Photocatalyst for catalyzing carboxylic acid to efficiently convert into long-chain alkane as well as preparation method and application of photocatalyst

By using titanium dioxide support and uniformly dispersed Ag as the photocatalyst, the problems of high cost of precious metal catalysts and low selectivity of long-chain alkanes in the prior art are solved, and efficient catalytic production of C5-C20 alkanes are achieved, reducing the production of C5-C20 alkanes Cost and improve selectivity.

CN119056444AActive Publication Date: 2024-12-03JILIN UNIVERSITY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411167807.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-12-03
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

In the process of catalyzing the conversion of carboxylic acids into long-chain alkanes, existing photocatalysts have high precious metal content and low yield and selectivity of long-chain alkanes, and have higher costs.

Method used

Using titanium dioxide as a support, Ag with a particle size of 0.3 to 1 nm is uniformly dispersed as active components to prepare a photocatalyst with a low Ag content, which is prepared by room temperature stirring and calcining reduction method, and is used to catalyze the conversion of C5 to C20 carboxylic acid to C5 to C5 to C5 to C5 to C20 alkane.

Benefits of technology

The yield and selectivity of C5-C20 alkanes are significantly improved, the cost is reduced, and the catalytic activity is improved. It is especially suitable for the production of long-chain alkanes. The selectivity of C5-C20 alkanes is as high as 97%, and the yield is greater than 78%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056444A_ABST
    Figure CN119056444A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of catalysts, and relates to a photocatalyst for catalyzing carboxylic acid to efficiently convert into long-chain alkane as well as a preparation method and application thereof. According to the photocatalyst, titanium dioxide serves as a carrier, Ag with the particle size being 0.3-1 nm serves as an active component, the proportion of the active component in the photocatalyst is 0.1 wt%-1 wt%, the dosage is small, and the cost is low. When the catalyst is used for catalyzing carboxylic acid to be converted into alkane, the conversion rate of various carboxylic acids can reach 97% or above, and C5-C20 alkane has high yield and selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalysts and relates to a photocatalyst for catalyzing carboxylic acids to efficiently convert long-chain alkanes, and a preparation method and application thereof. Background Art

[0002] Biodiesel refers to a renewable diesel fuel that can replace petrochemical diesel, which is made from oil crops such as soybeans, rapeseed, cotton, palm, wild oil plants and aquatic plant oils such as engineered microalgae, animal fats, and restaurant waste oil through ester exchange or thermochemical processes. Its main component is C5-C20 alkanes. C5-C20 alkanes can not only be used as the main component of biodiesel and jet fuel, but also as raw materials for the production of olefins and aromatics. In order to achieve sustainable development, existing technologies use fatty acids to replace non-renewable fossil resources to produce C5-C20 alkanes.

[0003] At present, the methods for preparing C5-C20 alkanes from fatty acids mainly include transesterification, thermochemical conversion, hydrogenation and photocatalysis. Among them, the photocatalysis method is favored by scientists because of its mild reaction conditions and low energy consumption. Precious metal catalysts are widely used in the production of C5-C20 alkanes from photocatalytic fatty acids. Such catalysts have excellent catalytic activity and low-temperature activity at normal pressure. The precious metals used mainly include elements such as Pt, Pd, and Au, but the content of precious metals is generally high, and the yield of long-chain alkanes is low. For example, in the Chinese patent literature with publication number CN111233603 A and publication date June 5, 2020, titanium dioxide is used as a carrier and precious metals Pt, Pd, Au, Ag, and Ru are used as active components. When 1wt% of Ag is used as the active component, the yield of long-chain alkanes is only 68%. In addition, the free radicals in the process of photocatalytic conversion of carboxylic acids to alkanes tend to form chain extension products through CC free radical coupling, and the selectivity of C5-C20 alkanes is usually less than 50%. Summary of the invention

[0004] The present invention provides a photocatalyst for catalyzing the efficient conversion of carboxylic acids into long-chain alkanes, and a preparation method and application thereof, with the aim of reducing the cost of existing photocatalysts for catalyzing the conversion of C5-C20 carboxylic acids into C5-C20 alkanes and improving the selectivity of C5-C20 alkanes.

[0005] In order to achieve the above invention objectives, the present invention uses titanium dioxide as a carrier and Ag as an active component to prepare a photocatalyst for catalyzing the decarboxylation of carboxylic acids to prepare alkanes. The photocatalyst can greatly improve the yield and selectivity of alkanes, and is particularly suitable for the production of long-chain alkanes, i.e., C5 to C20 alkanes.

