Cooking container and cooking container manufacturing method
By using water-based ceramic coatings and protective layers of titanium elements in a non-stick pan, and forming a raised portion in combination with the etching process, the corrosion resistance and adhesion problems of non-stick pan are solved, and better corrosion resistance and non-stick effects are achieved. .
Patent Information
- Application Number
- CN202411356600.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-12-03
AI Technical Summary
The corrosion resistance of existing non-stick pans is weak, which leads to rust easily in salt spray experiments, affecting service life. At the same time, increasing the thickness of the non-stick layer will reduce the adhesion firmness.
Using a protective layer containing aqueous ceramic coatings and corrosion-resistant components, especially the addition of titanium elements, adjust the corrosion resistance and adhesion of the protective layer, and form protrusions through the etching process to improve non-stickness, while using ceramic coatings to reduce Sintering temperature to cover the protrusions.
It significantly improves the corrosion resistance and non-stickness of the cooking container, extends the service life, and improves the aesthetics and physical non-stick effect of the container.
Smart Images

Figure CN119055093A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of cooking utensils, and in particular to a cooking container and a manufacturing method thereof. Background Art
[0002] Cooking containers (such as woks, frying pans, pressure cooker inner pots, steamers, etc.) are commonly used tools in the kitchen cooking process. Food is processed by putting food into the cooking cavity and then stir-frying it.
[0003] Based on the demand for non-stick properties, there are non-stick pans on the market. The principle of non-stick pans is to spray a layer of non-stick coating on the pan base and use the non-stick properties of the non-stick coating to achieve non-stick. Although the non-stick layer has a good non-stick effect, the corrosion resistance of the non-stick layer is weak. For example, rust spots may appear in some areas of the base under salt spray tests, thus affecting the service life of the non-stick pan. Although better corrosion resistance can be achieved by increasing the thickness of the non-stick layer, as the thickness of the non-stick layer increases, the adhesion firmness of the non-stick layer will also decrease accordingly. Therefore, how to increase the corrosion resistance of non-stick pans is a relatively important technical problem in the industry. Summary of the invention
[0004] In view of the above problems, the present application provides a cooking container to improve the protection of the base.
[0005] On the one hand, the present application provides a cooking container, comprising a pot body having a cooking cavity, wherein the side surface of the pot body facing the cooking cavity is an inner surface; the inner surface is covered with a protective layer containing a non-stick component, and the protective layer comprises: a first protective layer, connected to the inner surface and covering a portion of the inner surface; the material of the first protective layer includes water-based ceramic coating; a second protective layer, the material of the second protective layer includes water-based ceramic coating and corrosion-resistant components, and the mass proportion of the corrosion-resistant components in the second protective layer is Z, 3%wt≤Z≤20%wt.
[0006] By adding an additional corrosion-resistant component to the second protective layer, the second protective layer protects the pot body, thereby alleviating the problem of corrosion of the pot body.
[0007] In some embodiments, the corrosion-resistant component includes at least one of titanium and titanium alloy, and the total mass proportion of titanium in the second protective layer is greater than or equal to 3%.
[0008] Based on the data, when the titanium element accounts for less than 3%, the corrosion resistance is not significantly improved, while the corrosion resistance is improved in the implementation mode where the mass proportion of the titanium element is greater than or equal to 3%.
[0009] In addition, if titanium and titanium compounds are continued to be added so that the titanium element is greater than 20%wt, the corrosion resistance will not be significantly improved compared to the embodiment in which the titanium element is less than 20%wt, but the cost will be significantly increased. At the same time, the corrosion-resistant component will also have an impact on the adhesion of the protective layer. Too high a mass ratio will lead to a weakening of the adhesion and crack resistance of the protective layer. Therefore, optionally, the mass ratio of the titanium element in the second protective layer in the embodiment is maintained within the range of 3%wt-20%wt, for example, 3%wt, 4%wt, 5%wt, 7%wt, 9%wt, 10%wt, 12%wt, 15%wt, 18%wt, 20%wt, 21%wt, 22%wt, 25%wt, etc.
[0010] At the same time, based on the characteristics of water-based ceramic coatings, the toughness of the first and second protective layers is relatively general, and they are prone to cracking after being stressed. After adding titanium or titanium alloy, since these substances have good toughness, the toughness of the first and second protective layers can be adjusted, making the first and second protective layers less likely to crack, so that the first and second protective layers can provide better corrosion resistance and better long-lasting non-stick properties.
[0011] In some embodiments, the corrosion-resistant component includes titanium, and the first protective layer also includes the corrosion-resistant component; the mass percentage of titanium in the first protective layer is X, and the mass percentage of titanium in the second protective layer is Y, and |XY|≤5. For example, the mass percentage difference of titanium in the first protective layer and the second protective layer can be 0%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc.
[0012] In these embodiments, adding one or more of titanium, titanium oxide or titanium nitride to the first protective layer and the second protective layer can make the composition of the first protective layer and the second protective layer closer to the protective layer, thereby making the connection between the two more stable. Moreover, the addition of titanium can further optimize the corrosion resistance of the cooking container as a whole. At the same time, considering that a large difference in the content of titanium will lead to a large difference in the thermal expansion coefficients of the first protective layer and the second protective layer, thereby affecting the connection stability between the first protective layer and the second protective layer, it is set that |XY|≤5 so that the proportion of titanium in the two will not differ too much, thereby alleviating the problem of the protective layer falling off easily due to the large difference in the thermal expansion coefficients.
[0013] In some embodiments, the inner surface is provided with a plurality of protrusions protruding outward toward one side of the cooking cavity; the protrusions are higher than the adjacent first protective layer; and the second protective layer covers the protrusions.
[0014] A number of recessed areas are formed on the pot blank through an etching process, while the unetched areas form ridge-like protrusions. The recessed areas and the protrusions make the cooking cavity surface of the cooking container appear uneven, which helps to reduce the contact area between the food and the cooking cavity surface, thereby helping to improve the non-stickiness of the cooking container, and various patterns can be designed to improve the aesthetics of the cooking container.
[0015] However, the raised portion is in an upward convex shape, which is not only susceptible to impact by foreign objects such as spatulas, but also susceptible to physical wear; the raised portion is also closer to the food, and is therefore susceptible to corrosion by acidic and alkaline components of the food. Under the combined effect of the above problems, the raised portion is easily damaged, which not only loses the beneficial effects of the ridges, but also makes the appearance of the honeycomb pot unsightly.
[0016] Thus, the second protective layer covers the raised portion, which can provide effective protection for the raised portion on the one hand, making the raised portion less susceptible to corrosion; on the other hand, the second protective layer can also easily form a stack at the raised portion, so that the surface of the second protective layer also presents an uneven pattern, thereby also having the effect of improving the non-stickiness.
[0017] In some embodiments, the second protective layer includes: a protective layer connected to the protrusion and covering the protrusion; a non-stick layer connected to the protective layer and covering both the protective layer and the first protective layer; wherein the first protective layer, the protective layer and the non-stick layer all contain the same type of non-stick coating.
[0018] On the one hand, the non-stick layer can improve the non-stick properties at the raised portion; on the other hand, the first protective layer, the shielding layer and the non-stick layer are simultaneously added with the same type of non-stick coating, so that the three have similar compositions, thus having similar thermal expansion coefficients and good bonding ability, which is conducive to the stable connection of the three.
[0019] In some embodiments, the first protective layer has a predetermined color, the protective layer is translucent, and the non-stick layer is transparent; or, the first protective layer has a predetermined color, the protective layer is transparent, and the non-stick layer is translucent.
