfonated polyether ketone, sulfonated polyether sulfone, sulfonated polyether ether sulfone, sulfonated polysulfide, and sulfonated polyphenylene.

[0105] The polymer electrolyte contained in the polymer electrolyte membrane 11 and the polymer electrolyte 14 contained in the electrode catalyst layer 10 may be the same electrolyte or different electrolytes. However, considering the interface resistance at the interface between the polymer electrolyte membrane 11 and the electrode catalyst layer 10 and the dimensional change rate of the polymer electrolyte membrane 11 and the electrode catalyst layer 10 when the humidity changes, the polymer electrolyte contained in the polymer electrolyte membrane 11 and the polymer electrolyte 14 contained in the electrode catalyst layer 10 are preferably the same electrolyte or polymer electrolytes with similar thermal expansion coefficients.

[0106] [Structure of membrane electrode assembly]

[0107] Next, refer to Figure 5 The specific structure of the membrane electrode assembly 1 including the electrode catalyst layer 10 according to the present embodiment will be described. Figure 5 The following diagram shows a configuration example of a membrane electrode assembly according to the present embodiment. (a) is a plan view of the membrane electrode assembly viewed from the oxygen electrode side of the electrode catalyst layer 10 , and (b) is a cross-sectional view taken along the line XX′ in (a).

[0108] The membrane electrode assembly 1 includes a polymer electrolyte membrane 11, and electrode catalyst layers 10C and 10A bonded to the surface and back of the polymer electrolyte membrane 11, respectively. In the present embodiment, the electrode catalyst layer 10C formed on the upper surface (surface) of the polymer electrolyte membrane 11 is a cathode-side electrode catalyst layer constituting an oxygen electrode, and the electrode catalyst layer 10A formed on the lower surface (back surface) of the polymer electrolyte membrane 11 is an anode-side electrode catalyst layer constituting a fuel electrode. Hereinafter, when no distinction is required, a pair of electrode catalyst layers 10C and 10A are sometimes referred to as "electrode catalyst layers 10". In the membrane electrode assembly 1 according to the present embodiment, it is sufficient as long as the electrode catalyst layer 10 is provided on at least one surface of the polymer electrolyte membrane 11. In addition, in order to prevent gas leakage from the peripheral portion of the polymer electrolyte membrane 11 that is not bonded to the electrode catalyst layer 10, a gasket 16C on the oxygen electrode side and a gasket 16A on the fuel electrode side are arranged on the membrane electrode assembly 1.

[0109] [Method for producing membrane electrode assembly]

[0110] Next, a method for producing the membrane electrode assembly 1 will be described.

[0111] First, a catalyst ink is prepared. The catalyst material 12, the conductive carrier 13, the polymer electrolyte 14, and the fibrous material 15 are mixed in a dispersion medium, and then the mixture is subjected to a dispersion treatment to prepare the catalyst ink. The dispersion treatment can be performed using, for example, a planetary ball mill, a bead mill, or an ultrasonic homogenizer.

[0112] The dispersion medium of the catalyst ink may use a solvent that does not corrode the catalyst substance 12, the conductive carrier 13, the polymer electrolyte 14, and the fibrous substance 15, and can dissolve the polymer electrolyte 14 or disperse the polymer electrolyte 14 in the form of a fine gel while the dispersion medium has high fluidity. The dispersion medium may also contain water. The catalyst ink preferably contains a volatile liquid organic solvent. Since there is a risk of fire when the solvent is a lower alcohol, it is preferred to mix water in such a solvent. In the solvent, water may be mixed within a range that does not separate the polymer electrolyte 14 and does not cause the catalyst ink to become cloudy or gelled.

[0113] The prepared catalyst ink is applied to the substrate and then dried to remove the solvent from the coating of the catalyst ink. Thus, an electrode catalyst layer 10 is formed on the substrate. The substrate can use a polymer electrolyte membrane 11 or a transfer substrate. In the case of using a polymer electrolyte membrane 11 as a substrate, for example, the following method can be used: the catalyst ink is directly applied to the surface of the polymer electrolyte membrane 11, and then the solvent is removed from the coating of the catalyst ink to form the electrode catalyst layer 10. Then, the catalyst ink is directly applied to the surface on the opposite side of the polymer electrolyte membrane 11 in a manner that the polymer electrolyte membrane 11 is sandwiched and opposite to the electrode catalyst layer 10A, and then the solvent is removed from the coating of the catalyst ink, thereby forming the electrode catalyst layer 10A and obtaining the membrane electrode assembly 1.

[0114] When a transfer substrate is used, a catalyst ink is applied to the transfer substrate and then dried to produce a substrate with a catalyst layer. Then, for example, the surface of the electrode catalyst layer 10 in the substrate with a catalyst layer is brought into contact with the polymer electrolyte membrane 11 by heating and pressurizing to bond the electrode catalyst layer 10 to the polymer electrolyte membrane 11. By bonding the electrode catalyst layer 10 to both surfaces of the polymer electrolyte membrane 11, a membrane electrode assembly 1 can be produced.

[0115] In order to adjust the ratio of the number of nitrogen atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, sulfur and platinum elements obtained by energy dispersive X-ray spectroscopy in a specific area of ​​the electrode catalyst layer to the above-mentioned range, for example, it can be prepared by adjusting the fiber diameter of the nitrogen-containing fiber in the electrode catalyst layer, adjusting the amount of polymer electrolyte in the electrode catalyst layer, and adjusting the amount of nitrogen-containing fiber in the electrode catalyst layer.

[0116] In addition, when the gas diffusion layer 17 is used as a substrate, for example, a catalyst ink is applied to the surface of the gas diffusion layer 17 and then dried to produce the gas diffusion layer 17 with a catalyst layer. Then, the surface of the electrode catalyst layer 10 in the gas diffusion layer 17 with a catalyst layer is heated and pressurized in a state where the surface is in contact with the polymer electrolyte membrane 11, so that the electrode catalyst layer 10 is bonded to the polymer electrolyte membrane 11. By bonding the electrode catalyst layer 10 to both surfaces of the polymer electrolyte membrane 11, the membrane electrode assembly 1 can be produced.

[0117] Various coating methods can be used to apply the catalyst ink to the substrate. Examples of coating methods include die coating, roller coating, curtain coating, spray coating, and blade coating. The coating method preferably uses die coating. Die coating is preferred in that the film thickness is stable during coating and intermittent coating can be performed. The drying method of the catalyst ink coating film can be, for example, drying using a hot air oven, IR (far infrared) drying, drying using a hot plate, and reduced pressure drying. The drying temperature is between 40°C and 200°C, preferably between 40°C and 120°C. The drying time is between 0.5 minutes and 1 hour, preferably between 1 minute and 30 minutes.

[0118] When the electrode catalyst layer 10 is formed on the transfer substrate, the pressure and temperature applied to the electrode catalyst layer 10 when transferring the electrode catalyst layer 10 will affect the power generation performance of the membrane electrode assembly 1. In order to obtain a membrane electrode assembly with high power generation performance, the pressure applied to the electrode catalyst layer 10 is preferably above 0.1 MPa and below 20 MPa. By making the pressure below 20 MPa, the electrode catalyst layer 10 can be prevented from being over-compressed. By making the pressure above 0.1 MPa, the reduction in power generation performance caused by the reduction in the bonding between the electrode catalyst layer 10 and the polymer electrolyte membrane 11 can be suppressed. In view of improving the bonding of the interface between the polymer electrolyte membrane 11 and the electrode catalyst layer 10 and suppressing the interface resistance, the temperature during bonding is preferably near the glass transition temperature of the polymer electrolyte membrane 11 or the polymer electrolyte 14 contained in the electrode catalyst layer 10.

[0119] The transfer substrate can be, for example, a polymer film and a sheet formed by a fluororesin. The transferability of the fluororesin is excellent. Fluororesins can be, for example, ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroperfluoroalkyl vinyl ether copolymer (PFA) and polytetrafluoroethylene (PTFE). The polymer forming the polymer film can be, for example, polyimide, polyethylene terephthalate, polyamide (nylon (registered trademark)), polysulfone, polyether sulfone, polyphenylene sulfide, polyether / ether ketone, polyetherimide, polyarylate and polyethylene naphthalate. The transfer substrate can also be a gas diffusion layer.

[0120] Here, by adjusting the mixing ratio of the fibrous substance 15, the mixing ratio of the polymer electrolyte 14, the solvent composition of the catalyst ink, the dispersion strength during the preparation of the catalyst ink, the heating temperature of the catalyst ink after coating and its heating rate, etc., the electrode catalyst layer 10 can have sufficient gas diffusivity and proton conductivity.

[0121] For example, it is preferred that the proportion of the polymer electrolyte 14 in the electrode catalyst layer 10 is about the same as or about half of the weight of the conductive support 13. In addition, the proportion of the fibrous substance 15 is preferably equal to or less than the weight of the conductive support 13. The solid content ratio of the catalyst ink is preferably as high as possible within the range that can be applied to a thin film.

[0122] In addition, the proportion of the nitrogen-containing fibrous substance 15 containing nitrogen atoms in the electrode catalyst layer 10 is preferably about 1% by mass or more and about 10% by mass or less. When the proportion of the fibrous substance 15 containing nitrogen atoms in the electrode catalyst layer 10 is less than 1% by mass, not only can the effect of reducing the proton conduction resistance and improving the gas diffusivity not be fully obtained, but also cracks may be generated when the electrode catalyst layer 10 is formed, thereby reducing the durability during long-term operation. On the other hand, when the proportion of the fibrous substance 15 in the electrode catalyst layer 10 is greater than 10% by mass, the catalyst reaction may be hindered, thereby reducing the battery performance. The higher the solid content ratio of the catalyst ink is within the range that can be applied to the film, the better.

[0123] [Structure of solid polymer fuel cells]

[0124] Next, refer to Figure 6 A specific configuration example of a polymer electrolyte fuel cell 3 including the membrane electrode assembly 1 according to the present embodiment will be described. Figure 6 1 is an exploded perspective view showing a configuration example of a solid polymer fuel cell 3 equipped with a membrane electrode assembly 1. Figure 6 This is an example of a single cell configuration, and the polymer electrolyte fuel cell 3 is not limited to this configuration, but may be a configuration in which a plurality of single cells are stacked.

[0125] like Figure 6 As shown, the solid polymer fuel cell 3 includes a membrane electrode assembly 1, a gas diffusion layer 17C on the oxygen electrode side, and a gas diffusion layer 17A on the fuel electrode side. The gas diffusion layer 17C is arranged opposite to the electrode catalyst layer 10C, which is the cathode side electrode catalyst layer on the oxygen electrode side of the membrane electrode assembly 1. In addition, the gas diffusion layer 17A is arranged opposite to the electrode catalyst layer 10A, which is the anode side electrode catalyst layer on the fuel electrode side of the membrane electrode assembly 1. In addition, the oxygen electrode 2C is formed by the electrode catalyst layer 10C and the gas diffusion layer 17C, and the fuel electrode 2A is formed by the electrode catalyst layer 10A and the gas diffusion layer 17A. In addition, in order to prevent gas leakage from the peripheral portion of the polymer electrolyte membrane 11 that is not bonded to the electrode catalyst layer 10, a gasket 16C on the oxygen electrode side and a gasket 16A on the fuel electrode side are provided.