[0006] The first aspect of the present invention provides a photocatalyst for catalyzing the conversion of carboxylic acid into alkane, comprising:

[0007] A carrier, wherein the carrier is titanium dioxide;

[0008] An active component, wherein the active component is Ag, which is uniformly dispersed in the carrier and has a particle size of 0.3 to 1 nm;

[0009] The average particle size of the photocatalyst is 1 μm;

[0010] The proportion of the active component in the photocatalyst is X, 0.1wt%≤X≤1wt%.

[0011] In any embodiment of the present invention, the photocatalyst is used to catalyze the conversion of C5-C20 carboxylic acids into C5-C20 alkanes. Furthermore, the photocatalyst is used to catalyze the conversion of C5-C20 saturated fatty acids into C5-C20 alkanes.

[0012] In any embodiment of the present invention, the proportion of the active component in the photocatalyst is X, 0.25wt%≤X≤1.0wt%. Further, 0.25wt%≤X≤0.50wt%. Further, X is 0.25wt%.

[0013] The second aspect of the present invention provides a method for preparing the above-mentioned photocatalyst for catalyzing the conversion of carboxylic acid into alkane, comprising the following steps:

[0014] A titanium source is added dropwise to acetic acid, and then a soluble precursor of Ag is added, and the mixture is stirred at room temperature until the solution turns white to obtain a precursor liquid;

[0015] The precursor liquid is kept at 120-150°C for 10-30 hours, cooled naturally and centrifuged, the white precipitate is collected, washed, dried and crushed;

[0016] The crushed material is fully calcined in an oxygen atmosphere at 400-650°C, and the calcined product is cooled to room temperature and then placed in a hydrogen-containing atmosphere at 350-500°C for full reduction to obtain the above-mentioned photocatalyst for catalyzing the conversion of carboxylic acid into alkane.

[0017] In some embodiments of the present invention, the titanium source is one or more of tetrabutyl titanate, tetraisopropyl titanate, tetraethyl titanate, and tetramethyl titanate.

[0018] The third aspect of the present invention provides another method for preparing the above-mentioned photocatalyst for catalyzing the conversion of carboxylic acid into alkane, comprising the following steps:

[0019] TiO 2 The nanoparticles were dispersed in deionized water to obtain TiO 2 Suspension;

[0020] TiO 2 Add a soluble precursor of Ag to the suspension, mix thoroughly, dry, and crush;

[0021] The crushed material is fully calcined in an oxygen atmosphere at 400-650°C, and the calcined product is cooled to room temperature and then placed in a hydrogen-containing atmosphere at 350-500°C for full reduction to obtain the above-mentioned photocatalyst for catalyzing the conversion of carboxylic acid into alkane.

[0022] In some embodiments of the present invention, the soluble precursor of Ag is silver nitrate or silver ammonia solution.

[0023] In some embodiments of the present invention, the oxygen-containing atmosphere is air; and the hydrogen-containing atmosphere is hydrogen.

[0024] The fourth aspect of the present invention provides the use of the above-mentioned photocatalyst for catalyzing the conversion of carboxylic acids into alkanes in the production of alkanes. Preferably, the alkanes are C5 to C20 alkanes. Preferably, the production of alkanes is a step in the production of biodiesel.

[0025] A fifth aspect of the present invention provides a method for producing alkanes by photocatalytic carboxylic acid, comprising the following steps:

[0026] placing a carboxylic acid, the photocatalyst for catalyzing the conversion of the carboxylic acid into an alkane, and an organic solvent in a photoreactor;

[0027] The reaction is stirred at room temperature, in an oxygen-free atmosphere and under ultraviolet light irradiation to obtain an alkane.

[0028] In the present invention, the carboxylic acid is a fatty acid; preferably, the carboxylic acid is a saturated fatty acid; more preferably, the carboxylic acid is a C5-C20 saturated fatty acid, which is used to prepare C5-C20 alkanes; in some embodiments of the present invention, the carboxylic acid is one or more of stearic acid, palmitic acid, arachidic acid, myristic acid, and lauric acid.

[0029] In some embodiments of the present invention, the oxygen-free atmosphere is one of hydrogen, nitrogen, inert gas, nitrogen containing hydrogen, and inert gas containing hydrogen; and / or the gas pressure is 0.1 to 4 MPa. Preferably, it is a hydrogen atmosphere, and the gas pressure is preferably 0.2 to 4 MPa.

[0030] In some embodiments of the present invention, the photoreactor is purged with hydrogen before ultraviolet light irradiation and the hydrogen pressure in the photoreactor is controlled to be 0.1-4 MPa.

[0031] In some embodiments of the present invention, the organic solvent is C8-C16 alkane or acetonitrile; and / or the ultraviolet light uses an LED light source with a power of 10 to 40 W.