[0020] In these embodiments, the color of the first protective layer can be various colors, such as gold, black or white, etc., and it is only necessary to add a slurry with a specified color to the raw materials of the first protective layer. The protective layer is translucent, which allows the user to directly see the color of the first protective layer, so that the cooking container has a better appearance. Moreover, translucent means that the light can still pass through the first protective layer with a certain color, for example, it can present an atomized effect. Therefore, the protective layer can also play the role of modifying and improving the visual effect of the color of the first protective layer, so that the visual effect presented on the inner surface is more diverse and beautiful; the non-stick layer is transparent, which reduces the addition of pigments and has less impact on human health. In other embodiments, the composition of the coating is complex. In some cases, it is difficult for the protective layer to meet the requirement of full transparency. Therefore, the non-stick layer located on the outermost side is set to be translucent with a certain color, and the protective layer is set to be transparent. On the one hand, it can ensure that the translucent effect and pearlescent effect of the non-stick layer can be effectively recognized by consumers; on the other hand, due to the darker color of the first protective layer, even if the protective layer cannot completely achieve a transparent effect and becomes foggy or white, the foggy and whitening effect of the protective layer will be covered by the dark color of the first protective layer, thereby not significantly affecting the appearance.
[0021] By adding a non-stick layer, the total thickness of the protective layer can be further increased, so that the non-stick property is better. In addition, under certain backward process conditions, the protective layer may not cover the defective parts of the first protective layer, and the non-stick layer can play the role of filling these defective parts.
[0022] In some embodiments, the second protective layer covers the first protective layer and the protrusion, and the second protective layer includes a first part and a second part, wherein a surface of a side of the first part facing the cooking cavity is higher than a surface of a side of an adjacent second part facing the cooking cavity.
[0023] In these embodiments, the cooking cavity surface of the cooking container may have an uneven pattern, thereby reducing the contact area with the food and increasing the non-stick property at a physical level.
[0024] In some embodiments, along the thickness direction of the pot body, for any adjacent first part and second part, the height difference between the highest point of the first part and the lowest point of the adjacent second part is h, and the maximum distance between the first part and the adjacent first part is L, 0.06≤h / L≤0.5.
[0025] This implementation scheme can find a suitable balance between reducing the food contact area, the cooking feel and the oil storage effect, so that the cooking container has good non-stickiness, usage feel and oil storage effect.
[0026] On the other hand, the present application also provides a cooking container manufacturing method for producing a cooking container; the cooking container manufacturing method comprises the following steps: a molding step: processing a protrusion on the surface of a raw material, and molding the raw material into a pot blank having a cooking cavity; a first spraying step: spraying a non-stick coating on the inner surface to form a first protective layer; a curing step: drying the first protective layer to cure the surface of the first protective layer; a second spraying step: spraying coating on the pot blank to form a protective layer covering the protrusion; wherein the time interval between the end of the first spraying step and the start of the second spraying step is H, 1 hour ≤ H ≤ 100 hours.
[0027] By limiting the time interval between the end of the first spraying step and the beginning of the second spraying step to 1 hour-100 hours, on the one hand, sufficient time can be reserved between the first spraying step and the second spraying step to facilitate the transfer of the pot blank and other possible processes; on the other hand, the upper limit of the time is limited, thereby limiting the complete curing of the first protective layer to avoid the problem of unstable bonding between the protective layer and the completely cured first protective layer.
[0028] In some embodiments, the coating used in the second spraying step includes a first component and a second component, wherein the first component includes at least one of a fluorine coating or a ceramic coating, and the second component includes at least one of titanium, titanium dioxide or titanium nitride, so that the formed protective layer has a certain corrosion resistance effect.
[0029] In some embodiments, the second spraying step further includes a third spraying step: spraying a non-stick coating on the pot blank to form a non-stick layer covering the protective layer; wherein the non-stick coating is a ceramic coating.
[0030] Compared with fluorine coatings, ceramic coatings require a lower temperature for sintering and curing. Even if they are set thicker, they can be sintered and cured under the temperature conditions that can be achieved by existing equipment. Therefore, the protective layer can be set thicker to obtain a good non-stick effect. In addition, the reason why there is no non-stick coating on the raised part of the honeycomb non-stick pan in the prior art is partly because the sintering and curing temperature of the fluorine coating is relatively high. If the thickness of the fluorine coating is too large, it will cause incomplete curing of the fluorine coating and affect the adhesion effect. Therefore, more fluorine coating is removed during polishing to make the thickness of the fluorine coating thinner to facilitate sintering and curing. However, due to the constraints of existing equipment, fluorine coatings of conventional thickness cannot cover the raised part. The curing sintering temperature of ceramic coatings is relatively low. Even if the thickness reaches the thickness that covers the raised part, it can still be sintered and cured normally. Therefore, the protective layer can cover the raised part under the premise of using ceramic coatings to make the raised part also have a non-stick effect.
[0031] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, which can be implemented according to the contents of the specification, and to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0033] Figure 1 A schematic flow chart of a method for manufacturing a cooking container provided in one embodiment of the present application;
[0034] Figure 2 A half-section schematic diagram of a cooking container manufactured by the method for manufacturing a cooking container provided in an embodiment;
[0035] Figure 3 It is a schematic diagram of the structure of the cooking container after one-time spraying and polishing;
[0036] Figure 4 It is a schematic diagram of the structure of the cooking container after secondary spraying;
[0037] Figure 5 It is a structural schematic diagram of an embodiment of a cooking container after three sprayings;
[0038] Figure 6 It is a schematic diagram of a partial structure of the cooking cavity surface of the second embodiment of the cooking container;
[0039] Figure 7 is a schematic diagram of a partial structure of the cooking cavity surface of the third embodiment of the cooking container;
[0040] Figure 8 is a schematic diagram of a partial structure of the cooking cavity surface of a fourth embodiment of a cooking container;
[0041] Fig. 9 A schematic diagram of the cooking cavity surface effect of a cooking container manufactured without a cleaning step;
[0042] Fig.10 A schematic diagram of the surface effect of the cooking cavity of the cooking container manufactured by the cleaning step;
[0043] The reference numerals in the specific implementation manner are as follows:
[0044] 1. pot body; 10. cooking cavity; 11. raised part; 12. recessed part;
[0045] 2. The first protective layer;
[0046] 30. Notch portion; 31. Protective layer; 32. Non-stick layer; 321. First portion; 322. Second portion; 33. Accommodating groove; 34. Protruding point portion. DETAILED DESCRIPTION
[0047] In order to more clearly illustrate the overall concept of the present application, a detailed description is given below in an illustrative manner in conjunction with the accompanying drawings.
[0048] In the description of the embodiments of the present application, the orientations or positional relationships indicated by technical terms such as "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", and "circumferential" are based on the orientations or positional relationships shown in the accompanying drawings and are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.
[0049] In addition, the technical terms "first", "second", etc. are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0050] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.
[0051] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or that the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0052] Etched pattern pot is a common cooking container. Its structure is that a number of raised parts are processed on the cooking cavity surface of the pot body through etching and other processes, so that the surface of the cooking cavity presents a certain pattern. However, during use, these raised parts are prone to structural changes or even damage, resulting in the pattern being recycled, affecting the appearance and function.
[0053] According to the analysis, one of the reasons why the raised part is damaged is that the raised part is corroded by the food. This is because the raised part is in an upward convex state relative to the surrounding part, so the contact area between the raised part and the food is larger, making it more susceptible to corrosion. Based on this, the present application intends to start from the above perspective in order to improve the corrosion resistance of the raised part.
[0054] refer to Figure 2-Figure 5 The cooking container of this embodiment includes a pot body 1, which is bent to form a cooking cavity 10, wherein the side surface of the pot body 1 facing the cooking cavity 10 is the inner surface, and the inner surface is provided with a plurality of protrusions 11 and recesses 12, wherein the recesses 12 are formed between the protrusions 11, and the recesses 12 are in a concave form relative to the protrusions 11. The protrusions 11 and the recesses 12 can be formed by various existing processes, for example, by chemical etching, rolling or physical hammering, etc., and the forming method is not limited here. The inner surface of the pot body is covered with a protective layer for providing a non-stick effect, and the protective layer includes at least a first protective layer 2 and a second protective layer. The first protective layer 2 is arranged in the recess 12 and covers the recess 12, and the highest point of the surface of the first protective layer 2 facing the cooking cavity 10 is lower than the protrusion 11, and the protrusion 11 is in a convex form relative to the first protective layer 2 toward the cooking cavity 10. The second protective layer covers the first protective layer 2 and the protrusion 11 as a whole, that is, the first protective layer 2 and the protrusion 11 are both located in the second protective layer.