[0126] Furthermore, the solid polymer fuel cell 3 includes a separator 18C disposed opposite to the oxygen electrode 2C and a separator 18A disposed opposite to the fuel electrode 2A. The separator 18C includes a gas flow path 19C for the flow of reaction gas formed on the surface opposite to the gas diffusion layer 17C, and a cooling water flow path 20C for the flow of cooling water formed on the surface opposite to the surface on which the gas flow path 19C is formed. In addition, the separator 18A has the same structure as the separator 18C, and includes a gas flow path 19A formed on the surface opposite to the gas diffusion layer 17A, and a cooling water flow path 20A formed on the surface opposite to the surface on which the gas flow path 19A is formed. The separators 18C and 18A are made of a material having electrical conductivity and gas impermeability.

[0127] Then, in the solid polymer fuel cell 3, an oxidant such as air or oxygen is supplied to the oxygen electrode 2C through the gas flow path 19C of the separator 18C, and a hydrogen-containing fuel gas or an organic fuel is supplied to the fuel electrode 2A through the gas flow path 19A of the separator 18A, thereby generating electricity.

[0128] The polymer electrolyte fuel cell 3 according to the present embodiment uses the membrane electrode assembly 1 according to the present embodiment and therefore has sufficient water discharge and gas diffusivity, and can exhibit high power generation performance and high durability for a long period of time.

[0129] That is, according to the present embodiment, it is possible to provide an electrode catalyst layer 10, a membrane electrode assembly 1, and a solid polymer fuel cell 3 that have sufficient gas diffusivity and proton conductivity during the operation of the solid polymer fuel cell 3, thereby being able to exert high power generation performance and high durability for a long time. Therefore, the present disclosure can be applied to a stationary cogeneration system or a fuel cell vehicle using a solid polymer fuel cell, and has great industrial value.

[0130] Second invention group

[0131] Reference Figures 7 to 9 , an embodiment of an electrode catalyst layer, a membrane electrode assembly, and a solid polymer fuel cell is described. For ease of understanding, the various figures of the accompanying drawings are appropriately exaggerated. In addition, the configuration and materials of the electrode catalyst layer, membrane electrode assembly, solid polymer fuel cell, and their manufacturing methods of this embodiment are not limited to the configuration and materials described below, and include all materials and configurations that are analogized to have the same function.

[0132] [Membrane Electrode Assembly]

[0133] like Figure 7 As shown, the membrane electrode assembly 100 includes a polymer electrolyte membrane 11 , a cathode electrode catalyst layer 12C, and an anode electrode catalyst layer 12A.

[0134] The polymer electrolyte membrane 11 is a solid polymer electrolyte membrane. The polymer electrolyte membrane 11 is formed, for example, of a polymer material having proton conductivity. Examples of polymer materials having proton conductivity include fluororesins and hydrocarbon resins. Examples of fluororesins include Nafion (manufactured by DuPont, registered trademark), Flemion (manufactured by AGC, registered trademark), and Gore-Select (manufactured by WL Gore & Associates Inc., registered trademark). Examples of hydrocarbon resins include engineering plastics and engineering plastics into which sulfonic acid groups are introduced.

[0135] The cathode side electrode catalyst layer 12C is an electrode catalyst layer constituting an air electrode as a cathode, and is bonded to a surface on one side of the polymer electrolyte membrane 11. The cathode side electrode catalyst layer 12C is a layer for oxidizing protons transported via the polymer electrolyte membrane 11 using an oxygen-containing oxidant and receiving electrons from an external circuit. The anode side electrode catalyst layer 12A is an electrode catalyst layer constituting a fuel electrode as an anode, and is bonded to a surface on the opposite side of the surface of the polymer electrolyte membrane 11 bonded to the cathode side electrode catalyst layer 12C. The anode side electrode catalyst layer 12A is a layer for separating fuel gas into protons and electrons. In addition, hereinafter, it is sometimes described as an electrode catalyst layer in a conceptual form including the cathode side electrode catalyst layer 12C and the anode side electrode catalyst layer 12A.

[0136] [Electrode catalyst layer]

[0137] The first electrode catalyst layer and the second electrode catalyst layer as the electrode catalyst layer are described below. The cathode side electrode catalyst layer 12C and the anode side electrode catalyst layer 12A are both the first electrode catalyst layer. Alternatively, any one of the cathode side electrode catalyst layer 12C and the anode side electrode catalyst layer 12A is the first electrode catalyst layer, and any other is the second electrode catalyst layer. That is, at least one of the cathode side electrode catalyst layer 12C and the anode side electrode catalyst layer 12A is used as the first electrode catalyst layer. As a result, an improvement of 1.5 A / cm 2 It should be noted that, from the viewpoint of improving the above-mentioned effect, when only one of the cathode side electrode catalyst layer 12C and the anode side electrode catalyst layer 12A is used as the first electrode catalyst layer, it is preferred that the cathode side electrode catalyst layer 12C constituting the air electrode is used as the first electrode catalyst layer.

[0138] (First Electrode Catalyst Layer)

[0139] like Figure 8 As shown, the first electrode catalyst layer 20 includes catalyst-supported particles 21, a polymer electrolyte 22, and a fibrous substance 23. In addition, the first electrode catalyst layer 20 may include other known components contained in the electrode catalyst layer of a fuel cell as arbitrary components.

[0140] <Catalyst Supported Particles>

[0141] like Fig. 9 As shown, the catalyst-supporting particle 21 includes a catalyst 21 a and a carrier 21 b that supports the catalyst 21 a.

[0142] As the catalyst 21a, for example, metals included in the platinum group, metals other than the platinum group, or their alloys, oxides, composite oxides, carbides can be used. As metals included in the platinum group, for example, platinum, palladium, ruthenium, iridium, rhodium and osmium can be listed. As metals other than the platinum group, for example, gold, iron, lead, copper, chromium, cobalt, nickel, manganese, vanadium, molybdenum, gallium and aluminum can be listed. Among these, platinum, gold, palladium, rhodium, ruthenium and their alloys are highly active as catalysts and are suitable. It should be noted that the catalyst 21a constituting the catalyst-supported particles 21 may be only one of the above examples, or a combination of two or more.

[0143] The average particle size of the catalyst 21a is preferably 0.5 nm or more and 20 nm or less, and more preferably 1 nm or more and 5 nm or less. By setting the average particle size of the catalyst 21a to be 0.5 nm or more, the decrease in stability can be suppressed. In addition, by setting the average particle size of the catalyst 21a to be 20 nm or less, the decrease in activity can be suppressed. It should be noted that in this specification, the arithmetic mean particle size obtained by particle size measurement is defined as the average particle size.

[0144] As the carrier 21b, a material that is conductive, not corroded by the catalyst 21a, and capable of loading the catalyst 21a is used. As the above-mentioned material constituting the carrier 21b, for example, carbon materials such as carbon black, graphite, black lead, activated carbon, carbon nanotubes, carbon nanofibers, and fullerenes, and metal oxides can be listed. The metal oxide can be, for example, tin oxide. Tungsten or niobium can be doped in tin oxide. Thus, the conductivity of the carrier 21b can be improved. The carrier 21b is particularly preferably a carbon material. By selecting a carbon material as the carrier 21b, the surface area of ​​the carrier 21b can be increased compared to the case of selecting other carriers, and the catalyst 21a can be loaded at a high density. Thus, the catalytic activity of each carrier 21b can be improved. The carrier 21b constituting the catalyst-loaded particle 21 can be only one of the above examples, or a combination of two or more.

[0145] The specific surface area of ​​the carrier 21b is preferably within 50 m 2 / g above 2000m 2 / g or less, more preferably within 100 m 2 / g above 1500m 2 / g or less. By making the specific surface area of ​​the carrier 21b 50m 2 / g or more, the catalyst 21a can be loaded at a high density, thereby increasing the activity of the catalyst 21a. In addition, by making the specific surface area of ​​the carrier 21b 2000m 2 / g or less, the amount of micropores in the support 21b can be suppressed, thereby improving the gas diffusivity in the support 21b. This suppresses the increase in the material transport resistance of the first electrode catalyst layer 20, and as a result, it is possible to suppress the reduction in the output power characteristics of the fuel cell having the first electrode catalyst layer 20.

[0146] In the case where the carrier 21b is formed of carbon, the degree of graphitization of the carrier 21b is preferably within a range of 20% to 80%. When the degree of graphitization of the carrier 21b is 20% or more, the disappearance of the carrier 21b due to the operation and stop of the fuel cell is suppressed, thereby tending to suppress the reduction in the output power characteristics of the fuel cell. On the other hand, when the degree of graphitization of the carrier 21b is 80% or less, the load of the catalyst 21a is stable, and even if the fuel cell is used continuously, the increase in the particle size of the catalyst 21a tends to be suppressed. As a result, the reduction in the activity of the catalyst 21a tends to be suppressed, and the reduction in the output power of the fuel cell tends to be suppressed.

[0147] The shape of the carrier 21b is not particularly limited, and may be, for example, a particle shape or a fiber shape. It should be noted that from the perspective of smoothly transferring the electrons generated on the surface of the catalyst 21a to the outside of the system, the carrier 21b is preferably in a shape capable of supporting the catalyst 21a on its outer surface.

[0148] The average particle size of the carrier 21b is preferably 10 nm or more and 1000 nm or less, and more preferably 10 nm or more and 100 nm or less. By setting the average particle size of the carrier 21b to be 10 nm or more, it is easy to form an electron conduction path in the electrode catalyst layer. In addition, by setting the average particle size of the carrier 21b to be 1000 nm or less, the increase in resistance caused by the increase in the thickness of the first electrode catalyst layer 20 can be suppressed.

[0149] The catalyst-supported particles 21 may also have a hydrophobic coating. In other words, the particles supported by the catalyst 21a may be covered with a hydrophobic coating. In this case, the hydrophobic coating preferably has a film thickness that allows the reaction gas to pass through sufficiently. The film thickness of the hydrophobic coating is preferably less than 40nm. When thicker than this, the supply of the reaction gas to the active site may be hindered. On the other hand, if the hydrophobic coating is less than 40nm, the reaction gas fully passes through the hydrophobic coating, so the catalyst-supported particles can be given hydrophobicity. In addition, the film thickness of the hydrophobic coating covering the catalyst-supported particles 21 is preferably a film thickness that is sufficiently hydrophobic to the generated water. The film thickness of the hydrophobic coating is preferably more than 2nm. The hydrophobic coating has a thickness of more than 2nm, so that the retention of the generated water can be suppressed, thereby suppressing the supply of the reaction gas to the active site from being hindered.

[0150] The hydrophobic film covering the catalyst-supported particles 21 is formed, for example, by a fluorine-based compound having at least one polar group. Examples of polar groups include hydroxyl, alkoxy, carboxyl, ester, ether, carbonate, and amide groups. By the presence of the polar group, the fluorine-based compound can be fixed on the outermost surface of the first electrode catalyst layer 20. From the perspective of hydrophobicity and chemical stability, the part of the fluorine-based compound other than the polar group is preferably a structure consisting of fluorine and carbon. However, as long as the hydrophobic film has sufficient hydrophobicity and chemical stability, it is not limited to this structure.

[0151] <Polymer electrolyte>

[0152] As the polymer electrolyte 22, a substance having proton conductivity is used. As a substance having proton conductivity, for example, a fluorine-based polymer electrolyte and a hydrocarbon-based polymer electrolyte can be listed. As a fluorine-based polymer electrolyte, for example, a fluorine-based polymer electrolyte having a tetrafluoroethylene skeleton represented by Nafion (registered trademark) manufactured by DuPont can be listed. As a hydrocarbon-based polymer electrolyte, for example, sulfonated polyether ketone, sulfonated polyether sulfone, sulfonated polyether ether sulfone, sulfonated polysulfide, and sulfonated polyphenylene can be listed. It should be noted that the polymer electrolyte 22 constituting the first electrode catalyst layer 20 may be only one of the above examples, or a combination of two or more.