[0032] Compared with the prior art, the present invention has at least the following beneficial effects:

[0033] 1. The precious metal loaded on the photocatalyst for catalyzing the conversion of carboxylic acid into alkane of the present invention is Ag, and the Ag content is very low, which reduces the cost compared with the existing photocatalyst for catalyzing the conversion of carboxylic acid into alkane.

[0034] 2. The photocatalyst for catalyzing the conversion of carboxylic acids into alkanes of the present invention can increase the conversion rate of five common fatty acids to more than 97% under normal temperature and pressure reaction conditions, and the yield of the corresponding target alkanes is greater than 78%, and the selectivity of the target alkanes is relatively high. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0036] Figure 1 :Ag / TiO 2 SEM images of the catalysts; (a) Ag / TiO 2 -1; (b) Ag / TiO 2 -2; (c) Ag / TiO 2 -3; (d) Ag / TiO 2 -4.

[0037] Figure 2 :Ag / TiO 2 -3's EDS element distribution and analysis diagram, from left to right are Ag, Ti, and O elements.

[0038] Figure 3 :Ag / TiO 2 XRD patterns of the catalysts.

[0039] Figure 4 : Stearic acid conversion activity diagram of the catalyst prepared in Example 1; wherein, (a) stearic acid conversion rate and heptadecane selectivity; (b) stearic acid conversion rate and heptadecane selectivity at different reaction times and in different atmospheres.

[0040] Figure 5 :Ag / TiO 2 -3 fatty acid conversion activity diagram.

[0041] Figure 6 : Stearic acid conversion activity diagram of the catalyst prepared in Example 2.

[0042] Figure 7 : Stearic acid conversion activity diagram of the catalyst prepared in Example 3.

[0043] Figure 8 : Stearic acid conversion activity diagram of catalysts loaded with different active components.

[0044] Fig. 9 :(a) Ag / TiO 2 Photocurrent (It); (b) Ag / TiO 2 Electrochemical impedance spectroscopy (EIS) graph. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] For simplicity, only some numerical ranges are explicitly disclosed herein. However, any lower limit can be combined with any upper limit to form an unambiguous range; and any lower limit can be combined with other lower limits to form an unambiguous range. Similarly, any upper limit can be combined with any other upper limit to form an unambiguous range. In addition, although not explicitly stated, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unambiguous range.

[0047] It should be noted that, in the description of this article, unless otherwise specified, "above", "below" include the number, and the meaning of "multiple" in "one or more" is two or more. Relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "including one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements.

[0048] In the description of this specification, the description with reference to the terms "any embodiment / method", "one embodiment / method", "some embodiments / methods", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments / methods or examples. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, unless they are contradictory.

[0049] In the description of the present invention, the term "conversion rate" refers to the percentage of the amount of a reactant converted after participating in the reaction to the initial amount of the reactant, for example:

[0050]

[0051] In the description of the present invention, the term "yield" refers to the ratio of the amount of reactant converted to the target product to the initial amount of the reactant, for example:

[0052]

[0053] In the description of the present invention, the term "selectivity" refers to the ratio of the amount of reactant converted into the target product in the system to the total amount of the reactant converted by participating in all reactions, for example:

[0054]

[0055] Heptadecane yield = stearic acid conversion rate × heptadecane selectivity.

[0056] The above summary of the invention of the present invention is not intended to describe each disclosed embodiment or each implementation in the present invention. The following description more specifically illustrates exemplary embodiments. These embodiments can be used in various combinations. In each example, the enumeration is only used as a representative group and should not be interpreted as exhaustive.

[0057] As described in the background technology, the noble metal catalyst widely used in the production of biodiesel by photocatalytic fatty acids in the prior art has a generally high content of noble metals, and the yield of long-chain alkanes is low. The Chinese patent literature with publication number CN116217333A and publication date June 6, 2023 discloses a method for obtaining olefins from a variety of carboxylic acids under illumination, and the carrier of the catalyst used in the method is a mixture of rutile phase and anatase phase titanium dioxide with a weight ratio of 3: 1, and the active component loaded is Au, Rh or Pd, and the active component content is relatively high. The catalyst can prepare carboxylic acids into olefins, and it is not disclosed that it can prepare carboxylic acids into alkanes.

[0058] A Chinese patent document with publication number CN111233603 A and publication date June 5, 2020 discloses a method for preparing alkanes by hydrogenation photocatalytic decarboxylation of fatty acids. The method comprises mixing fatty acids, catalysts and solvents, placing them in a quartz reactor, replacing the atmosphere in the reactor with hydrogen and sealing it, stirring without adding light to cause a hydrogenation reaction, and then irradiating with an external light source to cause a decarboxylation reaction to generate alkanes. The catalysts used in the method mostly use precious metals as active components. When 1wt% of Ag is used as the active component, the yield of long-chain alkanes is only 68%.