[0055] In the above embodiment, the raised portion 11 is covered by the formed second protective layer, so the position of the surface of the cooking cavity 10 corresponding to the raised portion 11 also has non-stick properties. And because the second protective layer at the raised portion 11 is also in a convex form, when the second protective layer directly contacts the food, it helps to reduce the contact area between the surface of the protective layer and the surface of the food, so that the protective layer has better non-stick properties.
[0056] In some other embodiments, the second protective layer may also only cover the protrusion 11 , and the other areas of the cooking cavity surface are provided with a non-stick effect by the first protective layer 2 .
[0057] Considering that the material of the raised portion 11 is generally stainless steel or aluminum and other metals, the raised portion 11 may be corroded by food. Therefore, in some embodiments, at least one of the corrosion-resistant components such as titanium, titanium dioxide or titanium nitride may be added to the second protective layer. Specifically, in the second protective layer, the total mass proportion of one or more of titanium, titanium dioxide or titanium nitride is Z, and Z ≥ 3% wt. For example, the value of Z can be 3% wt, 5% wt, 10% wt, 15% wt, 20% wt, etc. Mixing a small amount of corrosion-resistant components such as titanium, titanium dioxide, titanium nitride or titanium carbide into the coating can improve the corrosion resistance of the formed second protective layer, making the raised portion 11 less susceptible to corrosion. However, in the embodiment, the value of Z should not be too large. For example, when it is greater than 20% wt, the use of a general spraying process may affect the bonding ability of the second protective layer, so that the obtained sample cannot complete the cooking experiment of 3 cycles. Therefore, in this embodiment, the value of Z is controlled to be below 20%.
[0058] Considering that the second protective layer contains corrosion-resistant components such as titanium, titanium dioxide or titanium nitride, the first protective layer 2 may also contain corrosion-resistant components, which on the one hand provides corrosion resistance and on the other hand makes the first protective layer 2 and the second protective layer similar in composition, which is beneficial to the combination of the first protective layer 2 and the second protective layer.
[0059] In addition, in some other embodiments, the pot body 1 may not be provided with the raised portion 11. Covering the pot body 1 without the raised portion 11 with the first protective layer 2 and the second protective layer at the same time can also play a role in improving the protection performance of the pot body 1.
[0060] Table 1 is the test data obtained after subjecting the above-mentioned embodiments and comparative examples to salt spray tests. Among them, the physical structures of comparative example 1, comparative example 2, experimental example 1, experimental example 2, and experimental example 3 are similar, and the material of the raised portion is 304 stainless steel. The difference is that in comparative example 1, the surface of the raised portion is directly exposed; in comparative example 2, the protective layer on the surface of the raised portion does not contain corrosion-resistant components such as titanium, titanium dioxide or titanium nitride, and the difference between the protective layer of comparative example 2 and the protective layer of the above-mentioned embodiment is only that it does not contain corrosion-resistant components; in experimental example 1, the mass proportion of the corrosion-resistant component is 1%; in experimental example 2, the mass proportion of the corrosion-resistant component is 3%; in experimental example 3, the mass proportion of the corrosion-resistant component is 5%. The salt spray test can be carried out in accordance with the national standard and is not limited here. The pot body of the example without raised portion is made of 304 stainless steel, and there is no raised portion on the pot body.
[0061] Table 1
[0062]
[0063]
[0064] It can be seen that in Comparative Examples 1 and 2 that do not contain corrosion-resistant components, the cooking containers cannot meet the test standard of no rust in the salt spray test for 24 hours; and in Experimental Example 1, due to the low mass proportion of the corrosion-resistant components, the test requirements cannot be met. When the mass proportion of the corrosion-resistant components reaches more than 3%, the cooking container can meet the test standard of no rust in 24 hours. Therefore, when the mass proportion of the corrosion-resistant components reaches more than 3%, the protective layer can effectively protect the protrusion 11. In addition, the example without the protrusion also shows the characteristic of no rust in 24 hours, so it can be seen that the second protective layer also has the characteristic of improving the corrosion resistance of the embodiment without the protrusion.
[0065] In some embodiments, the first protective layer 2 also contains titanium, and the difference in the mass percentage of titanium between the first protective layer 2 and the second protective layer is less than or equal to 5%, for example, the mass percentage of titanium is the same, or 0.5%, 1%, 2%, 3%, 4%, 5%, etc., so that the composition of the two is close, and the two have similar thermal expansion coefficients, so that the first protective layer 2 and the second protective layer can be connected more stably. In the case where the mass percentage of titanium differs by more than 5%, on the one hand, the sample may not be able to complete the cooking experiment for 3 cycles, and on the other hand, problems such as porcelain collapse may occur. Therefore, in the embodiment, the mass percentage difference of titanium between the first protective layer 2 and the second protective layer should be kept less than or equal to 5%.
[0066] Reference Figure 5 , the second protective layer includes a protective layer 31 and a non-stick layer 32, the non-stick layer 32 is attached to the protective layer 31, and the non-stick layer 32 covers the protective layer 31. Among them, the first protective layer 2 has a predetermined color, such as white, black, medical stone color and gold, etc. The method for obtaining the predetermined color is to add a slurry of a corresponding color to the raw material of the first protective layer 2, which belongs to the prior art and is not repeated here; the protective layer 31 is translucent, and the appearance effect of the first protective layer 2 can be adjusted, so that the visual effect presented on the surface of the cooking cavity 10 is more in line with the requirements; the non-stick layer 32 is fully transparent and has no obvious effect on the appearance.
[0067] The non-stick layer 32 includes a first portion 321 and a second portion 322, wherein the first portion 321 is correspondingly located on the raised portion 11, and the second portion 322 is correspondingly located on the recessed portion 12. Along the thickness direction of the pot body, the surface of the first portion 321 facing the cooking cavity 10 is higher than the surface of the adjacent second portion 322 facing the cooking cavity 10, that is, along the thickness direction of the pot body 1, the first portion 321 is in the form of protruding toward the side of the cooking cavity 10 relative to the adjacent second portion 322. The first portions 321 are mutually enclosed, so that the first portions 321 and the second portions 322 jointly form a plurality of receiving grooves 33, the first portions 321 constitute the side walls of the receiving grooves 33, and the second portions 322 enclosed in the first portions 321 constitute the bottom walls of the receiving grooves 33.
[0068] The first portion 321, as the side wall of the receiving groove 33, can limit the outflow of cooking oil from the receiving groove 33, so that after pouring cooking oil into the cooking container during cooking, a portion of cooking oil can be retained in each receiving groove 33 even during operations such as flipping the pan, thereby helping to improve the non-stickiness of the cooking container during cooking.
[0069] The shape formed by the first portion 321 and the receiving groove 33 can be as follows Figure 6 The hexagonal honeycomb shown may also be other shapes, and the shape is not particularly limited here.
[0070] Furthermore, the raised portions 11 also surround each other, so that the recess 12 is surrounded by raised portions 11 .
[0071] The raised portions 11 intersect and enclose the recessed portion 12 so that the recessed portion 12 is surrounded by raised portions 11 . Thus, no matter from which angle the spatula impacts the surface of the cooking cavity 10 , the raised portions 11 can provide protection for the recessed portion 12 .