[0153] The polymer electrolyte 22 may have a proton donating group. As the proton donating group, for example, a sulfonic acid group can be cited. In the polymer electrolyte 22, the dry weight (equivalent weight EW) per 1 mol of the proton donating group is preferably included in the range of 600 g / mol to 1200 g / mol, and more preferably included in the range of 700 g / mol to 1000 g / mol. By making the equivalent weight EW above 600 g / mol, the reduction in power generation performance caused by overflow tends to be suppressed. By making the equivalent weight EW below 1200 g / mol, the reduction in proton conductivity is suppressed, so in a fuel cell having an electrode catalyst layer, the reduction in power generation performance tends to be suppressed. The dry weight is the weight measured after the polymer electrolyte 22 is dried under reduced pressure at 100°C for more than 1 day.

[0154] For example, when the content of the carrier 21b in the first electrode catalyst layer 20 is set to 100 parts by mass, the content of the polymer electrolyte in the first electrode catalyst layer 20 is preferably 40 parts by mass or more and 140 parts by mass or less. By setting the content of the polymer electrolyte to 40 parts by mass or more, the reduction in proton conductivity caused by the defect in the proton conduction path can be suppressed. As a result, it is easy to ensure the balance between proton conductivity and electron conductivity in the first electrode catalyst layer 20. By setting the content of the polymer electrolyte to 140 parts by mass or less, the catalyst 21a of the catalyst-supported particles 21 can be appropriately exposed. As a result, the catalyst activity of the first electrode catalyst layer 20 is improved.

[0155] <Fibrous substances>

[0156] The fibrous material 23 may be a material that is not affected by the catalyst 21a and the polymer electrolyte 22, preferably a hydrophilic carbon fiber and a polymer fiber. The fibrous material 23 makes it difficult to generate cracks in the electrode catalyst layer, and the durability of the electrode catalyst layer is improved. As hydrophilic carbon fibers, for example, VGCF (Vapor Grown Carbon Fiber) and CNT (Carbon Nano Tube) that impart hydrophilicity can be cited.

[0157] The fibrous substance 23 may contain Lewis acidic or Lewis basic functional groups in the molecular structure of its material. Thus, the polymer electrolyte 22 is easily present around the fibrous substance 23. As the fibrous substance 23 having Lewis acidic functional groups, hydrophilic carbon fibers and polymer fibers having hydroxyl, carbonyl, sulfonic acid and phosphite groups can be listed. As the fibrous substance 23 having Lewis basic functional groups, polymer fibers having imide structures or azole structures can be listed. The proton conductive sites such as sulfonyl groups contained in the polymer electrolyte 22 form hydrogen bonds with the Lewis acidic functional groups in the fibrous substance 23, so that the polymer electrolyte 22 is easily present around the fibrous substance 23. On the other hand, in the case of having basic functional groups in the fibrous substance 23, the acidic proton conductive sites such as sulfonyl groups contained in the polymer electrolyte 22 are combined due to acid and base, so that the polymer electrolyte 22 is easily present around the fibrous substance 23. Compared with hydrogen bonds, the binding force of acid-base bonds is stronger, so the fibrous substance 23 preferably contains Lewis basic functional groups. Among these, the fibrous substance 23 preferably has an azole structure. The azole structure refers to a 5-membered heterocyclic structure containing more than one nitrogen, such as an imidazole structure and an oxazole structure. The substance containing nitrogen atoms preferably has a benzoxazole structure such as a benzimidazole structure and a benzoxazole structure. As specific examples of substances containing nitrogen atoms, polymers such as polybenzimidazole and polybenzoxazole can be listed.

[0158] The shape of the fibrous material 23 is not particularly limited, and may be, for example, a hollow structure or a solid structure. It should be noted that the fibrous material 23 constituting the first electrode catalyst layer 20 may be only one of the above examples, or a combination of two or more.

[0159] The ratio of the number of fluorine atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, sulfur and platinum elements obtained by energy dispersive X-ray spectroscopy in a specific area of ​​the cross section of the first electrode catalyst layer 20 is 0.2 at% or more. By making the ratio of the number of fluorine atoms within such a range, the proton conduction path in the first electrode catalyst layer 20 can be appropriately constructed. As a result, the first electrode catalyst layer 20 has excellent initial power generation performance from the low current density region to the high current density region. The ratio of fluorine atoms is preferably 0.3 at% or more, more preferably 0.4 at% or more. The ratio of fluorine atoms can be 1 at% or less.

[0160] The specific region is a region that contains 50% by area or more of the fibrous substances 23 and does not contain the catalyst-supported particles 21 . Figure 2 Schematic diagram showing an example of a cross section of the first electrode catalyst layer. The cross section of the first electrode catalyst layer is composed of a region R1 containing catalyst-supported particles 21 and a region R2 not containing catalyst-supported particles 21. The region R2 is composed of fibrous substances 23 and a region n not containing fibrous substances 23. Figure 2 In the figure, the specific region (observation region) is represented by A. The shape of the region (observation region) can be a rectangle (including a square), for example, a square of 150 nm×150 nm. In the specific region, the fibrous substance 23 can occupy 100% of the area. The specific region only needs to be one in the cross section.

[0161] As a method for exposing the cross section of the first electrode catalyst layer 20, for example, known methods such as ion milling and ultrathin sectioning can be used. When performing the process of exposing the cross section, in order to reduce damage to the polymer electrolyte 22 constituting the polymer electrolyte membrane 11 and the first electrode catalyst layer 20, it is particularly preferred to use low-temperature ion milling while cooling the first electrode catalyst layer 20.

[0162] The composition ratio of the elements in a specific region can be measured, for example, by performing element mapping using a transmission electron microscope (TEM-EDX) equipped with an energy dispersive X-ray spectrometer. It is appropriate to set the acceleration voltage of the X-rays in EDX to 200 kV. With such an acceleration voltage, the electron beam can be made to penetrate to a thickness of about nm in a specific region, and information on the elements of the fibrous substance 23 and its surroundings can be obtained.

[0163] The polymer electrolyte 22 may be coated with at least a portion of the surface of the fibrous substance 23. As a result, the durability of the obtained membrane electrode assembly is improved, and it tends to exhibit high power generation characteristics even under low humidification conditions. At least a portion of the surface of the fibrous substance 23 coated with the polymer electrolyte 22 can be confirmed by the following method. That is, for a specific area of ​​the cross section of the first electrode catalyst layer 20, element mapping is performed using a transmission electron microscope (TEM-EDX) equipped with an energy dispersive X-ray spectrometer or a scanning transmission electron microscope (STEM-EDX) equipped with an energy dispersive X-ray spectrometer. The element to be measured is set to at least one of fluorine atoms and atoms contained in the fibrous substance 23. With regard to the mapping results, the boundary between the region where the atoms contained in the fibrous substance 23 are not confirmed and the region where the atoms contained in the fibrous substance 23 are not confirmed is taken as the surface of the fibrous substance. When fluorine is confirmed within a range of 10nm from the surface of the fibrous substance, it is judged that at least a portion of the surface of the fibrous substance 23 is coated.

[0164] The thickness of the polymer electrolyte 22 covering the fibrous substance 23 may be the distance from the fluorine detected at the farthest position from the surface of the fibrous substance 23 to the surface of the fibrous substance 23. The thickness of the polymer electrolyte 22 covering the fibrous substance 23 is preferably 3 nm to 30 nm, more preferably 10 nm to 30 nm. By setting the thickness of the coating layer within this range, protons can move on the fibrous substance 23.

[0165] The fibrous material 23 may have the ability to adsorb the polymer electrolyte 22. By adsorbing the polymer electrolyte 22 on the fibrous material 23, the generation of cracks can be suppressed, durability can be improved by high mechanical properties, and high power generation performance can be obtained by forming a proton conduction path through the polymer electrolyte 22. The adsorption of the polymer electrolyte 22 on the fibrous material 23 can be confirmed by a scanning transmission electron microscope (STEM-EDX) equipped with energy dispersive X-ray spectroscopy.

[0166] From the perspective of improving mechanical properties, the adsorption capacity of the fibrous substance 23 for the polymer electrolyte 22 is preferably 10 mg / g or more, more preferably 15 mg / g or more, and can be 30 mg / g or less. The adsorption capacity of the fibrous substance 23 for the polymer electrolyte 22 can be measured by the following method. That is, the fibrous substance 23 is brought into contact with a dispersion in which the polymer electrolyte 22 is dispersed at a predetermined concentration. The fibrous substance 23 is taken out from the dispersion, and the dispersion is filtered with a predetermined filter (for example, a diameter of 0.3 to 0.5 μm). The concentration of the polymer electrolyte contained in the filtrate is measured. Based on the concentration, the amount of polymer electrolyte adsorbed per 1 g of the fibrous substance is calculated.

[0167] The average fiber diameter of the fibrous substance 23 is preferably within a range of 10 nm to 500 nm, more preferably within a range of 10 nm to 300 nm. By making the fiber diameter within this range, the catalysts 21a can be brought close to each other inside the first electrode catalyst layer 20, and a high output power of the fuel cell having the first electrode catalyst layer 20 can be achieved. The average fiber diameter of the fibrous substance 23 can be measured by scanning electron microscope (SEM) observation.

[0168] The average fiber length of the fibrous substance 23 is preferably within a range of 0.7 μm to 40 μm, more preferably within a range of 2 μm to 30 μm. By making the average fiber length within this range, the strength of the first electrode catalyst layer 20 tends to be improved, thereby suppressing the generation of cracks. As a result, the durability of the first electrode catalyst layer 20 to physical impact tends to be improved. In addition, by making the average fiber length within this range, the number of pores formed in the first electrode catalyst layer 20 increases, tending to achieve high output power of the fuel cell. The average fiber length of the fibrous substance 23 can be measured by SEM observation.

[0169] In addition, in a fuel cell, as a result of the battery reaction, the amount of generated water generated in the electrode catalyst layer is proportional to the amount of chemical reaction. Therefore, in the case of power generation at a high current density, the amount of generated water increases. When the generated water cannot be fully discharged outside the electrode catalyst layer, the generated water retained in the electrode catalyst layer may block the diffusion path of the gas. In this case, a phenomenon in which the reaction gas cannot reach the active point and the power generation performance is significantly reduced is overflow (flooding). By using the fibrous substance 23 as the constituent material of the first electrode catalyst layer 20, an appropriate space is ensured in the first electrode catalyst layer 20, and a side that can promote the drainage of the above-mentioned generated water is also provided.

[0170] When the content of the support 21 b in the first electrode catalyst layer 20 is 100 parts by mass, the content of the fibrous substance 23 in the first electrode catalyst layer 20 is preferably 5 parts by mass to 20 parts by mass, and more preferably 5 parts by mass to 10 parts by mass.

[0171] By setting the content of the fibrous substance 23 to 5 parts by mass or more, a network of the fibrous substances 23 can be formed, and the electrode catalyst layer can be easily formed. As a result, the construction of the proton conduction path in the electrode catalyst layer, the construction of the electron conduction path, and the structural reinforcement of the electrode catalyst layer can be fully carried out. As a result, the power generation performance of the fuel cell is improved. By setting the content of the fibrous substance 23 to 20 parts by mass or less, the increase in resistance caused by the increase in the thickness of the first electrode catalyst layer 20 can be suppressed.