[0059] The inventors have found that when a photocatalyst with titanium dioxide as a carrier, Ag with a loaded particle size of 0.3 to 1 nm as an active component and a loading amount of 0.1 wt% to 1 wt% is used to photocatalyze the conversion of carboxylic acids into alkanes, the selectivity for C5 to C20 alkanes is high, and the yield is greater than 70%. In particular, when the Ag content is 0.25 wt% to 1.0 wt%, the selectivity for C5 to C20 alkanes is as high as more than 95%, and the yield is more than 85%; in particular, when the Ag content is 0.25 wt%, the selectivity and yield of C5 to C20 alkanes are both the highest, and the cost is greatly reduced relative to existing catalysts.

[0060] The prior art believes that the principle of photocatalytic conversion of carboxylic acids into alkanes is:

[0061] R-CH 2 CH 2 COOH→R-CH 2 CH 2 COO - +H + (1)

[0062]

[0063] H + +e - →H · (3)

[0064] H · +H· →H 2 (4)

[0065]

[0066]

[0067]

[0068]

[0069] The free radicals in this process tend to form chain-extended products with more than 20 carbon atoms through CC free radical coupling, and the selectivity of C5-C20 alkanes is usually less than 50%.

[0070] The photocatalyst of the present invention uses titanium dioxide as a carrier and carries Ag as an active component. Titanium dioxide can generate photocurrent under ultraviolet light irradiation, showing excellent photogenerated charge transfer and separation efficiency, which is conducive to reducing H+ to H·, and promoting the coupling of alkyl free radicals and H· to generate alkanes. The photocatalyst has the function of inhibiting free radical oligomerization. The photocatalyst can convert carboxylic acid into alkanes in either hydrogen atmosphere or nitrogen atmosphere, especially when catalyzing carboxylic acid into alkanes in hydrogen atmosphere at normal temperature and pressure, the selectivity of C5-C20 alkanes is as high as 97%. In addition, the photocatalyst only carries ≤1wt% of the active component Ag, and the cost is very low.

[0071] Photocatalyst

[0072] The photocatalyst for catalyzing the conversion of carboxylic acid into alkane provided by the present invention comprises:

[0073] A carrier, wherein the carrier is titanium dioxide;

[0074] An active component, wherein the active component is Ag, which is uniformly dispersed in the carrier and has a particle size of 0.3 to 1 nm;

[0075] The average particle size of the photocatalyst is 1 μm;

[0076] The proportion of the active component in the photocatalyst is X, 0.1wt%≤X≤1wt%.

[0077] The average particle size of the photocatalyst is 1 μm, and the loaded active component is Ag with a particle size of 0.3 to 1 nm. When the loading amount is 0.1 wt% to 1 wt%, the yield of preparing alkanes by hydrodeoxygenation of carboxylic acids can reach more than 70%, and the conversion rate of alkanes can reach more than 95%, which reduces the cost compared with existing catalysts.

[0078] In some embodiments of the present invention, the photocatalyst is in the shape of a sea urchin, which further increases the specific surface area, can improve its catalytic activity, and improve the conversion rate of alkanes.

[0079] The proportion of the active component Ag in the photocatalyst of the present invention is X, 0.25wt%≤X≤1.0wt%, X can control the yield of alkanes to be greater than 80% within the above range, and the photocatalyst can ensure a higher C5-C20 alkane yield (>78%) and a carboxylic acid conversion rate at normal temperature and pressure (>97%). Further, 0.25wt%≤X≤0.50wt%, the cost of the photocatalyst is further reduced, and the yield and selectivity of C5-C20 alkanes are not affected. Further, X is 0.25wt%, the cost of the catalyst is further reduced, and the yield and selectivity of C5-C20 alkanes are both the highest. Optionally, the proportion of Ag in the photocatalyst includes but is not limited to 0.10wt%, 0.20wt%, 0.25wt%, 0.30wt%, 0.40wt%, 0.50wt%, 0.60wt%, 0.70wt%, 0.80wt%, 0.90wt%, 1.0wt%.

[0080] In some embodiments of the present invention, the titanium dioxide is anatase phase titanium dioxide or rutile phase titanium dioxide.

[0081] Preparation method

[0082] The present invention provides a method for preparing the above-mentioned photocatalyst for catalyzing the conversion of carboxylic acid into alkane, comprising the following steps:

[0083] A titanium source is added dropwise to acetic acid, and then a soluble precursor of Ag is added, and the mixture is stirred at room temperature until the solution turns white to obtain a precursor liquid;

[0084] The precursor liquid is kept at 120-150°C for 10-30 hours, cooled naturally and centrifuged, the white precipitate is collected, washed, dried and crushed;

[0085] The crushed material is fully calcined in an oxygen atmosphere at 400-650°C, and the calcined product is cooled to room temperature and then placed in a hydrogen-containing atmosphere at 350-500°C for full reduction to obtain the above-mentioned photocatalyst for catalyzing the conversion of carboxylic acid into alkane.