[0072] The layered structures of the embodiments can be referred to Figure 2 The area in the cooking container where the protective layer is provided is the cooking area B. In the illustrated embodiment, the bottom surface of the cooking cavity and the side surface connected to the bottom surface together constitute the cooking area B (i.e. Figure 2 The cooking cavity surface below the dotted line is shown in the figure below the dotted line to make the diagram clear. Figure 2 The structure of the receiving groove 33 is omitted in the cooking zone B), and the ratio of the projection of the receiving groove 7 in the cooking zone B to the area of the cooking zone B is greater than or equal to 85%. For example, it can be 85%, 86%, 88%, 89%, 90%, 91%, 94%, 95%, 97%, 98%, 99%, 99.5%, etc. Since the receiving groove 33 is arranged in most areas of the cooking zone B, the receiving groove 33 can store part of the edible oil, so that the cooking zone B can be filled with edible oil as much as possible, thereby obtaining an ideal non-stick effect.
[0073] Reference Figure 5 and Figure 6 In the embodiment shown, the maximum spacing between the side walls of the receiving groove 33 is L mm, that is, for each receiving groove 33, the maximum spacing between the first parts 321 constituting the receiving groove 33 is L mm. Figure 6 In the embodiment of , L is the diagonal length of the hexagonal receiving groove 33. The depth of the receiving groove 33 is h mm. Among them, 0.06≤h / L≤0.5.
[0074] Among them, the larger the h is, the deeper the depth of the receiving groove 33 is, and the less likely the food is to contact the bottom surface of the receiving groove 33; and the smaller L is, the easier it is for the food to be lifted up by more adjacent first parts 321, so that the food is not easy to enter the receiving groove 33. It can be seen that the larger the value of h / L is, the less likely the food is to contact the bottom surface of the receiving groove 33, that is, the better the physical non-stick effect. However, the value of h / L cannot be increased indefinitely. On the one hand, a too large h value will affect the cooking feel. On the other hand, a too small L value will make the opening of the receiving groove 33 too small, making it difficult for oil to flow in, resulting in poor oil storage effect. After comprehensive consideration, within the value range of 0.06≤h / L≤0.5, the oil storage effect, physical non-occupancy and cooking feel can be taken into account.
[0075] exist Figure 6 In the illustrated embodiment, the spacing between the diagonal points of the side walls of each regular hexagonal receiving groove 33 is 8 mm, that is, the maximum spacing between the side walls of the receiving groove 33 is 8 mm. Of course, the spacing can also be 5 mm, 6.5 mm, 7 mm, 10 mm, 12 mm, etc., as long as L is less than or equal to 12. Under this size, the spacing between the side walls of the receiving groove 33 is small, and after edible oil is adsorbed, the oil beads in the receiving groove 33 can be continuously distributed, so that the oil can be distributed more evenly in the receiving groove 33. In addition, the minimum value of L is 3, so that the oil storage tank can store oil normally.
[0076] In some embodiments, the thickness of the first protective layer 2 may be 15 μm-30 μm, for example, 15 μm, 16 μm, 20 μm, 24 μm, 25 μm, 28 μm, and 30 μm. Within this thickness range, on the one hand, the first protective layer 2 has a sufficient thickness so that the first protective layer has good non-stick properties; on the other hand, the thickness value is adapted to the height of the protrusion 11 formed by the conventional process, so that the thickness of the first protective layer 2 will not be greater than the height of the protrusion 11, so as to meet the purpose of the protrusion 11 being higher than the first protective layer 2. The thickness of the protective layer 31 is 3 μm-8 μm, for example, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, or 8 μm. Since the protective layer 31 is located between the first protective layer 2 and the non-stick layer 32, the protective layer 31 can be set thinner accordingly, which is beneficial to material saving on the one hand, and the thinner protective layer 31 is also convenient for sintering and curing on the other hand. The thickness of the non-stick layer 32 is 3 μm-10 μm, such as 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, so that the total thickness of the non-stick layer 32 and the protective layer 31 is larger, so that the protrusion 11 has a good non-stick effect.
[0077] In some embodiments, the non-stick layer 32 can be thicker than the protective layer 31, so that even if the total thickness of the non-stick layer 32 and the protective layer 31 is larger, the translucent and thinner protective layer 31 is less likely to appear foggy and white. In addition, the thinner protective layer 31 is also easier to dry as a whole later.
[0078] Specifically, the thickness ratio of the protective layer 31 to the non-stick layer 32 is Q, and 0.7≤Q<1, so that the protective layer 31 can be dried and cured more completely.
[0079] In some embodiments, the thickness of the first protective layer 2 is greater than the thickness of the non-stick layer 32 and greater than the thickness of the protective layer 31. Since the first protective layer 2 is protected by the protrusion 11, it is not easy to fall off even if it is thick, so the first protective layer 2 can be set thicker accordingly to obtain a better non-stick effect.
[0080] exist Figure 7 In another embodiment shown, the second part 322 is provided with a plurality of convex points 34, and the convex points 34 are in the form of upward protrusion relative to the bottom surface of the surrounding receiving grooves 33, that is, the surface of the second part 322 corresponding to the area located at the convex points 34 is higher than the surface of the adjacent second part 322. The provision of the convex points 34 helps to further reduce the contact area between the food and the surface of the cooking cavity, thereby improving the non-stickiness. The convex points 34 can be formed by providing a plurality of convex points on the substrate, and after spraying the coating, the coating covers the convex points, and the convex points 34 can be naturally formed.
[0081] The main material of the protective layer in the above embodiment, except for the corrosion-resistant component, can be ceramic coating. Ceramic coating is a common non-stick coating in the field of cooking utensils. Since ceramic coating has a lower sintering and curing temperature, it is more suitable for the above embodiment with a thicker total thickness of the protective layer. That is, the use of ceramic coating is more convenient for sintering and curing during production, so that the protective layer has an adhesion firmness that meets the requirements.
[0082] For the pot body 1, one embodiment of the pot body 1 includes an outer layer, a heat-conductive middle layer and an inner layer, wherein the material of the outer layer is the existing 430 magnetic stainless steel, the material of the heat-conductive middle layer is aluminum, and the material of the inner layer is 304 stainless steel or 316L stainless steel. 430 magnetic stainless steel can make the pot body 1 suitable for induction cookers; aluminum has good thermal conductivity, so the heat-conductive middle layer can transfer the heat of the outer layer to the inner layer; the inner layer has good anti-rust performance. The inner layer refers to a layer of the layered structure of the pot body 1 facing the cooking cavity 10, the outer layer refers to a layer of the layered structure of the pot body 1 facing the outside of the pot body 1, and the heat-conductive middle layer is a layered structure sandwiched between the inner layer and the outer layer.
[0083] In another embodiment of the pot body 1, only an outer layer and an inner layer are included, wherein the outer layer is made of aluminum, and the inner layer is made of 304 stainless steel or 316L stainless steel, so as to be suitable for open flame scenes, and the overall weight of the pot body 1 is relatively light.
[0084] Figure 8 The embodiment shown is Figure 2 and Figure 7 The structures of the embodiments shown are basically the same, except that: Figure 8 The first middle portion 321 is provided with a plurality of notches 30 , which allow adjacent receiving grooves 33 to communicate with each other, thereby facilitating the mutual circulation of edible oil in each receiving groove and further facilitating the uniform distribution of edible oil.
[0085] The non-stickiness comparison results of the embodiment and the comparative example provided in this application can be referred to Table 2. The structure of Experimental Example 7 in Table 2 can be referred to Figure 2 and Figure 5 The pot body 1 of the fourth experimental example includes an outer layer made of 430 magnetic conductive stainless steel, a heat conductive middle layer made of aluminum, and an inner layer made of 304 stainless steel. Figure 5 and Figure 6 The honeycomb-shaped raised portion 11 is shown, and the raised portion 11 surrounds the recess 12. The surface of the inner layer is attached with a protective layer formed by spraying ceramic coating, and the protective layer includes a first protective layer 2, a protective layer 31 and a non-stick layer 32, wherein the first protective layer 2 covers the recess 12, the protective layer 31 covers the raised portion 11 and the recess 12, the non-stick layer 32 covers the protective layer 31, and the non-stick layer 32 forms a first part 321 at the position corresponding to the raised portion 11, and the non-stick layer 32 forms a second part 322 at the position corresponding to the recess 12, the first part 321 protrudes outward relative to the adjacent second part 322, and the first part 321 intersects with each other, and together with the second part 322, forms a receiving groove 33. In addition, a plurality of protruding convex points 34 are formed on the bottom surface of the receiving groove 33.