[0172] The density of the first electrode catalyst layer 20 is preferably within 1000 mg / cm 3 Above 5000mg / cm 3 The following range is more preferably included in 1500mg / cm 3 Above 4000mg / cm 3 By setting the density of the first electrode catalyst layer 20 to 1000 mg / cm 3 In this way, the amount of catalyst per unit volume can be prevented from decreasing, and thus the output power of the fuel cell can be prevented from decreasing. 3 As a result, the distance between the polymer electrolyte 22 and the fibrous material 23 can be suppressed from increasing, and the electrode catalyst layer 12 tends to be less likely to collapse. As a result, the durability of the first electrode catalyst layer 20 tends to be improved. By setting the density to 5000 mg / cm 3 The internal structure of the electrode catalyst layer 12 does not become too dense, which tends to suppress the reduction of water drainage and gas diffusion. As a result, the first electrode catalyst layer 20 tends to be able to suppress the reduction of output power even at high output power. In addition, when the density is 5000 mg / cm 3 When the value is less than 0.5, the reduction in the bonding strength of the first electrode catalyst layer 20 tends to be suppressed.

[0173] (Second Electrode Catalyst Layer)

[0174] As the second electrode catalyst layer, a known electrode catalyst layer applied to a membrane electrode assembly can be used. As the second electrode catalyst layer, for example, it is different from the first electrode catalyst layer 20 in that it does not contain hydrophilic carbon fibers or high molecular polymer fibers, and other structures can be listed as the same electrode catalyst layer as the first electrode catalyst layer 20.

[0175] It should be noted that the above-mentioned materials used in the constituent components of the first electrode catalyst layer and the second electrode catalyst layer may be the same as or at least partially different from the materials used in the cathode electrode catalyst layer 12C and the anode electrode catalyst layer 12A.

[0176] The ratio (T2 / T1) of the average thickness T2 of the anode side electrode catalyst layer 12A to the average thickness T1 of the cathode side electrode catalyst layer 12C is preferably 1.0 times or more and 2.0 times or less. By making T2 / T1 more than 1.0 times, the catalyst layer thickness is larger than the cathode side electrode catalyst layer 12C, and the volume of water that can be retained becomes more. In this case, the diffusion of water generated at the cathode side electrode catalyst layer 12C to the anode side electrode catalyst layer 12A is promoted, and the gas diffusion resistance in the cathode side electrode catalyst layer 12C is sometimes reduced. As a result, the output power of the fuel cell tends to increase. On the other hand, by making T2 / T1 less than 2.0 times, the thickness of the cathode side electrode catalyst layer 12C becomes smaller, and the mechanical strength of the membrane electrode assembly 100 sometimes becomes smaller. As a result, the cathode side membrane of the polymer electrolyte membrane 11 sometimes breaks, so that the fuel cell cannot work.

[0177] [Solid polymer fuel cell]

[0178] Next, the structure of a solid polymer fuel cell having a membrane electrode assembly 100 is described. Hereinafter, as an example of a solid polymer fuel cell, a single-cell solid polymer fuel cell is described. The solid polymer fuel cell is not limited to a single-cell structure, but may also have a structure in which a plurality of single cells are stacked.

[0179] like Fig.10 As shown, the polymer electrolyte fuel cell 30 includes a membrane electrode assembly 100, a pair of gas diffusion layers 31a, 31b, and a pair of separators 32a, 32b.

[0180] The gas diffusion layers 31a and 31b are layers for uniformly diffusing the reaction gas. The gas diffusion layer 31a is arranged to face the cathode side electrode catalyst layer 12C of the membrane electrode assembly 100. The gas diffusion layer 31b is arranged to face the anode side electrode catalyst layer 12A of the membrane electrode assembly 100. A pair of gas diffusion layers 31a and 31b sandwich the membrane electrode assembly 100 in the thickness direction of the membrane electrode assembly 100. In addition, the cathode side electrode catalyst layer 12C and the gas diffusion layer 31a form an air electrode as a cathode. The anode side electrode catalyst layer 12A and the gas diffusion layer 31b form a fuel electrode as an anode.

[0181] The gas diffusion layers 31a and 31b are made of a material having electron conductivity and gas diffusivity. As the material constituting the gas diffusion layers 31a and 31b, for example, a porous carbon material can be used. Examples of the porous carbon material include carbon cloth, carbon paper, and nonwoven fabric.

[0182] The separators 32a and 32b are components that take out electrons to an external circuit and are disposed outside the gas diffusion layer 31b. The pair of separators 32a and 32b sandwich the membrane electrode assembly 100 and the pair of gas diffusion layers 31a and 31b in the thickness direction of the membrane electrode assembly 100.

[0183] The separators 32a and 32b have gas flow paths 33a and 33b and cooling water flow paths 34a and 34b. The gas flow paths 33a and 33b are flow paths for circulating the reaction gas and are formed on the surfaces of the separators 32a and 32b facing the gas diffusion layers 31a and 31b. The cooling water flow paths 34a and 34b are flow paths for circulating cooling water and are formed on the surfaces of the separators 32a and 32b on the opposite side of the surfaces facing the gas diffusion layers 31a and 31b.

[0184] The separators 32a and 32b are formed of a material having electrical conductivity and gas impermeability. Examples of materials constituting the separators 32a and 32b include carbon materials and metal materials. In addition, the material constituting the separators 32a and 32b is preferably a material having a certain degree of strength and good formability.

[0185] The gas flow path 33a of the separator 32a facing the gas diffusion layer 31a constituting the air electrode is supplied with an oxidant gas as a reaction gas. The oxidant gas is, for example, air or oxygen. The gas flow path 33b of the separator 32b facing the gas diffusion layer 31b constituting the fuel electrode is supplied with a fuel gas as a reaction gas. The fuel gas is, for example, hydrogen.

[0186] In the solid polymer fuel cell 30, a fuel gas containing hydrogen is supplied to the fuel electrode and an oxidant gas containing oxygen is supplied to the air electrode, so that the electrode reactions shown in the following formulas 1 and 2 occur in the fuel electrode and the air electrode to generate electricity. In addition, the solid polymer fuel cell is used in combination with associated equipment such as a gas supply device and a cooling device.

[0187] Fuel electrode: H2→2H + +2e - ···(Formula 1)

[0188] Air electrode: 1 / 2O2+2H + +2e - →H2O···(Formula 2)

[0189] [Method for producing membrane electrode assembly]

[0190] Next, a method for manufacturing the membrane electrode assembly 100 will be described.

[0191] The method for manufacturing the membrane electrode assembly 100 includes a preparation step of preparing a catalyst ink and a formation step of forming an electrode catalyst layer using the catalyst ink.

[0192] (Preparation process)

[0193] In the preparation step, the catalyst ink is prepared by mixing the components constituting the electrode catalyst layer using a dispersion medium.

[0194] The dispersion medium is not particularly limited as long as it can disperse the components constituting the electrode catalyst layer. As the dispersion medium, for example, water, alcohol, ketones or mixtures thereof can be listed. Specifically, alcohols such as water, methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutanol, and tert-butanol can be appropriately used; ketones such as acetone, methyl ethyl ketone, methyl propyl ketone, methyl butyl ketone, methyl isobutyl ketone, methyl amyl ketone, amyl ketone, heptanone, cyclohexanone, methylcyclohexanone, acetonyl acetone, diethyl ketone, dipropyl ketone, and diisobutyl ketone can be appropriately used.

[0195] The catalyst ink may contain a dispersant for dispersing the components constituting the electrode catalyst layer in a favorable manner. Examples of the dispersant include anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants.

[0196] Examples of the anionic surfactant include alkyl ether carboxylates, ether carboxylates, alkanoyl sarcosines, alkanoyl glutamates, acyl glutamates, oleic acid / N-methyltaurine, potassium oleate / diethanolamine salts, alkyl ether sulfate / triethanolamine salts, polyoxyethylene alkyl ether sulfate / triethanolamine salts, amine salts of specially modified polyether ester acids, amine salts of higher fatty acid derivatives, amine salts of specially modified polyester acids, amine salts of high molecular weight polyether ester acids, amine salts of specially modified phosphate esters, and high molecular weight polyester acid aminoamine salts. Aminoamine salts of special fatty acid derivatives, alkylamine salts of higher fatty acids, aminoamine salts of high molecular weight polycarboxylic acids, sodium laurate, sodium stearate, sodium oleate and other carboxylic acid type surfactants; dialkyl sulfosuccinates, dialkyl sulfosuccinates, 1,2-di(alkoxycarbonyl)-1-ethanesulfonates, alkyl sulfonates, alkyl sulfonates, alkane sulfonates, α-olefin sulfonates, linear alkylbenzene sulfonates, alkylbenzene sulfonates, polynaphthalene methanesulfonates, polynaphthalene methanesulfonates, naphthalene sulfonate-formalin condensates, alkylnaphthalenesulfonic acids Sulfonic acid surfactants such as esters, alkanoyl methyl taurine, sodium dodecyl sulfate, sodium hexadecyl sulfate, sodium octadecyl sulfate, sodium oleyl sulfate, sodium dodecyl ether sulfate, sodium alkylbenzene sulfonate, oil-soluble alkylbenzene sulfonate, α-olefin sulfonate; alkyl sulfate ester salts, alkyl sulfate ester salts, alkyl sulfate esters, alkyl ether sulfate esters, polyoxyethylene alkyl ether sulfate esters, alkyl polyethoxy sulfates, polyethylene glycol ether sulfates, alkyl polyoxyethylene sulfates, sulfated oils, highly sulfated oils, etc. Acid ester type surfactants; phosphate ester type surfactants such as (mono or di) alkyl phosphates, (mono or di) alkyl phosphate esters, (mono or di) alkyl phosphate ester salts, alkyl polyoxyethylene phosphate salts, alkyl ether phosphate esters, alkyl polyethoxy / phosphate salts, polyoxyethylene alkyl ethers, alkylphenyl / polyoxyethylene phosphate salts, alkylphenyl ether / phosphate esters, alkylphenyl / polyethoxy / phosphate salts, polyoxyethylene / alkylphenyl / ether phosphate esters, higher alcohol monoester disodium salts, higher alcohol diester disodium salts, dialkyl zinc dithiophosphates, etc.

[0197] Examples of the cationic surfactant include benzyldimethyl{2-[2-(P-1,1,3,3-tetramethylbutylphenoxy)ethoxy]ethyl}ammonium chloride, octadecylamine acetate, tetradecylamine acetate, octadecyltrimethylammonium chloride, tallow trimethylammonium chloride, dodecyltrimethylammonium chloride, coconut trimethylammonium chloride, hexadecyltrimethylammonium chloride, behenyltrimethylammonium chloride, coconut dimethylbenzyl ammonium chloride, tetradecyldimethylbenzyl ammonium chloride, octadecyldimethylbenzyl ammonium chloride, dioleyldimethylammonium chloride, 1-hydroxyethyl-2-tallow imidazoline quaternary ammonium salt, 2-heptadecenyl-hydroxyethyl imidazoline, stearamidoethyldiethylamine acetate, stearamidoethyldiethylamine hydrochloride, triethanolamine monostearate formate, alkylpyridinium salts, higher alkylamine ethylene oxide adducts, polyacrylamide amine salts, modified polyacrylamide amine salts, and perfluoroalkyl quaternary ammonium iodides.

[0198] Examples of the amphoteric surfactant include dimethyl coconut betaine, dimethyl lauryl betaine, sodium laurylaminoethyl glycinate, sodium laurylaminopropionate, stearyl dimethyl betaine, lauryl dihydroxyethyl betaine, amido betaine, imidazolinium betaine, lecithin, sodium 3-[ω-fluoroalkanoyl-N-ethylamino]-1-propanesulfonate, and N-[3-(perfluorooctyl)sulfonamido]propyl-N,N-dimethyl-N-carboxymethylene ammonium betaine.