[0086] The method loads the active component on the carrier while the carrier anatase phase titanium dioxide is formed. The method can make the active component more evenly dispersed on the carrier, and the utilization rate of the soluble precursor of the active component is high. The crushed material is fully calcined in an oxygen atmosphere at 400-650°C, and the oxide of the active component is obtained while obtaining the anatase phase titanium dioxide. After the calcined product is cooled to room temperature, it is placed in a hydrogen-containing atmosphere at 350-500°C for full reduction, so that the oxide of the active component can be reduced to the zero-valent metal of the active component. Starting from simple and easily available raw materials, the method does not separate intermediates, and continuously performs multiple steps of reaction, which reduces the synthesis time and cost, and the steps are simple and easy to operate.

[0087] In some embodiments of the present invention, the titanium source is one or more of tetrabutyl titanate, tetraisopropyl titanate, tetraethyl titanate, and tetramethyl titanate. These titanium sources can form a white precipitate, i.e., an amorphous titanium dioxide sol, in the presence of acetic acid. During this process, the titanium dioxide sol can maximize the adsorption and encapsulation of the soluble precursor of the active component, thereby fully utilizing the soluble precursor of the active component.

[0088] The present invention provides another method for preparing the above-mentioned photocatalyst for catalyzing the conversion of carboxylic acid into alkane, comprising the following steps:

[0089] TiO 2 The nanoparticles were dispersed in deionized water to obtain TiO 2 Suspension;

[0090] TiO 2 Add a soluble precursor of Ag to the suspension, mix thoroughly, dry, and crush;

[0091] The crushed material is fully calcined in an oxygen atmosphere at 400-650°C, and the calcined product is cooled to room temperature and then placed in a hydrogen-containing atmosphere at 350-500°C for full reduction to obtain the above-mentioned photocatalyst for catalyzing the conversion of carboxylic acid into alkane.

[0092] This method uses homemade or commercially available TiO 2 To prepare the photocatalyst, the Ag soluble precursor is dissolved in water and immersed in TiO 2 The photocatalyst can be obtained by drying the nanoparticles and then calcining and reducing them in sequence. The method is simple and easy to operate.

[0093] The soluble precursor of Ag used in the above two methods is silver nitrate or silver ammonia solution.

[0094] The calcination and reduction in the above two methods can be carried out by the same means. In some embodiments, for the sake of simplicity, the oxygen atmosphere is selected as air, and the hydrogen-containing atmosphere is selected as hydrogen, but this should not be regarded as a limitation of the oxygen atmosphere and the hydrogen-containing atmosphere of the present invention. Those skilled in the art can also select an inert gas mixed with oxygen or nitrogen mixed with oxygen as the oxygen atmosphere, and an inert gas mixed with hydrogen or nitrogen mixed with hydrogen as the hydrogen-containing atmosphere.

[0095] In the above two methods, the purpose of pulverization is to make the photocatalyst calcined and reduced more fully, and there is no need to limit the particle size of the pulverized material. There is no obvious change in the pulverized material before and after calcination and before and after reduction.

[0096] application

[0097] The present invention uses the above-mentioned photocatalyst for catalyzing the conversion of carboxylic acid into alkane to catalyze the conversion of carboxylic acid into alkane, especially for catalyzing the hydrodeoxygenation of C5-C20 saturated fatty acids to prepare C5-C20 alkanes, and this application can be a link in the production of biodiesel. For example, when using a mixture of C5-C20 saturated fatty acids and oils to produce biodiesel, the C5-C20 saturated fatty acids are first catalyzed to be hydrodeoxygenated to prepare C5-C20 alkanes, and then the oils are catalyzed to form long-chain alkanes, or the oils are first catalyzed to form long-chain alkanes, and then the C5-C20 saturated fatty acids are hydrodeoxygenated to prepare C5-C20 alkanes.

[0098] Method for producing alkanes by photocatalysis of carboxylic acid

[0099] The present invention uses the above-mentioned photocatalyst for catalyzing the conversion of carboxylic acid into alkane to catalyze the conversion of carboxylic acid into alkane. The provided method for photocatalytically converting carboxylic acid into alkane comprises: placing carboxylic acid, the above-mentioned photocatalyst for catalyzing the conversion of carboxylic acid into alkane, and an organic solvent in a photoreactor; stirring the reaction at room temperature, in an oxygen-free atmosphere, and under ultraviolet light irradiation to obtain alkane.