[0086] The structure of the pot body 1 of comparative example 3 is the same as that of the embodiment, and the only difference is that the comparative example only includes a protective layer covering the recessed portion 12, that is, the surface of the raised portion 11 of comparative example 1 has no protective layer.
[0087] The overall structure of Comparative Example 4 is the same as that of Comparative Example 1, but the difference is that the protective layer material of Comparative Example 2 is fluorine coating.
[0088] The test methods are based on the national standard GB / T32388 fried egg test for initial non-stickiness, and the national standard GB / T32388 vibration wear test followed by a fried egg test to verify long-term non-stickiness.
[0089] The test results are shown in Table 3:
[0090] Table 2
[0091] Initial non-stickiness Long-lasting non-stickiness Experimental Example 4 Level 1 Level 2 Comparative Example 3 Level 3 Level 3 Comparative Example 4 Level 2 Level 2
[0092] It can be seen that compared with comparative example 3, the initial non-stickiness and the lasting non-stickiness of experimental example 4 are significantly improved, which shows that providing a protective layer on the surface of the raised portion 11 can significantly improve the initial non-stickiness and the lasting non-stickiness of the cooking container; and compared with comparative example 4, embodiment 4 has better initial non-stickiness and basically equivalent lasting non-stickiness. It can be seen that after providing multiple protective layers, the protective layer of the ceramic coating can have a non-stick effect equivalent to that of the fluorine coating, and can also avoid the disadvantage of the fluorine coating that toxic substances are easily volatilized at high temperatures, making the cooking container healthier.
[0093] In addition, refer to Fig. 9 and Fig.10 , Fig. 9 A comparative example of a cooking container without a cleaning step, Fig.10 The surface appearance of the cooking cavity of the cooking container manufactured by the manufacturing method of the cooking container including the cleaning step is compared with Fig. 9 , Fig.10 It can be clearly seen from the embodiment that after the impurities are removed, there is no obvious accumulation of stains on the bottom of the first portion 321 (i.e., the bottom of the raised portion 11), and the appearance of the surface of the cooking cavity is more neat and beautiful. In addition, in combination with the above experimental results, in the absence of stain accumulation, the long-lasting non-stickiness of the cooking container is improved.
[0094] The present application provides a method for manufacturing a cooking container. The process steps included in the optional embodiment can be referred to Figure 1 The specific embodiments of each step are as follows:
[0095] The forming step is to form the raw material into a pot blank of a predetermined shape by die casting, stretching, spinning or any other commonly used process. The shape of the pot blank is not limited, and can be a frying pan, a steamer, an inner pot or other conventional cooking container shapes, which can be determined according to specific needs. For example, the forming step adopted in a certain embodiment is: a plate made of composite steel is selected as the raw material. The composite steel includes three layers, wherein the first layer is made of 304 stainless steel or 316 stainless steel, the second layer is made of thermal conductive aluminum, and the third layer is made of 430 stainless steel with magnetic conductivity, and the second layer is sandwiched between the first layer and the third layer. The composite steel plate is formed into a pot blank by a stretching process. After stretching, the surface of the first layer faces the cooking cavity of the pot blank, and the surface of the third layer faces the outside of the pot blank. In other embodiments, the composite steel may also include only two layers, the first layer is made of 304 stainless steel or 316 stainless steel, and the second layer is made of thermal conductive aluminum. After stretching, the surface of the first layer faces the cooking cavity of the pot blank, and the surface of the second layer faces the outside of the pot blank.
[0096] The roughening step refers to roughening the surface of the side of the pot blank facing the cooking cavity by a process such as sandblasting, so that the roughness of the surface of the side of the pot blank facing the cooking cavity is increased, so as to increase the contact area with the coating. For example, the roughening step adopted by a certain exemplary embodiment is: after the pot blank is formed, an alkaline, acidic or neutral solvent is sprayed on the surface of the pot blank to remove tiny debris on the surface of the pot blank to prevent the debris from affecting the subsequent sandblasting process. This method of removing debris can also be called an oiling process, which is a conventional debris removal process in the industry. The specific process parameters, solvent composition and principle are not repeated here. After removing the debris, a high-speed sand flow is used to impact the surface of the pot blank facing the cooking cavity, that is, the inner surface of the pot blank, so that the inner surface of the pot blank forms an uneven plane, so that the protective layer formed by the first spraying can be stably attached. The abrasive used in the sandblasting process can be a mixture of 60 mesh and 80 mesh brown corundum or white corundum, or other sandblasting process conditions can be used, as long as the roughness of the inner surface of the pot blank obtained after treatment meets the expectations. After sandblasting, the roughness of the inner surface of the pot blank is Ra2.5μm-4.0μm, and the overall surface is relatively uniform.
[0097] The first spraying step is to spray a non-stick coating on the inner surface of the pot blank, thereby forming a first protective layer 2 attached to the inner surface of the pot blank. The non-stick coating can be a fluorine coating, a ceramic non-stick coating, or other coatings that can be applied to the field of cooking containers. The specific components of the coating are not specifically limited. In some embodiments, the sandblasted pot blank is first dusted before spraying to remove impurities remaining after sandblasting, and then the pot blank is preheated before spraying, and the pot blank is preheated to 50°C-60°C for standby use. The first spraying step adopted in the embodiment is: the coating used in this example is a ceramic coating. Specifically, the ceramic coating is a siloxane-based ceramic coating containing silica sol, siloxane, an acidic solvent and a pigment slurry. The ceramic coating is sprayed with a spray gun, and the caliber of the spray gun is set to 1.0mm-2.0mm. For example, the caliber of the spray gun can be 1mm, 1.5mm or 2mm; the spraying pressure of the spray gun is set to 2kg / cm 2 -3kg / cm 2 , for example, it can be 2kg / cm 2 , 2.5kg / cm 2 or 3kg / cm 2 . Under this working condition, the thickness of the first protective layer formed after one spraying is about 20μm-40μm, which meets the basic thickness requirement of non-stick coatings, and under this spraying pressure, the first protective layer can fit tightly to the inner surface of the pot blank, which helps to improve the bonding strength between the first protective layer and the pot blank after curing.
[0098] The purpose of preheating is to suppress the problem of rapid cooling and curing of the coating in contact with the low-temperature pot body 1, especially to alleviate the problem of rapid cooling and curing of the silicon-based ceramic coating, thereby helping to improve the connection stability between the first protective layer 2 and the pot body 1. On the other hand, if the temperature of the pot body is too low, the coating may scatter due to the large temperature difference after contacting the pot body, thereby forming a number of solid particles that cannot be stably attached to the pot body. The solid particles, as impurities, will affect the adhesion of the coating to the pot body.
[0099] The curing step refers to drying and curing the surface of the first protective layer so that the first protective layer forms a solid surface with a certain hardness, so that the first protective layer can be processed in the subsequent process steps. For example, the curing step adopted in a certain embodiment is: sintering and curing the cooking container after the first spraying in a sintering furnace. In the example where the coating is a ceramic coating, the sintering temperature in the furnace is maintained at 100°C-150°C, for example, it can be 100°C, 110°C, 120°C, 130°C, 140°C or 150°C; the sintering and curing time is 5 minutes-20 minutes, for example, it can be 5 minutes, 7 minutes, 10 minutes, 13 minutes, 15 minutes, 18 minutes or 20 minutes. In other embodiments, when the coating composition changes, it is only necessary to adjust the curing temperature and curing time according to the actual situation. For example, the curing temperature of the fluorine coating is about 400°C. The specific working conditions can be selected according to the conventional technical means of the industry, and will not be described one by one here.