[0199] Examples of the nonionic surfactant include coconut fatty acid diethanolamide (1:2 type), coconut fatty acid diethanolamide (1:1 type), tallow fatty acid diethanolamide (1:2 type), tallow fatty acid diethanolamide (1:1 type), oleic acid diethanolamide (1:1 type), hydroxyethyl laurylamine, polyethylene glycol laurylamine, polyethylene glycol coconut amine, polyethylene glycol stearylamine, polyethylene glycol tallowamine, polyethylene glycol tallow propylene diamine, polyethylene glycol dioleylamine, dimethyl laurylamine oxide, dimethyl stearylamine oxide, dihydroxyethyl laurylamine oxide, perfluoroalkylamine oxide, polyvinyl pyrrolidone, higher alcohol ethylene oxide adducts, alkylphenol ethylene oxide adducts, fatty acid ethylene oxide adducts, polypropylene glycol ethylene oxide adducts, fatty acid esters of glycerol, fatty acid esters of pentaerythritol, fatty acid esters of sorbitol, fatty acid esters of sorbitan, and fatty acid esters of sucrose.

[0200] Among the above-mentioned surfactants, sulfonic acid-type surfactants such as alkylbenzenesulfonic acid, oil-soluble alkylbenzenesulfonic acid, α-olefinsulfonic acid, sodium alkylbenzenesulfonate, oil-soluble alkylbenzenesulfonate, and α-olefinsulfonate can be preferably used as the dispersant, because they are excellent in the carbon dispersion effect and are unlikely to cause changes in catalyst performance due to dispersant residue.

[0201] The dispersion method in the preparation process is not particularly limited as long as it can disperse the components contained in the catalyst ink, and a known dispersion method can be used. As a known dispersion method, for example, a method using a planetary ball mill, a bead mill or an ultrasonic homogenizer can be cited. In addition, the mixing ratio of each component in the catalyst ink and the dispersion medium can be appropriately selected according to the coating property and the required power generation performance.

[0202] (Formation process)

[0203] In the forming step, the catalyst ink obtained in the preparation step is applied to a substrate, and then a drying process is performed to volatilize the dispersion medium, thereby forming a coating-like electrode catalyst layer. As the substrate, a polymer electrolyte membrane 11, a transfer substrate, or a gas diffusion layer 31a, 31b can be used.

[0204] The coating method for coating the catalyst ink on the substrate is not particularly limited, and a known coating method applied when coating a slurry-like mixture on the substrate with a uniform film thickness can be used. Examples of known coating methods include die coating, rod coating, spray coating, dipping, and screen printing. Among these, die coating is preferably used because the viscosity range of the catalyst ink that can be coated is relatively wide and the coating can be performed with high film thickness uniformity.

[0205] The drying method used in the drying treatment is not particularly limited as long as it is a method that can volatilize the dispersion medium, and known drying methods such as an oven, a hot plate, and a method using far infrared rays can be used. In addition, the drying temperature and drying time in the drying treatment can be appropriately selected according to the material used in the electrode catalyst layer and the substrate.

[0206] When a transfer substrate is used as the substrate, the electrode catalyst layer formed on the transfer substrate is transferred from the transfer substrate to the polymer electrolyte membrane 11. As a transfer method at this time, for example, a transfer method based on thermocompression bonding can be used.

[0207] The transfer substrate is not particularly limited as long as it is a substrate that can demould the formed electrode catalyst layer and transfer it to the polymer electrolyte membrane. As the transfer substrate, for example, a fluororesin film can be used. The transferability of the fluororesin film is excellent. As fluororesins constituting the fluororesin film, for example, ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroperfluoroalkyl vinyl ether copolymer (PFA), polytetrafluoroethylene (PTFE) can be listed.

[0208] When the polymer electrolyte membrane 11 or the transfer substrate is used as the transfer substrate, the membrane electrode assembly 100 can be obtained by providing electrode catalyst layers on both sides of the polymer electrolyte membrane 11. Then, the obtained membrane electrode assembly 100, gas diffusion layers 31a, 31b, and separators 32a, 32b are stacked to obtain a solid polymer fuel cell 30.

[0209] In addition, when the gas diffusion layers 31a and 31b are used as the transfer substrate, the membrane electrode assembly 100 having the gas diffusion layers 31a and 31b can be obtained by stacking the polymer electrolyte membrane 11 and the gas diffusion layers 31a and 31b on which the electrode catalyst layers are formed. Then, by stacking the separators 32a and 32b on the obtained membrane electrode assembly 100, the solid polymer fuel cell 30 can be obtained.

[0210] It should be noted that the electrode catalyst layer manufacturing method when manufacturing the cathode electrode catalyst layer 12C and the electrode catalyst layer manufacturing method when manufacturing the anode electrode catalyst layer 12A may be the same or different.

[0211] Example

[0212] Study 1

[0213] Hereinafter, a membrane electrode assembly according to an embodiment of the present disclosure will be described.

[0214] [Example 1A1]

[0215] In Example 1A1, a carbon catalyst loaded with platinum (TEC10E50E, manufactured by Tanaka Precious Metals Co., Ltd.), water, 1-propanol, a polymer electrolyte (20% Nafion (registered trademark) dispersion, manufactured by Wako Pure Chemical Industries, Ltd.) and a fibrous substance containing nitrogen atoms (polyazole fibers, average fiber diameter of 100-400nm, average fiber diameter distribution peak of 210nm) were mixed. The mixture was dispersed at 300rpm for 60 minutes using a planetary ball mill. At this time, zirconia balls with a diameter of 5mm were added to about one-third of the zirconia container. It should be noted that the catalyst ink was prepared by adjusting the weight of the polymer electrolyte to 100% by weight relative to the weight of the carbon carrier in the carbon catalyst loaded with platinum, the weight of the fibrous substance containing nitrogen atoms to 10% by weight relative to the weight of the carbon carrier in the carbon catalyst loaded with platinum, the proportion of water in the dispersion medium to 50% by weight, and the solid content concentration to 10% by weight.

[0216] Using a slit die coater, the catalyst ink was applied to a single surface of a polymer electrolyte membrane (Nafion (registered trademark) 211, manufactured by DuPont) in a manner of 200 μm in thickness, thereby forming a coating. Next, the polymer electrolyte membrane formed with the coating was placed in a hot air oven at 80°C, and the coating was dried until the coating was not sticky, thereby forming a cathode side electrode catalyst layer. Next, using a slit die coater, the catalyst ink was applied to the surface on the opposite side of the polymer electrolyte membrane in a manner of 50 μm in thickness, thereby forming a coating. Next, the polymer electrolyte membrane formed with the coating was placed in a hot air oven at 80°C, and the coating was dried until the coating was not sticky, thereby forming an anode side electrode catalyst layer. Thus, the membrane electrode assembly of Example 1A1 was obtained. The nitrogen element composition ratio in the catalyst layer is 12%.

[0217] [Example 1A2]

[0218] The membrane electrode assembly of Example 1A2 was obtained by the same method as Example 1A1 except that the amount of the fibrous substance containing nitrogen atoms was set to twice that of Example 1A1 (20% by weight relative to the weight of the carbon support) when preparing the catalyst ink. The nitrogen element composition ratio in the catalyst layer was 20%.

[0219] [Example 1A3]

[0220] The membrane electrode assembly of Example 1A3 was obtained by the same method as Example 1A2 except that the amount of the fibrous substance containing nitrogen atoms was set to 1 / 2 of that of Example 1A1 (5% by weight relative to the weight of the carbon support) when preparing the catalyst ink. The nitrogen element composition ratio in the catalyst layer was 2%.

[0221] [Comparative Example 1A1]

[0222] A membrane electrode assembly of Comparative Example 1A1 was obtained by the same method as in Example 1A1 except that carbon nanofibers (VGCF-H (registered trademark), manufactured by Showa Denko Packaging Co., Ltd.) were added in place of the fibrous substance containing nitrogen atoms when preparing the catalyst ink. The nitrogen element composition ratio in the catalyst layer was 0%.

[0223] [Comparative Example 1A2]

[0224] The membrane electrode assembly of Comparative Example 1A2 was obtained by the same method as in Example 1A1 except that the amount of the fibrous substance containing nitrogen atoms was set to 1 / 10 of that in Example 1A1 (1% by weight relative to the weight of the carbon support) when preparing the catalyst ink. The nitrogen element composition ratio in the catalyst layer was 0.8%.

[0225] [Comparative Example 1A3]

[0226] The membrane electrode assembly of Comparative Example 1A3 was obtained by the same method as in Example 1A1 except that the amount of the fibrous substance containing nitrogen atoms was set to 3 times that of Example 1A1 (30% by weight relative to the weight of the carbon support) when preparing the catalyst ink. The nitrogen element composition ratio in the catalyst layer was 21%.

[0227] Hereinafter, the comparison results of the fibrous material content, power generation performance and durability of the polymer electrolyte fuel cells including the membrane electrode assemblies of Examples 1A1 to 1A3 and the membrane electrode assemblies of Comparative Examples 1A1 to 1A3 will be described.

[0228] [Example 1B1]

[0229] In Example 11, a carbon catalyst loaded with platinum (TEC10E50E, manufactured by Tanaka Precious Metals Industries, Ltd.), water, 1-propanol, a polymer electrolyte (Nafion (registered trademark) dispersion, manufactured by Wako Pure Chemical Industries, Ltd.) and a fibrous substance 15 (polyazole fiber, with an average fiber diameter of 200 nm, a peak value of fiber diameter distribution of 205 nm, and an average fiber length of about 20 μm) were mixed. The mixture was dispersed at 500 rpm for 60 minutes using a planetary ball mill (P-7 manufactured by Fritsch Japan Co., Ltd.). At this time, zirconia balls with a diameter of 5 mm were added to about one-third of the zirconia container. It should be noted that the catalyst ink was prepared by adjusting the mass of the polymer electrolyte to 100% by mass relative to the mass of the carbon particles, the mass of the fibrous substance in the solid component to 1% by mass, the proportion of water in the dispersion medium to 50% by mass, and the solid component concentration to 10% by mass.

[0230] Using a slit die coater, the catalyst ink was applied to a single surface of a polymer electrolyte membrane (Nafion (registered trademark) 211, manufactured by Dupont) in a manner of 100 μm thick, thereby forming a coating. Next, the polymer electrolyte membrane formed with the coating was placed in a hot air oven at 80°C, and the coating was dried until the coating was not sticky, thereby forming a cathode side electrode catalyst layer. Next, using a slit die coater, the catalyst ink was applied to the surface on the opposite side of the polymer electrolyte membrane in a manner of 50 μm thick, thereby forming a coating. Next, the polymer electrolyte membrane formed with the coating was placed in a hot air oven at 80°C, and the coating was dried until the coating was not sticky, thereby forming an anode side electrode catalyst layer. Thus, the membrane electrode assembly of Example 1B1 was obtained.

[0231] [Example 1B2]

[0232] A membrane electrode assembly of Example 1B2 was obtained by the same method as in Example 1B1 except that polyazole fibers having a peak value of 195 nm in fiber diameter distribution were used.

[0233] [Example 1B3]

[0234] A membrane electrode assembly of Example 1B3 was obtained by the same method as in Example 1B1 except that polyazole fibers having a peak value of 225 nm in fiber diameter distribution were used.