[0100] The method for producing alkanes from carboxylic acids using photocatalysis can rapidly prepare alkanes at room temperature, and both the yield and selectivity of the alkanes are high.

[0101] In the present invention, the carboxylic acid is a fatty acid; preferably, the carboxylic acid is a saturated fatty acid; more preferably, the carboxylic acid is a C5-C20 saturated fatty acid, and the method is used to prepare C5-C20 alkanes with high yield and selectivity; in some embodiments of the present invention, the carboxylic acid is one or more of stearic acid, palmitic acid, arachidic acid, myristic acid, and lauric acid. These carboxylic acids can be converted into C5-C20 alkanes with extremely high C5-C20 alkane selectivity and high yield under the conditions of the above photocatalyst.

[0102] In some embodiments of the present invention, the oxygen-free atmosphere is one of hydrogen, nitrogen, an inert gas, nitrogen containing hydrogen, and an inert gas containing hydrogen; and / or the gas pressure is 0.1 to 4 MPa. Preferably, it is a hydrogen atmosphere, and the gas pressure is preferably 0.2 to 4 MPa. Preferably, the photoreactor is purged with hydrogen before ultraviolet light irradiation and the hydrogen pressure in the photoreactor is controlled to be 0.1 to 4 MPa. The hydrogen pressure can be between 0.1 and 4 MPa, and the reaction can be carried out at normal pressure (0.1 MPa) or at high pressure (0.2 to 4 MPa). A higher carboxylic acid conversion rate (>97%) can be guaranteed at normal temperature and pressure, and the conversion rate will be higher during high pressure reaction.

[0103] In some embodiments of the present invention, the organic solvent used in the above-mentioned method for producing alkanes from photocatalytic carboxylic acids is C8-C16 alkane or acetonitrile. The ultraviolet light uses an LED light source with a power of 10-40W; preferably, the ultraviolet light uses an LED light source with a central wavelength of 365nm and a power of 40W.

[0104] Example

[0105] The following are examples of the present invention. The examples described below are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention. If the specific technology or conditions are not specified in the examples, they shall be carried out according to the technology or conditions described in the literature in the field or according to the product instructions. The reagents or instruments used without indicating the manufacturer are all conventional products that can be obtained commercially. The anatase phase titanium dioxide used in the present invention can be conventional commercially available anatase phase titanium dioxide, or it can be prepared by the following method: Preparation method of anatase phase titanium dioxide: add 30mL of acetic acid to a 50mL polytetrafluoroethylene container, add 100μL of deionized water; then add 1mL of tetrabutyl titanate, stir at room temperature for about 2h, wait until the solution turns white, transfer the polytetrafluoroethylene container to a stainless steel autoclave, keep it at 140°C for 24 hours, and then let it cool naturally in the air. Centrifuge, collect the white precipitate, wash it thoroughly with ethanol and water, and then dry it at 60°C for 3 hours. The dried product is then placed in a muffle furnace and completely calcined at 650° C. for 3 hours, and the resulting calcined product is anatase phase titanium dioxide.

[0106] Example 1: One-pot preparation of Ag / TiO 2 catalyst

[0107] Add 30 mL of acetic acid into a 50 mL polytetrafluoroethylene container, add 1 mL of tetrabutyl titanate, and add AgNO 3, stirred at room temperature for about 2 hours, and when the solution turned white, the polytetrafluoroethylene container was transferred to a stainless steel autoclave, kept at 140°C for 24 hours, and then allowed to cool naturally in the air. Centrifuged, the white precipitate was collected, thoroughly washed with ethanol and water, and then dried at 60°C for 3 hours. The dried product was then placed in a muffle furnace and completely calcined at 650°C for 3 hours; after cooling to room temperature, the sample was then placed in a hydrogen atmosphere, heated to 500°C at a heating rate of 1°C / min, and reduced at 500°C in a hydrogen atmosphere for 5 hours to obtain Ag / TiO 2 catalyst.

[0108] Press AgNO 3 The addition amount was different to obtain Ag / TiO with Ag mass fraction of 0wt%, 0.05wt%, 0.10wt%, 0.25wt%, 0.50wt%, 1.0wt%, and 2wt%. 2 The catalysts are named TiO 2 、Ag / TiO 2 -1. Ag / TiO 2 -2. Ag / TiO 2 -3. Ag / TiO 2 -4. Ag / TiO 2 -5. Ag / TiO 2 -6.

[0109] Example 2: Preparation of Ag / TiO by impregnation-calcination method 2 -A Catalyst

[0110] 1. Disperse commercially available anatase titanium dioxide nanoparticles in deionized water to obtain TiO 2 Suspension; each TiO 2 The suspension consisted of 30 mL of deionized water and 1 g of carrier. 2 The mass fraction of the catalyst is 0wt%, 0.05wt%, 0.10wt%, 0.25wt%, 0.50wt%, 1.0wt%, 2wt% to each portion of TiO 2 Different amounts of AgNO were added to the suspension. 3 powders and mix well to obtain a slurry.