[0100] The polishing step refers to polishing the surface of the first protective layer 2 after the first spraying. The purpose of polishing is to make the surface of the first protective layer 2 flat, limit the problem of impurities accumulating in the pits and being difficult to remove in the subsequent process, and make the surface of the first protective layer 2 neat and beautiful.
[0101] The specific method of polishing can refer to the prior art, for example, the surface of the first protective layer 2 can be smoothed using sandpaper, and then large debris left over from polishing can be removed using a scouring pad. Alternatively, other conventional polishing techniques in the prior art can be used, which will not be described in detail here.
[0102] The cleaning step refers to cleaning the surface of the first protective layer 2 after the first spraying to remove impurities on the surface of the first protective layer 2. It is required that after the impurities are removed, there is basically no visible accumulation of impurities on the surface of the first protective layer 2 that can be easily removed by wiping. After the cleaning step is completed, the method for testing whether there are residual impurities can be to wipe the surface of the first protective layer 2 with a white paper towel. If the surface of the white paper towel is obviously discolored, it proves that the impurities are not completely removed, and it is necessary to continue cleaning to remove the impurities until the white paper towel does not change color or only changes color very slightly. The main purpose of removing impurities is to reduce the interference of impurities with the spraying effect, that is, to enable the subsequently sprayed protective layer 31 to directly contact and fit with the first protective layer 2. In addition, removing impurities can also eliminate the interference of impurities on the appearance of the cooking container.
[0103] Here are three cleaning examples that can be selected based on actual process conditions:
[0104] Cleaning experiment example 1:
[0105] Use high-pressure air to remove impurities on the surface of the first protective layer. Specifically, spray high-pressure air directly onto the surface of the first protective layer 2, and use the high-pressure air to blow the impurities directly out of the accommodation cavity. Then use a lint-free towel or paper towel to repeatedly wipe the surface of the first protective layer 2 several times to remove the remaining impurities.
[0106] The effect of using high-pressure air to remove impurities is that there are fewer solid impurities entrained in general air, and it is not easy to continue to increase impurities on the surface of the first protective layer 2 that affect the mutual adhesion of the first protective layer 2 and the protective layer 31. Basically, no subsequent treatment is required, and the impurity removal effect is better.
[0107] Specifically, the spray pressure of the high-pressure air is set to P≥0.5kpa, and the distance between the spray position of the high-pressure air and the first protective layer 2 is less than 50mm. For example, a high-pressure air gun can be used for cleaning, and the jet pressure of the high-pressure air gun is set to 0.5kpa, or 0.8kpa or 1kpa, etc., and the muzzle of the high-pressure air gun is set to a position about 30mm above the surface of the first protective layer 2, or 20mm, 39mm, 40mm, etc. The high-pressure air gun sprays high-pressure gas at an angle directly facing the surface of the first protective layer 2 to blow away impurities on the surface of the first protective layer 2. Based on experiments, when the above process parameters are used for spraying and removing impurities, the paper towel will only change color slightly or not change color after wiping it with a paper towel, and the spray gun distance is greater than 50mm or the air pressure is less than 0.5kpa, which will cause the paper towel to change color more obviously, that is, the cleaning effect is not ideal.
[0108] Cleaning experiment example 2:
[0109] Clean the debris using high-pressure water flow and dry the residual liquid after cleaning. Specifically, a high-pressure water gun can be used to rinse the surface of the first protective layer 2, and after rinsing, the cooking container can be dried to remove the residual liquid. Compared with gas, the rinsing effect of high-pressure liquid is better. Generally, after rinsing once, physical wiping is not required again to meet the cleaning requirements. The drying temperature can be controlled below the curing and drying temperature of the first protective layer, that is, the drying temperature for removing the cleaning liquid is W1, and the drying and curing temperature of the first protective layer is W2, where W1 < W2. This temperature is relatively low compared to the temperature of the curing step. Drying within this temperature range helps reduce the risk of cracking of the first protective layer 2.
[0110] Cleaning experimental example three:
[0111] Directly use a wiping cloth to repeatedly wipe the surface of the first protective layer 2 to remove the attached impurities. The method for testing the wiping result can also be to wipe with a white paper towel. When the paper towel does not change color significantly, it can be considered that there are no impurities on the surface of the first protective layer 2.
[0112] In cleaning experimental example three, note that the wiping cloth should be a non-shedding flannel to avoid further increasing impurities.
[0113] The above three cleaning embodiments can also be used simultaneously or in pairs to obtain a better cleaning effect.
[0114] The second spraying step refers to continuing to spray the coating on the inner wall of the pot body 1 to form a protective layer 31. The coating used in the second spraying step is a transparent non-stick coating, and the main components of this coating can be the same as or different from those of the first protective layer 2. For example, in a certain exemplary embodiment, the second spraying step is as follows: Use a spray gun with a caliber of 1.0 mm - 2.0 mm for spraying, and set the spraying pressure to 1.5 kg / cm 2 - 2.5 kg / cm 2 , for example, the spraying pressure can be 1.5 kg / cm 2 、2 kg / cm 2 or 2.5 kg / cm 2 . After spraying, a protective layer 31 with a thickness slightly thinner than that of the first protective layer 2 can be formed. The thickness of the protective layer 31 formed under the working conditions of this embodiment is about 3 μm - 12 μm. The thickness of the protective layer 31 is relatively thin. Based on tests, on the one hand, the thinner the protective layer 31, the less likely it is to fall off after being impacted; on the other hand, the protective layer 31 with this thickness can have a primary non-stickiness of level 1 and a persistent non-stickiness of level 2 after vibration testing based on GB / T 32388 when combined with the first protective layer 2. Therefore, the non-stickiness can also meet the requirements, that is, the protective layer 31 within this range can balance the connection stability and non-stickiness.
[0115] In addition, in certain further embodiments, the interval time between the first spraying step and the second spraying step is required to be H, 1 hour ≤ H ≤ 100 hours. If the interval time is greater than 100 hours, the first protective layer may be completely cured, and the completely cured first protective layer and the uncured second protective layer may have the defect of being difficult to stably combine, thereby affecting the bonding stability of the first protective layer and the second protective layer; and if the interval time is less than 1 hour, the interval time is too short and the surface of the first protective layer may not be completely cured, resulting in the polishing step and the cleaning step being difficult to proceed normally. After experimental verification, controlling the interval time between the first spraying step and the second spraying step to 1 hour-100 hours can take into account both the requirements that the first protective layer will not be completely cured and the surface of the first protective layer is dry and cured, and the time arrangement is reasonable, which is convenient for the connection of each process.
[0116] The third spraying step refers to spraying the pot body 1 with the protective layer 31 for the third time to form a non-stick layer 32. Similar to the protective layer 31, the coating used to form the non-stick layer 32 can be the same as the main component of the coating of the first protective layer 2, or it can be different, and the non-stick layer 32 is transparent. The specific method adopted in the third spraying step can also refer to the second spraying step. The formed non-stick layer 32 can further enhance the lasting non-stickiness on the one hand, and on the other hand, it can complement the appearance of the protective layer 31. For example, the protective layer 31 and the non-stick layer 32 are both transparent protective layers with a certain base color. After the two are superimposed, a new appearance style can be formed, thereby improving the aesthetics.
[0117] The overall curing step refers to sintering and curing the first protective layer 2, the protective layer 31 and the non-stick layer 32. The specific process flow and parameters of the overall curing step can refer to the aforementioned curing step or the prior art, and only the protective layer 31 and the non-stick layer 32 need to be cured.