[0235] [Example 1B4]

[0236] A membrane electrode assembly of Example 1B4 was obtained by the same method as in Example 1B1 except that polyazole fibers having a peak value of 215 nm in fiber diameter distribution were used.

[0237] [Example 1B5]

[0238] A membrane electrode assembly of Example 1B5 was obtained by the same method as in Example 1B1 except that polyazole fibers having a peak value of 205 nm in fiber diameter distribution were used.

[0239] [Example 1B6]

[0240] A membrane electrode assembly of Example 1B6 was obtained by the same method as in Example 1B1 except that polyazole fibers having a peak value of 185 nm in fiber diameter distribution were used.

[0241] [Example 1B7]

[0242] The catalyst ink was prepared by the same method as in Example 1B6. Using a slit die coater, the catalyst ink was applied to the surface of the PTFE membrane in a manner of 100 μm thick to form a coating. Then, the PTFE membrane with the coating was placed in a hot air oven at 80°C, and the coating was dried until the coating was non-sticky, thereby obtaining a transfer substrate with a cathode side electrode catalyst layer. Next, using a slit die coater, the catalyst ink was applied to the surface of another PTFE membrane in a manner of 50 μm thick to form a coating. Next, the PTFE membrane with the coating was placed in a hot air oven at 80°C, and the coating was dried until the coating was non-sticky, thereby obtaining a transfer substrate with an anode side electrode catalyst layer.

[0243] The transfer substrate with the cathode side electrode catalyst layer and the transfer substrate with the anode side electrode catalyst layer were arranged on the surface and back of the polymer electrolyte membrane (Nafion (registered trademark) 211, manufactured by Dupont) in a manner opposite to each other to form a stack. Then, the stack was hot-pressed at 120°C and 1 MPa to bond the electrode catalyst layers to the surface and back of the polymer electrolyte membrane. Finally, the membrane electrode assembly of Example 1B7 was obtained by peeling off the PTFE membrane from each electrode catalyst layer.

[0244] [Example 1B8]

[0245] A membrane electrode assembly of Comparative Example 1B8 was obtained by the same method as in Example 1B1 except that polyazole fibers having a peak value of 295 nm in fiber diameter distribution were used.

[0246] [Comparative Example 1B1]

[0247] A membrane electrode assembly of Comparative Example 1B1 was obtained by the same method as in Example 1B1 except that the polyazole fiber was not added when preparing the catalyst ink.

[0248] [Comparative Example 1B2]

[0249] A membrane electrode assembly of Comparative Example 1B2 was obtained by the same method as in Example 1B1 except that carbon nanofibers (VGCF (registered trademark)-H, manufactured by Showa Denko K.K.) were added instead of polyazole fibers when preparing the catalyst ink.

[0250] [Measurement of power generation performance]

[0251] In the measurement of power generation performance, according to the "Battery Evaluation and Analysis Procedure" published by the New Energy and Industrial Technology Development Organization (NEDO), a gas diffusion layer, a gasket, and a separator are arranged on both sides of the membrane electrode assembly, and after being fastened in a manner to achieve a predetermined surface pressure, the resulting JARI standard battery is used as an evaluation single cell. Then, the IV measurement described in the "Battery Evaluation and Analysis Procedure" (set as "standard" conditions) and the IV measurement with the relative humidity of the anode and the relative humidity of the cathode both set to RH100% (set as "high humidity" conditions) were implemented.

[0252] It should be noted that regarding the evaluation of power generation performance, the case where the current is 25 A or more when the voltage is 0.6 V under "standard" conditions, and the current is 30 A or more when the voltage is 0.6 V under "high humidity" conditions is set as "A", and on the other hand, the case where the above current values ​​are not met is set as "B".

[0253] [Determination of durability A and B]

[0254] In the durability measurement, the same single cell as the evaluation single cell used for the power generation performance measurement was used as the evaluation single cell, and the durability was measured by the humidity cycle test described in the above-mentioned "Battery Evaluation and Analysis Procedure".

[0255] It should be noted that in the evaluation of durability A, the case where the hydrogen cross leak current after 8000 cycles is less than 10 times the initial value is set as "A", and the case where it is more than 10 times is set as "B". In addition, in the evaluation of durability B, the case where the current after 10,000 cycles is more than 50% of the initial value is set as "A", and the case where it is less than 50% is set as "B".

[0256] [Measurement of fiber diameter distribution peak]

[0257] The fiber diameter distribution peak is measured by observing the cross section of the membrane electrode assembly using a scanning electron microscope (SEM). Specifically, a small piece of the membrane electrode assembly 1 is first bonded to a metal plate, and the cross section sample preparation device IB-19520CCP made by NEPCO is used to expose the cross section of the electrode catalyst layer. Next, the exposed cross section is observed at an observation magnification of 50,000 times using the FE-SEM S-4800 manufactured by Hitachi High-Technologies Corp., and the fiber diameter of the polymer fiber in the field of view is measured using the diameter measurement function of the circle. In the case where the fiber is beveled, the diameter of the true circle obtained by fitting along the minor axis is measured. In addition, in the case where the surface of the fiber is exposed instead of the cross section of the fiber, the width of the fiber orthogonal to the major axis of the exposed fiber is measured. It is implemented unbiasedly at multiple observation points in the catalyst layer, and a data set of the fiber diameters of 30 polymer fibers is obtained. Using this data set, the grade width is set to 10nm to make a frequency distribution table, and a histogram representing the fiber diameter distribution is obtained. The median value of the class with the highest frequency in the histogram is obtained as the peak value of the fiber diameter distribution of the polymer fiber.

[0258] [Measurement of Nitrogen Atomic Ratio in a Specific Region of a Cross Section]

[0259] The ratio of the number of nitrogen atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, sulfur and platinum elements obtained by energy dispersive X-ray spectroscopy in a specific area of ​​the electrode catalyst layer was measured. Specifically, first, a cross-section of the electrode catalyst layer was obtained by low-temperature ion milling while processing while cooling the electrode catalyst layer. Next, a transmission electron microscope (TEM-EDX) equipped with energy dispersive X-ray spectroscopy was used to perform element mapping of a specific area of ​​the cross-section, obtain the element ratio of each element, and calculate the nitrogen atomic ratio. The acceleration voltage was set to 200 kV. The specific area is 150 nm × 150 nm in size, which is a range in which the fibrous material containing nitrogen atoms occupies more than 50% of the field of view area.

[0260] [Comparison results]

[0261] The conditions and results of each embodiment and comparative example are shown in Table 1.

[0262] [Table 1]

[0263]

[0264] As shown in Table 1, the nitrogen atomic ratio in the electrode catalyst layer of Examples 1A and 1B was 2% or more and 20% by weight or less. Moreover, the power generation performance and durability A and B were both "A". That is, in Examples 1A and 1B, a membrane electrode assembly capable of constituting a fuel cell having excellent power generation performance and durability was obtained.

[0265] On the other hand, in Comparative Examples 1A1 to 1A3 and 1B1 to 1B2, the nitrogen atomic ratio in the electrode catalyst layer is outside the range of 2 at% to 20 at%. Moreover, at least one of the power generation performance and durability A and B is "B". That is, when the nitrogen element composition ratio in the electrode catalyst layer is outside the above range, at least one of the power generation performance and durability is reduced.

[0266] Therefore, it can be seen that when the nitrogen element composition ratio in the electrode catalyst layer is 2 at % or more and 20 at % or less, a membrane electrode assembly capable of constituting a fuel cell having a more excellent power generation performance can be obtained.

[0267] As shown in Table 1, in the examples where the peak value of the fiber diameter distribution of the polymer fiber was 150 nm or more and 250 nm or less, the characteristics were further improved.

[0268] Study 2

[0269] Next, the above-mentioned embodiment of the second invention group will be described in more detail with reference to Examples and Comparative Examples. It should be noted that the present disclosure is not limited to the configurations described in the Examples section.

[0270] [Manufacturing of membrane electrode assembly]

[0271] (Example 2A1)

[0272] Catalyst ink was prepared by dispersing a mixed solution of catalyst-supported particles, a polymer electrolyte, a fibrous substance and a dispersion medium. The amount of the polymer electrolyte was 70 parts by mass relative to 100 parts by mass of the carrier contained in the catalyst-supported particles. The amount of the fibrous substance was 5 parts by mass relative to 100 parts by mass of the carrier contained in the catalyst-supported particles. The amount of the dispersion medium was set to an amount such that the solid content concentration of the catalyst ink was 10% by mass. A zirconia ball with a diameter of 3 mm and a planetary ball mill were used to perform a dispersion treatment for 60 minutes at a rotation speed of 600 rpm. The details of each component used in the catalyst ink are as follows.

[0273] Catalyst supported particles: Platinum supported carbon catalyst (supporting density 50 mass %)

[0274] Polymer electrolyte: Fluorine-based polymer electrolyte (Nafion (registered trademark), manufactured by Wako Pure Chemical Industries, Ltd.) dispersion containing proton-donating groups, dry weight per 1 mol of proton-donating groups: 1100 g / mol)

[0275] Fibrous material: High molecular weight polymer fiber containing azole structure (average fiber diameter 300nm×average fiber length 10μm)

[0276] Dispersion medium: a mixture of water and 1-propanol (mass of water:mass of 1-propanol = 1:1)

[0277] Next, the prepared catalyst ink was applied to one side of a polymer electrolyte membrane (Nafion (registered trademark) 211 manufactured by Dupont) using a die coater to form a 50 mm long x 50 mm wide quadrilateral coating. The amount of catalyst ink applied was set so that the platinum loading was 0.3 mg / cm 2 Then, a drying treatment was performed using an oven at 80° C. to volatilize the dispersion medium contained in the coating film, thereby forming a cathode-side electrode catalyst layer.

[0278] Next, the prepared catalyst ink was applied to the surface of the polymer electrolyte membrane opposite to the surface on which the cathode electrode catalyst layer was formed, forming a 50 mm long x 50 mm wide square coating. The amount of catalyst ink applied was set so that the platinum loading amount was 0.1 mg / cm 2 Then, a drying treatment was performed in an oven at 80° C. to volatilize the dispersion medium contained in the coating film to form an anode-side electrode catalyst layer, thereby obtaining a membrane electrode assembly.

[0279] (Example 2A2)

[0280] A membrane electrode assembly was obtained in the same manner as in Example 2A1 except that the amount of the fibrous substance added was 20 parts by mass based on 100 parts by mass of the carrier contained in the catalyst-supported particles when preparing the catalyst slurry.

[0281] (Comparative Example 2A1)

[0282] A membrane electrode assembly was obtained in the same manner as in Example 2A1 except that the amount of the fibrous substance added was 30 parts by mass based on 100 parts by mass of the carrier contained in the catalyst-supporting particles when preparing the catalyst slurry.

[0283] (Comparative Example 2A2)

[0284] A membrane electrode assembly was obtained by the same method as in Example 2A1 except that the type of the fibrous substance was changed. The details of the fibrous substance used in Comparative Example 2A2 are as follows.

[0285] Fibrous material: non-hydrophilized carbon fiber (VGCF-H (registered trademark) manufactured by Showa Denko K.K., average fiber length: 6 μm, average fiber diameter: 150 nm)

[0286] (Comparative Example 2A3)

[0287] A membrane electrode assembly was obtained in the same manner as in Comparative Example 2A2 except that the amount of the fibrous substance added was 20 parts by mass based on 100 parts by mass of the carrier contained in the catalyst-supported particles when preparing the catalyst slurry.