[0111] 2. The slurry was stirred overnight at ambient temperature and in the dark, and then dried at 100.5°C for 12 hours. The obtained solid was crushed in a quartz boat to obtain Ag / TiO 2 powder.

[0112] 3. Ag / TiO 2The powder was first calcined at 400 °C in a muffle furnace for 4 h, cooled to room temperature at a cooling rate of 10 °C / min, and then placed in a hydrogen atmosphere and heated to 500 °C at a heating rate of 1 °C / min, and maintained at 500 °C for 5 h to obtain Ag / TiO 2 Catalyst. Ag / TiO with Ag mass fraction of 0wt%, 0.05wt%, 0.10wt%, 0.25wt%, 0.50wt%, 1.0wt%, and 2wt% 2 The catalysts were named TiO 2 -A, Ag / TiO 2 -A1, Ag / TiO 2 -A2, Ag / TiO 2 -A3, Ag / TiO 2 -A4, Ag / TiO 2 -A5, Ag / TiO 2 -A6.

[0113] Example 3: Preparation of Ag / TiO by impregnation-calcination method 2 -R Catalyst

[0114] 1. Disperse commercially available rutile titanium dioxide nanoparticles in deionized water to obtain TiO 2 Suspension; each TiO 2 The suspension consisted of 30 mL of deionized water and 1 g of carrier. 2 The mass fraction of the catalyst is 0wt%, 0.05wt%, 0.10wt%, 0.25wt%, 0.50wt%, 1.0wt%, 2wt% to each portion of TiO 2 Different amounts of AgNO were added to the suspension. 3 powders and mix well to obtain a slurry.

[0115] 2. The slurry was stirred overnight at ambient temperature and in the dark, and then dried at 100.5°C for 12 hours. The obtained solid was crushed in a quartz boat to obtain Ag / TiO 2 powder.

[0116] 3. Ag / TiO 2 The powder was first calcined at 400 °C in a muffle furnace for 4 h, cooled to room temperature at a cooling rate of 10 °C / min, and then placed in a hydrogen atmosphere and heated to 500 °C at a heating rate of 1 °C / min, and maintained at 500 °C for 5 h to obtain Ag / TiO 2 Catalyst. Ag / TiO with Ag mass fraction of 0wt%, 0.05wt%, 0.10wt%, 0.25wt%, 0.50wt%, 1.0wt%, and 2wt% 2The catalysts were named TiO2-R, Ag / TiO 2 -R1, Ag / TiO 2 -R2, Ag / TiO 2 -R3, Ag / TiO 2 -R4, Ag / TiO 2 -R5, Ag / TiO 2 -R6.

[0117] Example 4: 0.25wt% platinum-based titanium dioxide catalyst (0.25wt% Pt / TiO 2 )

[0118] 1. Disperse commercially available anatase titanium dioxide nanoparticles in deionized water to obtain TiO 2 Suspension; each TiO 2 The suspension consisted of 30 mL of deionized water and 1 g of support. 2 The mass fraction of the catalyst is 0.25wt% TiO 2 Add H 2 PtCl 6 powders and mix well to obtain a slurry.

[0119] 2. The slurry was stirred overnight at ambient temperature and in the dark, and then dried at 100.5°C for 12 hours. The obtained solid was crushed in a quartz boat to obtain Pt / TiO 2 powder.

[0120] 3. Pt / TiO 2 The powder was first placed in a muffle furnace, calcined at 400 °C in an air atmosphere for 4 hours, and then cooled to room temperature at a cooling rate of 10 °C / min; then placed in a hydrogen atmosphere, heated to 350 °C at a heating rate of 1 °C / min, and maintained at 350 °C for 4 hours to obtain Pt / TiO 2 Catalyst, named 0.25wt%Pt / TiO 2 .

[0121] Example 5: 0.25wt% gold-based titanium dioxide catalyst (0.25wt% Au / TiO 2 )

[0122] 1. Disperse commercially available anatase titanium dioxide nanoparticles in deionized water to obtain TiO 2 Suspension; each TiO 2 The suspension consisted of 30 mL of deionized water and 1 g of carrier. 2 The mass fraction of the catalyst is 0.25wt% TiO 2 Add H2 AuCl 6 powders and mix well to obtain a slurry.

[0123] 2. The slurry was stirred overnight at ambient temperature and in the dark, and then dried at 100.5°C for 12 hours. The obtained solid was crushed in a quartz boat to obtain Au / TiO 2 powder.