[0118] In addition, in some optional embodiments, the following process is used for overall curing: first, the pot body is placed in an environment of 80°C-150°C for 5 minutes-18 minutes, for example, it can be placed in an environment of 80°C for 18 minutes, an environment of 100°C for 15 minutes, an environment of 120°C for 10 minutes, or an environment of 140°C for 8 minutes. The specific temperature or time can be adjusted according to the actual situation. If the curing is not complete, it can be considered to increase the temperature within the range or extend the placement time. After that, the environment is heated to 200°C-250°C, such as 200°C, 220°C, 240°C, etc., and continue to be placed for 5 minutes-28 minutes. The heating process can make the curing effect more complete, so that the part below the surface can also be effectively cured, and the occurrence of cracking of the protective layer can be suppressed. After two drying treatments, the first protective layer 2, the protective layer 31 and the non-stick layer 32 are completely dried and tightly combined and not easy to fall off.
[0119] After the overall solidification, the surface of the cooking cavity 10 of the pot body 1 can be polished as needed, so that the surface of the cooking cavity 10 presents a style that meets the requirements.
[0120] In some other embodiments, the method for manufacturing a cooking utensil is used to produce a cooking container having an etched pattern. Figure 2 The cooking container produced includes a pot body 1, a first protective layer 2, a protective layer 31 and a non-stick layer 32, wherein the surface of the cooking cavity 10 facing the pot body 1 has a plurality of protrusions 11, and the protrusions 11 form etching lines with a certain pattern on the surface of the pot body 1. The highest point of the first protective layer 2 is lower than the highest point of the protrusions 11, so that the first protective layer 2 is located in the concave portion 12 formed between adjacent protrusions 11 and is concave relative to the protrusions 11, so that the protrusions 11 can make it difficult for foreign objects such as spatulas to directly contact the first protective layer 2, play a role in protecting the first protective layer 2, and the etching line pattern formed by the protrusions 11 can be seen. The protective layer 31 is formed on the surface of the first protective layer 2, and the protective layer 31 covers the first protective layer 2 and the protrusions 11 at the same time, that is, the highest point of the protrusions 11 is located inside the protective layer 31. Since the protective layer 31 covers the raised portion 11, the food will not directly contact the raised portion 11 if the protective layer 31 is not detached, thereby helping to improve the anti-stickiness of the pot body 1. The non-stick layer 32 covers the protective layer 31, which helps to increase the overall thickness of the protective layer, thereby further improving the non-stickiness of the cooking container.
[0121] The manufacturing method of the cooking utensil for producing a cooking container with etching lines comprises Figure 1 The steps shown in the embodiment further include the following steps compared with the above embodiment:
[0122] The raw material used in the forming step is a composite plate that has been etched, and a plurality of protrusions 11 have been formed on the composite plate.
[0123] The structure after the polishing step can be referred to Figure 3 In the polishing step, it is necessary to completely remove the first protective layer 2 on the surface of the raised portion 11 so that the highest point of the raised portion 11 protrudes from the first protective layer 2. On the one hand, only when the raised portion 11 protrudes relative to the first protective layer 2 can it effectively play a protective effect. On the other hand, the etching lines formed by the raised portion 11 have a certain appearance style, and the first protective layer 2 is a colored protective layer. Therefore, in order to make the etching lines visible, the first protective layer 2 on the surface of the raised portion 11 needs to be completely removed. In addition, after this step, the surface of the cooking cavity 11 presents an uneven style, which is conducive to increasing the contact area with the protective layer 31 and also facilitates the subsequent attachment of the protective layer 31.
[0124] The structure after the second spraying step can be referred to Figure 4It should be noted that the sprayed protective layer 31 needs to completely cover the first protective layer 2 and the protrusion 11 to provide a good initial non-stick effect.
[0125] Specifically, an optional embodiment of a method for manufacturing a cooking utensil is provided, which is used to produce a cooking container with an etched pattern, and specifically comprises the following steps:
[0126] The raw materials of the pot body 1 are selected from a composite plate with an outer layer of 430 magnetic conductive plate, an intermediate layer of aluminum heat conductive plate, and an inner layer of 304 or 316L with etched patterns; the coating of the protective layer is selected from a ceramic coating containing silica sol, siloxane, acidic solvent and pigment slurry. Since the sintering temperature of ceramic coating is lower than that of fluorine coating, the ceramic coating can be set thicker to improve the non-stickiness. Moreover, the sintering temperature of fluorine coating is relatively high, and fluorine coating is easy to decompose at high temperature, and the sintering temperature of fluorine coating is close to the high-temperature decomposition temperature of fluorine coating, so it is possible that the fluorine coating will decompose and produce harmful substances during sintering. When using ceramic coating, ceramic coating will not produce harmful substances at the sintering temperature, thereby avoiding the unhealthy phenomenon caused by fluorine coating.
[0127] The pot body 1 is formed by a stretching process using a composite plate that has been etched.
[0128] After stretching, the surface of the pot body 1 is degreased by spraying an alkaline, acidic or neutral solvent onto the pot body 1 to remove the larger impurities.
[0129] After degreasing, the inner surface of the pot body 1 is sandblasted to clean and roughen the inner surface of the pot body 1 by the impact of high-speed sand flow. The sandblasting uses a mixture of 60 and 80 mesh brown corundum or white corundum. Sandblasting can increase the surface tension, provide physical and chemical bonding strength for the combination of the coating and the substrate, extend the durability of the coating, facilitate the leveling of the coating, and strengthen the direct bonding between the base oil layer of the ceramic coating and the pot blank. After sandblasting, the inner surface roughness of the pot body 1 is Ra2.5μm~4.0μm, and the inner surface of the pot body 1 is uniform everywhere.
[0130] Preheat the pot body 1 after sandblasting: The pot body temperature should be preheated to 50℃~60℃ before the pot body is sent to the spray room for primer spraying. The reason for preheating is that, on the one hand, the temperature difference between the pot body and the paint is too large, and the paint may solidify quickly after contacting the surface of the pot body due to the large temperature difference, affecting the normal adhesion of the paint to the pot body and the stability of the connection between the two; on the other hand, if the temperature of the pot body is too low, the paint may scatter due to the large temperature difference after contact, thus forming a number of solid particles that cannot be stably attached to the pot body. The solid particles, as impurities, will affect the adhesion of the paint to the pot body. After the pot body is preheated, the above problems can be effectively suppressed.
[0131] After preheating, spray the first protective layer 2: adjust the spray gun diameter to 1.0mm~1.5mm, and adjust the atomization pressure to 2.5Kg / cm 2 ~3.0Kg / cm 2 The thickness of the first protective layer 2 after spraying is 20 μm to 25 μm.
[0132] After spraying the first protective layer 2, it is dried for subsequent polishing: After spraying the first protective layer 2, it is dried in a sintering furnace at 100° C. to 110° C. for 7 to 15 minutes. The main purpose of this drying step is to solidify the surface of the first protective layer 2 for subsequent polishing.
[0133] Polishing is performed after drying: the pot body 1 is placed in the mold and kept rotating, and the first protective layer 2 is removed from the etched raised part and the part near the pot mouth without etched lines with 180-grit sandpaper, and then wiped with a scouring pad to remove large impurities.
[0134] After polishing, cleaning and dust removal are performed to remove the remaining small impurities to prevent the impurities from affecting the adhesion of the protective layer 31.
[0135] After cleaning, the pot body 1 is preheated for the second time: before spraying the protective layer 31 , the surface temperature of the pot body 1 is raised to 30° C. to 50° C.
[0136] The purpose of the secondary preheating is to avoid the problem of rapid solidification of the protective layer 31 during the secondary spraying, and it is also beneficial to reduce the impurities generated after the spraying of the protective layer 31, and improve the bonding stability of the non-stick layer 32 and the protective layer 31. In addition, considering that the first protective layer 2 has been formed before the secondary preheating, the highest temperature of the pot body after the secondary preheating needs to be less than or equal to the lowest temperature after preheating, that is, less than or equal to 50°C, so as to avoid the problem of the first protective layer 2 changing shape due to the high temperature of the pot body after preheating.