[0288] (Comparative Example 2A4)

[0289] An electrode assembly was obtained in the same manner as in Comparative Example 2A2 except that the amount of the fibrous substance added was 30 parts by mass based on 100 parts by mass of the carrier contained in the catalyst-supported particles when preparing the catalyst slurry.

[0290] (Example 2B1)

[0291] 100 mg of catalyst-loaded particles (platinum-loaded carbon, trade name: "TEC10E50E", manufactured by Tanaka Precious Metals Industries, Ltd., platinum content: 50 mg, carbon content: 50 mg) and 5 mg of fibrous material (polymer fibers containing an azole structure, average fiber diameter 300 nm × average fiber length 10 μm) were placed in a container. 1.0 g of water was added to the container and mixed, and a dispersion (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) was further added to the container and stirred. The dispersion contained 1.0 g of 1-propanol and 60 mg of a polymer electrolyte (Nafion (registered trademark), containing proton-donating groups, dry weight per 1 mole of proton-donating groups: 1100 g / mol). Thus, a catalyst slurry was obtained. The catalyst slurry was applied to both sides of the polymer electrolyte membrane by die coating and dried to obtain a membrane electrode assembly.

[0292] (Example 2B2)

[0293] A membrane electrode assembly was obtained by the same method as in Example 2B1 except that hydrophilic carbon fibers (average fiber diameter: 150 nm×average fiber length: 30 μm) were used as the fibrous material when preparing the catalyst slurry.

[0294] (Example 2B3)

[0295] A membrane electrode assembly was obtained by the same method as in Example 2B1 except that the blending amount of the high molecular weight polymer fibers containing an azole structure was changed to 15 mg when preparing the catalyst slurry.

[0296] (Example 2B4)

[0297] A membrane electrode assembly was obtained by the same method as in Example 2B1 except that the blending amount of the high molecular weight polymer fiber containing an azole structure was changed to 0.5 mg when preparing the catalyst slurry.

[0298] (Example 2B5)

[0299] When preparing the catalyst slurry, a dispersion containing 1.0 g of 1-propanol and 70 mg of a polymer electrolyte (Nafion (registered trademark), containing proton-donating groups, dry weight per 1 mol of proton-donating groups: 1300 g / mol) was used as a dispersion liquid. Except for this, a membrane electrode assembly was obtained by the same method as Example 2B1.

[0300] (Example 2B6)

[0301] When preparing the catalyst slurry, a dispersion containing 1.0 g of 1-propanol and 30 mg of a polymer electrolyte (Nafion (registered trademark), containing proton-donating groups, dry weight per 1 mol of proton-donating groups: 500 g / mol) was used as a dispersion liquid. Except for this, a membrane electrode assembly was obtained by the same method as Example 2B1.

[0302] (Example 2B7)

[0303] A membrane electrode assembly was obtained by the same method as in Example 2B1 except that the average fiber diameter of the fibrous substance was 100 nm and the average fiber length was 0.5 μm.

[0304] (Example 2B8)

[0305] A membrane electrode assembly was obtained by the same method as in Example 2B1 except that the average fiber diameter of the fibrous substance was 200 nm and the average fiber length was 50 μm.

[0306] (Example 2B9)

[0307] A membrane electrode assembly was obtained by the same method as in Example 2B1 except that the average fiber diameter of the fibrous substance was 5 nm and the average fiber length was 8 μm.

[0308] (Example 2B10)

[0309] A membrane electrode assembly was obtained by the same method as in Example 2B1 except that the average fiber diameter of the fibrous substance was 1000 nm and the average fiber length was 30 μm.

[0310] (Example 2B11)

[0311] A dispersion (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) and 1.0 g of water were added to a container and stirred. The dispersion contained 5 mg of a fibrous substance (polymer fibers containing an azole structure, with an average fiber diameter of 300 nm × fiber length of 10 μm) and 60 mg of a polymer electrolyte (Nafion (registered trademark), containing proton-donating groups, dry weight per 1 mol of proton-donating groups: 1100). Then, 100 mg of catalyst-supported particles (platinum-supported carbon, trade name "TEC10E50E", manufactured by Tanaka Precious Metals Industries, Ltd., platinum amount: 50 mg, carbon amount: 50 mg) and 1.0 g of 1-propanol were added to a container and stirred. Thus, a catalyst slurry was obtained. The catalyst slurry was applied to both sides of the polymer electrolyte membrane by die coating and dried to obtain a membrane electrode assembly.

[0312] (Comparative Example 2B1)

[0313] A membrane electrode assembly was obtained by the same method as in Example 2B2 except that hydrophobic carbon fibers were used as the fibrous material.

[0314] (Comparative Example 2B2)

[0315] A membrane electrode assembly was obtained by the same method as in Comparative Example 2B1 except that the fibrous material was not blended when preparing the catalyst slurry.

[0316] (Example 2C1)

[0317] Catalyst ink was prepared by dispersing a mixed solution containing catalyst-supported particles, a polymer electrolyte, a fibrous substance, and a dispersion medium. The amount of the polymer electrolyte was set to 80 parts by mass relative to 100 parts by mass of the carrier contained in the catalyst-supported particles. The amount of the fibrous substance was set to 10 parts by mass relative to 100 parts by mass of the carrier contained in the catalyst-supported particles. The amount of the dispersion medium was set to an amount such that the solid content concentration of the catalyst ink was 12% by mass. A bead mill was used for the dispersion. The details of each component used in the catalyst ink are as follows.

[0318] Catalyst supported particles: platinum-supported carbon catalyst (trade name: "TEC10E50E", manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.)

[0319] Polymer electrolyte: Fluorine-based polymer electrolyte (Nafion (registered trademark) dispersion, manufactured by Wako Pure Chemical Industries, Ltd.)

[0320] Fibrous material: polymer fiber with sulfonic acid group attached, average fiber diameter: 300nm

[0321] Dispersion medium: a mixture of water and 1-propanol (mass of water:mass of 1-propanol = 1:1)

[0322] The prepared catalyst ink was directly applied to both surfaces of a polymer electrolyte membrane (Nafion 211 (registered trademark), manufactured by Dupont) using a slot die coater and dried to form an electrode catalyst layer, thereby obtaining a membrane electrode assembly.

[0323] (Example 2C2)

[0324] A membrane electrode assembly was obtained by the same procedure as in Example 2C1 except that high molecular polymer fibers (sulfonic acid groups were added, average fiber diameter: 15 nm) were used as the fibrous material.

[0325] (Example 2C3)

[0326] A membrane electrode assembly was obtained by the same procedure as in Example 2C1 except that high molecular polymer fibers (sulfonic acid groups were added, average fiber diameter: 0.8 μm) were used as the fibrous material.

[0327] (Example 2C4)

[0328] A membrane electrode assembly was obtained by the same procedure as in Example 2C1 except that high molecular polymer fibers (amino groups added, average fiber diameter: 300 nm) were used as the fibrous material.

[0329] (Example 2C5)

[0330] A membrane electrode assembly was obtained by the same procedure as in Example 2C1 except that high molecular polymer fibers (hydroxyl groups added, average fiber diameter: 300 nm) were used as the fibrous material.

[0331] (Comparative Example 2C1)

[0332] A membrane electrode assembly was obtained by the same procedure as in Example 2C1 except that the fibrous material was not added when preparing the catalyst slurry.

[0333] (Comparative Example 2C2)

[0334] A membrane electrode assembly was obtained by the same procedure as in Example 2C1 except that high molecular polymer fibers (having no Lewis acidic or Lewis basic functional groups, average fiber diameter: 300 nm) were used as the fibrous material.

[0335] (Comparative Example 2C3)

[0336] A membrane electrode assembly was obtained by the same procedure as in Example 2C1 except that high molecular polymer fibers (having no Lewis acidic or Lewis basic functional groups, average fiber diameter: 15 nm) were used as the fibrous material.

[0337] (Comparative Example 2C4)

[0338] A membrane electrode assembly was obtained by the same procedure as in Example 2C1 except that high molecular polymer fibers (having no Lewis acidic or Lewis basic functional groups, average fiber diameter: 0.8 μm) were used as the fibrous material.

[0339] [Measurement of the Amount of Polymer Electrolyte Around the Fibrous Material in the Electrode Catalyst Layer]

[0340] (Examples 2A1, 2A2, 2B1 to 2B11, Comparative Examples 2A1 to 2A4, 2B1, 2B2)

[0341] The ratio of the number of fluorine atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, sulfur and platinum elements obtained by energy dispersive X-ray spectroscopy in a specific area of ​​the electrode catalyst layer was measured. Specifically, first, a cross-section of the electrode catalyst layer was obtained by low-temperature ion milling while processing while cooling the electrode catalyst layer. Next, a transmission electron microscope (TEM-EDX) equipped with energy dispersive X-ray spectroscopy was used to perform element mapping of a specific area of ​​the cross-section, obtain the element ratio of each element, and calculate the fluorine atomic ratio. The acceleration voltage was set to 200 kV. The specific area is 150 nm × 150 nm in size, which is a range where the fibrous material occupies more than 50% of the area of ​​the field of view.

[0342] [Evaluation of initial power generation performance]

[0343] (Examples 2A1, 2A2, 2B1 to 2B11, 2C1 to 2C5, Comparative Examples 2A1 to 2A4, 2B1, 2C2 to 2C4)

[0344] For the membrane electrode assembly, carbon paper as a gas diffusion layer was pasted in a manner of sandwiching the membrane electrode assembly to produce a sample. Each sample was set in a power generation evaluation cell, and the current and voltage were measured using a fuel cell measuring device. The cell temperature during the measurement was set to 80°C. The humidification conditions were set to: the relative humidity on the anode side was 90% RH, and the relative humidity on the cathode side was 30% RH. In addition, hydrogen was used as the fuel gas and air was used as the oxidant gas. At this time, hydrogen was allowed to flow at a flow rate at which the hydrogen utilization rate became 80%, and air was allowed to flow at a flow rate at which the oxygen utilization rate became 40%. It should be noted that the back pressure was set to 50 kPa.

[0345] The power generation performance of each membrane electrode assembly is shown in Tables 2 to 4. In Tables 2 to 4, as an index of power generation performance at low current density, "A" is used to indicate that the current density is 0.2 A / cm 2 When the voltage is 0.8 V or more, "B" indicates that the voltage is less than 0.8 V. Similarly, as an indicator of power generation performance at a high current density, "A" indicates that the current density is 1.5 A / cm 2 When the voltage is 0.65V or more, "B" is used to indicate that the voltage is less than 0.65V.

[0346] [Evaluation of covering status]

[0347] (Examples 2B1 to 2B11, Comparative Example 2B1)

[0348] Whether the fibrous material of the electrode catalyst layer is covered by a coating layer composed of a polymer electrolyte was evaluated. Specifically, first, a cross-section of the electrode catalyst layer was obtained by low-temperature ion milling while cooling the electrode catalyst layer. Then, a transmission electron microscope (TEM-EDX) equipped with an energy dispersive X-ray spectrometer was used to map the elements of a specific area of ​​the cross-section. The elements of the measured object were set to carbon, nitrogen, oxygen, fluorine, sulfur and platinum. The acceleration voltage was set to 200kV. The measurement area was 150nm×150nm in size, which was a range where the fibrous material occupied more than 50% of the field of view. When fluorine was detected within a range of 10nm from the surface of the fibrous material, it was judged that the fibrous material was covered by a coating layer composed of a polymer electrolyte. When fluorine was not detected within a range of 10nm from the surface of the fibrous material, it was judged that the fibrous material was not covered by a coating layer composed of a polymer electrolyte. In addition, the distance between the fluorine detected at the farthest position from the surface of the fibrous material and the fibrous material was taken as the thickness of the coating layer. The presence or absence of the coating layer and its thickness were evaluated according to the following evaluation criteria. The results are shown in Table 3.