[0137] Spraying protective layer 31: Adjust the spray gun diameter to 1.0mm~1.5mm, and the atomization pressure to 2.0Kg / cm 2 ~2.5Kg / cm 2 The ceramic coating is sprayed to form a protective layer 31, and the thickness of the protective layer 31 is 3 μm to 5 μm. The protective layer 31 is in a semi-transparent state, that is, the protective layer 31 is a transparent protective layer with a certain color.
[0138] Spray the non-stick layer 32 immediately after spraying the protective layer 31: adjust the spray gun diameter to 1.0mm-1.5mm and the atomization pressure to 2.0Kg / cm 2 ~2.5Kg / cm 2, spraying ceramic coating to form a non-stick layer 32, the thickness of the non-stick layer 32 is 5μm to 7μm. The spraying process of the protective layer 31 and the non-stick layer 32 is completed continuously in a spray room, and a wet-spray-wet mode is adopted, that is, the non-stick layer 32 is sprayed immediately before the protective layer 31 is cured, so that the protective layer 31 is in a partially liquid form and adheres to the non-stick layer 32.
[0139] After spraying, the whole is cured: the pot body 1 is kept in an environment of 80°C to 150°C for 8 minutes to 15 minutes, and then the ambient temperature is raised to 220°C to 250°C and maintained for another 8 minutes to 15 minutes to complete the overall curing of the first protective layer 2, the protective layer 31 and the non-stick layer 32.
[0140] Final polishing: Use 180-grit sandpaper to remove the ceramic coating from the area without etching on the pot mouth of the pot body 1, and then wipe it with a towel to make the mouth of the cooking container smooth. Generally speaking, consumers do not have a non-stick requirement for the pot mouth, and the pot mouth is prone to bumps. Removing the ceramic coating from the pot mouth will not have a significant adverse effect on the performance of the cooking container, and it will also help reduce the risk of coating shedding due to abnormal actions such as bumps and knocks.
[0141] Table 1 shows the comparison of the effects of three experimental examples made by the manufacturing method of the above-mentioned cooking container and comparative example 5, wherein experimental example 5 uses a high-pressure air gun for cleaning and dust removal; experimental example 6 uses a high-pressure water gun for cleaning and dust removal and drying; experimental example 7 uses manual wiping for cleaning and dust removal; comparative example 5 does not perform cleaning and dust removal. In view of the fact that the protective layer 31 and the non-stick layer 32 are transparent, it is difficult to accurately judge whether there is any shedding by direct observation in some cases. Therefore, the non-stickiness of the cooking container after the simulated cooking test is used as an indirect evaluation method. If the non-stick effect decreases, it means that the coating has partially fallen off. Among them, the steps of the simulated cooking test refer to the national standard GB / T32095.4 Food Simulation Test Specifications and Evaluation Methods for a cyclic cooking test, and the non-stick test rating refers to the fried egg non-stick rating item of GB / T32388. The test results are as follows:
[0142] Table 3
[0143]
[0144] It can be seen that the non-stickiness of Comparative Example 5 dropped to Level 2 after one cycle, and the coating had visibly fallen off after three cycles, which shows that the coating of Comparative Example 5 fell off more obviously. However, Experimental Examples 5, 6, and 7, which were cleaned and dusted, still maintained Level 1 non-stickiness after one cycle, and the protective layer did not fall off visibly after five cycles. Obviously, the bonding strength of the non-stick coating was enhanced after cleaning and dusting.
[0145] It should be noted that the cooking containers in this application refer to various utensils used for cooking food, such as woks, frying pans, pressure cooker inner pots and steamers, including utensils that come into direct contact with open flames, utensils that are heated by electromagnetic means, etc., and also include utensils used for holding food in household appliances such as rice cookers, electric pressure cookers, soy milk makers, and food processors.
[0146] Anything not described in this application can be achieved by adopting or drawing on existing technologies.
[0147] Each embodiment in this specification is described in a progressive manner, and the same and similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. The above is only an embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.
Claims
1. A cooking container, characterized in that: It comprises a pot body having a cooking cavity, wherein a side surface of the pot body facing the cooking cavity is an inner surface; The inner surface is covered with a protective layer containing a non-stick component, and the protective layer includes: A first protective layer connected to the inner surface and covering a portion of the inner surface; the material of the first protective layer includes water-based ceramic coating; The second protective layer, the material of the second protective layer includes water-based ceramic coating and corrosion-resistant components, the mass proportion of the corrosion-resistant components in the second protective layer is Z, 3%wt≤Z≤20%wt.
2. The cooking container according to claim 1, characterized in that: The corrosion-resistant component includes titanium, and the first protective layer also includes the corrosion-resistant component; the mass proportion of titanium in the first protective layer is X, the mass proportion of titanium in the second protective layer is Y, |XY|≤5.
3. The cooking container according to claim 1, characterized in that: The inner surface is provided with a plurality of protrusions protruding outwards toward one side of the cooking cavity; the protrusions are higher than the adjacent first protective layer; The second protection layer covers the protrusion.
4. The cooking container according to claim 3, characterized in that: The second protective layer comprises: A protective layer connected to the raised portion and covering the raised portion; A non-stick layer connected to the protective layer, and the non-stick layer covers the protective layer and the first protective layer at the same time; Wherein, the materials of the first protective layer, the shielding layer and the non-stick layer all include fluorine coating or ceramic coating.
5. The cooking container according to claim 4, characterized in that: The first protective layer has a predetermined color, the protective layer is translucent, and the non-stick layer is transparent; Alternatively, the first protective layer has a predetermined color, the protection layer is transparent, and the non-stick layer is translucent.
6. The cooking container according to any one of claims 3 to 5, characterized in that: The second protective layer covers the first protective layer and the protrusion, and the second protective layer includes a first part and a second part, wherein a surface of the first part facing the cooking cavity is higher than a surface of the adjacent second part facing the cooking cavity.
7. The cooking container according to claim 6, characterized in that: Along the thickness direction of the pot body, for any adjacent first part and second part, the height difference between the highest point of the first part and the lowest point of the adjacent second part is h, and the maximum distance between the first part and the adjacent first part is L, 0.06≤h / L≤0.
5.
8. A method for manufacturing a cooking container, characterized in that: Used for producing a cooking container as described in any one of claims 1 to 7; The cooking container manufacturing method comprises the following steps: Forming step: processing a convex portion on the surface of the raw material, and forming the raw material into a pot blank with a cooking cavity; A first spraying step: spraying paint onto the inner surface to form a first protective layer; Curing step: drying the first protective layer to solidify the surface of the first protective layer; Second spraying step: spraying paint onto the pot blank to form a protective layer covering the raised portion; Wherein, the time interval between the end of the first spraying step and the start of the second spraying step is H, 1 hour≤H≤100 hours.
9. The method for manufacturing a cooking container according to claim 8, characterized in that: The coating used in the second spraying step comprises a first component and a second component, wherein the first component is a water-based ceramic coating, and the second component comprises at least one of a single titanium substance or a titanium alloy, and the mass proportion of the second component in the coating is A, 5%wt≤A≤25%wt.
10. The method for manufacturing a cooking container according to claim 8, characterized in that: The third spraying step is also included after the second spraying step: spraying coating on the pot blank to form a non-stick layer covering the protective layer; Wherein, the coatings used in the first spraying step, the second spraying step and the third spraying step all contain ceramic coatings.
Citation Information
Patent Citations
Titanium-containing ceramic paint and protective coating
CN103013193A
Pot and cooking utensil with same
CN110859518A
Ceramic coating for etching pot as well as preparation method and application of ceramic coating
CN117384546A
Cooking utensil
CN212698557U
Coating structure and coating method for inner surfaces of cookware