[0349] <Evaluation Criteria>

[0350] D: No coating layer.

[0351] C: It has a coating layer, and the thickness of the coating layer is less than 3 nm.

[0352] B: A coating layer is present, and the thickness of the coating layer is 3 nm or more and less than 10 nm.

[0353] A: A coating layer is present, and the coating layer has a thickness of 10 nm to 30 nm.

[0354] [Measurement of the adsorption amount of polymer electrolyte]

[0355] (Examples 2C1 to 2C5, Comparative Examples 2C1 to 2C4)

[0356] The fibrous material was brought into contact with a dispersion containing a polymer electrolyte (polymer electrolyte concentration: 1 mass %). The fibrous material was taken out from the dispersion and the dispersion was filtered through a filter (diameter: 0.4 μm). The concentration of the polymer electrolyte contained in the filtrate was measured. Based on the concentration, the amount of polymer electrolyte adsorbed per 1 g of the fibrous material was calculated. The results are shown in Table 4.

[0357] [Evaluation of cracks and peeling]

[0358] (Examples 2A1, 2A2, 2C1 to 2C5, Comparative Examples 2A1 to 2A4, 2C1 to 2C4)

[0359] The electrode catalyst layer was evaluated for cracks and peeling. In order to confirm the presence of cracks, the amount of light transmitted through the electrode catalyst layer was measured. 2 ) was converted to a binary image. When the ratio (B / W) of the number of black pixels (B) representing the non-transmitting area to the number of white pixels (W) representing the transmitting area was 10,000 or more, it was judged that there was no crack; when it was less than 10,000, it was judged that there was a crack. The peeling between the electrode catalyst layer and the polymer electrolyte membrane was observed using a SEM (scanning electron microscope). The results are shown in Tables 2 and 4.

[0360] [Table 2]

[0361]

[0362] [Table 3]

[0363]

[0364] [Table 4]

[0365]

[0366] It can be seen from the results of each embodiment and comparative example that even if the amount of fibrous material added is the same, power generation performance cannot be obtained when the amount of polymer electrolyte containing fluorine atoms around the fibrous material is low. The inventors have speculated on the mechanism of the excellent initial power generation performance of the membrane electrode assembly obtained in each embodiment from low current density to high current density. That is, in order to obtain the structural strength of the electrode catalyst layer, a part of the polymer electrolyte is adsorbed on the periphery of the fibrous material that constructs a three-dimensional network in the electrode catalyst layer. Thus, a three-dimensional proton conduction path is constructed. As a result, the initial power generation performance from low current density to high current density is improved.

[0367] As apparent from the above description, according to this embodiment, in the electrode catalyst layer including the fibrous substance, the presence of a certain amount or more of the polymer electrolyte around the fibrous substance can improve the initial power generation performance from the low current density region to the high current density region.

[0368] The gist of the present disclosure lies in the following [1] to

[12] .

[0369] [1] An electrode catalyst layer, which is an electrode catalyst layer bonded to a polymer electrolyte membrane, comprising:

[0370] catalyst,

[0371] Fluorinated polymer electrolytes, and

[0372] Fibrous material,

[0373] The ratio of the number of fluorine atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, sulfur and platinum elements obtained by energy dispersive X-ray spectroscopy in a specific area of ​​the cross-section of the electrode catalyst layer is greater than 0.2 at %, and the specific area is an area containing more than 50 area % of fibrous material and no catalyst.

[0374] [2] The electrode catalyst layer according to [1], wherein the fibrous substance has an azole structure.

[0375] [3] The electrode catalyst layer according to [1] or [2], wherein

[0376] comprising: a carrier that supports a catalyst and together with the catalyst constitutes catalyst-supported particles,

[0377] When the content of the carrier is 100 parts by mass, the content of the fibrous substance is 5 parts by mass or more and 20 parts by mass or less.

[0378] The specific area is an area that does not contain a carrier.

[0379] [4] The electrode catalyst layer according to any one of [1] to [3], wherein the polymer electrolyte covers at least a portion of the surface of the fibrous substance.

[0380] [5] The electrode catalyst layer according to [4], wherein the thickness of the polymer electrolyte covering the fibrous substance is 3 nm to 30 nm.

[0381] [6] The electrode catalyst layer according to any one of [1] to [5], wherein

[0382] The polymer electrolyte contains proton-donating groups.

[0383] The dry weight per 1 mol of the proton-donating groups of the polymer electrolyte is 600 g / mol or more and 1200 g / mol or less.

[0384] [7] The electrode catalyst layer according to any one of [1] to [6], wherein the average fiber length of the fibrous substance is 0.7 μm to 40 μm.

[0385] [8] The electrode catalyst layer according to any one of [1] to [7], wherein the average fiber diameter of the fibrous substance is 10 nm to 500 nm.

[0386] [9] The electrode catalyst layer according to any one of [1] to [8], wherein the fibrous material has a capability of adsorbing a polymer electrolyte.

[0387]

[10] The electrode catalyst layer according to [9], wherein the fibrous material has an adsorption capacity for the polymer electrolyte of 10 mg / g or more.

[0388]

[11] A membrane electrode assembly comprising:

[0389] Polymer electrolyte membranes, and

[0390] The electrode catalyst layer according to any one of [1] to

[10] ,

[0391] The electrode catalyst layer is joined to the polymer electrolyte membrane.

[0392]

[12] A solid polymer fuel cell comprising:

[0393]

[11] the membrane electrode assembly,

[0394] a pair of gas diffusion layers sandwiching the membrane electrode assembly in a thickness direction of the membrane electrode assembly, and

[0395] A pair of separators sandwich the membrane electrode assembly and the pair of gas diffusion layers in the thickness direction of the membrane electrode assembly.

[0396] Explanation of symbols

[0397] 1, 100 ... membrane electrode assembly, 2C ... oxygen electrode, 2A ... fuel electrode, 3, 30 ... solid polymer fuel cell, 4 ... gap, 10, 10C, 10A ... electrode catalyst layer, 11 ... polymer electrolyte membrane, 12 ... catalyst substance, 12C ... cathode side electrode catalyst layer, 12A ... anode side electrode catalyst layer, 13 ... conductive support, 14 ... polymer electrolyte, 15 ... fibrous substance containing nitrogen atoms, 16C, 16A ... gasket, 17C, 17A, 31a, 31b ... gas diffusion layer, 18C, 18A, 32a, 32b ... separator, 19C, 19A, 33a, 33b ... gas flow path, 20C, 20A, 34a, 34b ... cooling water flow path. 20 ... first electrode catalyst layer, 21 ... catalyst-supported particles, 21a ... catalyst, 21b ... carrier, 22 ... polymer electrolyte, 23 ... fibrous substance.

Claims

1. An electrode catalyst layer, which is an electrode catalyst layer for a solid polymer fuel cell, characterized in that: The electrode catalyst layer comprises: a catalyst substance, a conductive carrier supporting the catalyst substance, a polymer electrolyte, and a fibrous substance containing nitrogen atoms. The ratio of the number of nitrogen atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, sulfur and platinum elements obtained by energy dispersive X-ray spectroscopy in a specific area of ​​the cross-section of the electrode catalyst layer is greater than 2 at % and less than 20 at %, and the specific area is an area that contains more than 50 area % of the fibrous material containing nitrogen atoms and does not contain the catalyst substance and the conductive carrier.

2. The electrode catalyst layer according to claim 1, characterized in that The average fiber diameter of the fibrous material containing nitrogen atoms is 50 nm or more and 400 nm or less.

3. The electrode catalyst layer according to claim 1 or 2, wherein: The fibrous material containing nitrogen atoms is a polymer fiber.

4. The electrode catalyst layer according to claim 3, wherein: The fibrous substance containing nitrogen atoms has an azole structure.

5. The electrode catalyst layer according to any one of claims 1 to 4, wherein The peak value of the fiber diameter distribution of the fibrous material containing nitrogen atoms is 150 nm or more and 250 nm or less.

6. The electrode catalyst layer according to any one of claims 1 to 5, characterized in that The content of the fibrous substance containing nitrogen atoms in the electrode catalyst layer is 1 wt % to 10 wt %.

7. The electrode catalyst layer according to any one of claims 1 to 6, characterized in that The thickness of the electrode catalyst layer is not less than 2 μm and not more than 10 μm.

8. A membrane electrode assembly, characterized in that: The electrode catalyst layer according to any one of claims 1 to 7 is provided on at least one surface of a polymer electrolyte membrane.

9. A solid polymer fuel cell, characterized in that: A membrane electrode assembly according to claim 8 is provided.

10. An electrode catalyst layer, which is an electrode catalyst layer bonded to a polymer electrolyte membrane, comprising: catalyst, Fluorinated polymer electrolytes, and Fibrous material, The ratio of the number of fluorine atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, sulfur and platinum elements obtained by energy dispersive X-ray spectroscopy in a specific area of ​​the cross-section of the electrode catalyst layer is greater than 0.2 at %, and the specific area is an area containing more than 50 area % of the fibrous substance and does not contain the catalyst.

11. The electrode catalyst layer according to claim 10, wherein The fibrous substance has an azole structure.

12. The electrode catalyst layer according to claim 10 or 11, wherein comprising: a carrier that supports the catalyst and together with the catalyst constitutes catalyst-supported particles, When the content of the carrier is 100 parts by mass, the content of the fibrous substance is 5 parts by mass or more and 20 parts by mass or less. The specific region is a region that does not include the carrier.

13. The electrode catalyst layer according to any one of claims 10 to 12, wherein: The polymer electrolyte covers at least a portion of the surface of the fibrous substance.

14. The electrode catalyst layer according to claim 13, wherein The thickness of the polymer electrolyte covering the fibrous substance is not less than 3 nm and not more than 30 nm.

15. The electrode catalyst layer according to any one of claims 10 to 14, wherein The polymer electrolyte contains a proton donating group, The dry weight of the proton-donating groups in the polymer electrolyte is 600 g / mol or more and 1200 g / mol or less per 1 mol.

16. The electrode catalyst layer according to any one of claims 10 to 15, wherein The average fiber length of the fibrous material is 0.7 μm or more and 40 μm or less.

17. The electrode catalyst layer according to any one of claims 10 to 16, wherein The average fiber diameter of the fibrous material is not less than 10 nm and not more than 500 nm.

18. The electrode catalyst layer according to any one of claims 10 to 17, wherein The fibrous material has the ability to adsorb the polymer electrolyte.

19. The electrode catalyst layer according to claim 18, wherein The fibrous material has an adsorption capacity of 10 mg / g or more for the polymer electrolyte.

20. A membrane electrode assembly comprising: Polymer electrolyte membranes, and The electrode catalyst layer according to any one of claims 10 to 19, The electrode catalyst layer is joined to the polymer electrolyte membrane.

21. A solid polymer fuel cell comprising: The membrane electrode assembly according to claim 20, a pair of gas diffusion layers sandwiching the membrane electrode assembly in a thickness direction of the membrane electrode assembly, and A pair of separators sandwich the membrane electrode assembly and the pair of gas diffusion layers in a thickness direction of the membrane electrode assembly.

Citation Information

Cited By

  • Cathode catalyst slurry introduced with serine polybenzimidazole and preparation method of cathode catalyst slurry

    CN121506967A

  • A cathode catalyst slurry incorporating serine polybenzimidazole and a method of making the same

    CN121506967B