[0124] 3. Au / TiO 2 The powder was first placed in a muffle furnace, calcined at 400 °C in an air atmosphere for 4 hours, and then cooled to room temperature at a cooling rate of 10 °C / min; then placed in a hydrogen atmosphere, heated to 350 °C at a heating rate of 1 °C / min, and maintained at 350 °C for 4 hours to obtain Au / TiO 2 Catalyst, named 0.25wt% Au / TiO 2 .

[0125] Example 6: 0.25wt% ruthenium-based titanium dioxide catalyst (0.25wt%Ru / TiO 2 )

[0126] 1. Disperse commercially available anatase titanium dioxide nanoparticles in deionized water to obtain TiO 2 Suspension; each TiO 2 The suspension consisted of 30 mL of deionized water and 1 g of carrier. 2 The mass fraction of the catalyst is 0.25wt% TiO 2 RuCl was added to the suspension 3 powders and mix well to obtain a slurry.

[0127] 2. The slurry was stirred overnight at ambient temperature and in the dark, and then dried at 100.5°C for 12 hours. The obtained solid was crushed in a quartz boat to obtain Ru / TiO 2 powder.

[0128] 3. Ru / TiO 2 The powder was first placed in a muffle furnace, calcined at 400 °C in an air atmosphere for 4 hours, and then cooled to room temperature at a cooling rate of 10 °C / min; then placed in a hydrogen atmosphere, heated to 350 °C at a heating rate of 1 °C / min, and maintained at 350 °C for 4 hours to obtain Ru / TiO 2 Catalyst, named 0.25wt%Ru / TiO 2 .

[0129] test:

[0130] Ag / TiO 2 Catalyst morphology:

[0131] The Ag / TiO prepared in Example 1 2 The catalyst was scanned by electron microscope. Figure 1 As shown in the SEM images, Ag / TiO 2 -3 sea urchin-shaped ( Figure 1 c), Ag / TiO 2 -3 has an average particle size of about 1 μm, Ag / TiO 2 -1( Figure 1 a) Ag / TiO 2 -2( Figure 1 b) and Ag / TiO 2 -4( Figure 1 d) Average particle size and Ag / TiO 2 -3 have a similar average particle size.

[0132] Ag / TiO 2 Elemental analysis of catalyst:

[0133] Energy dispersive X-ray spectrometer (EDS) was used to detect the Ag / TiO 2 -3 in Ag, Ti, O elements. Figure 2 As shown in the SEM images, Ag / TiO 2 -3 catalyst has uniform distribution of Ti and O elements, and in the Ag / TiO 2 -3 Highly dispersed and uniformly loaded Ag can be seen on the surface, and the particle size of Ag is 0.3-1nm.

[0134] Ag / TiO 2 Crystallization analysis of catalyst:

[0135] The Ag / TiO prepared in Example 1 was detected by X-ray powder diffraction (XRD). 2 The crystallinity of the catalyst. Figure 3 The X-ray powder diffraction pattern of Ag / TiO 2 -1. Ag / TiO 2 -2. Ag / TiO 2 -3. Ag / TiO 2 -4 All four catalysts are in anatase phase, Ag / TiO 2 -1 has the highest crystallinity. As the Ag content increases, part of the Ag enters the TiO 2 lattice, resulting in a gradual decrease in crystallinity. Figure 3 There is no Ag diffraction peak in the MgO2 phase, indicating that metallic Ag is highly dispersed in the anatase phase of TiO2.

[0136] Ag / TiO 2 Stearic acid conversion activity test of catalyst:

[0137] The TiO prepared in Example 1 2 、Ag / TiO 2 -1. Ag / TiO 2 -2. Ag / TiO 2 -3. Ag / TiO 2 -4. Ag / TiO 2 -5. Ag / TiO 2 -6 was used to test the stearic acid conversion activity. The test conditions were as follows: 30 mg of stearic acid, 20 mg of a single photocatalyst, and 10 mL of acetonitrile were placed in a stainless steel photoreactor; the stainless steel photoreactor was heated with H 2 or N 2 The stainless steel photoreactor was purged five times and pressurized to 0.1 MPa. When the temperature reached 28°C, the stainless steel photoreactor was irradiated with an LED light source (central wavelength of 365 nm, power of 40 W), the stirring rate was 1000 rpm, and the reaction time was 2 h.

[0138] like Figure 4 The stearic acid conversion activity shown by Ag / TiO 2 -3 and Ag / TiO 2 -4 as a photocatalyst, the conversion rate of stearic acid reached more than 95%, and Ag / TiO 2 -1 as a photocatalyst has a much higher conversion rate of stearic acid than TiO 2 As a photocatalyst. Figure 4 As shown in (a), the Ag / TiO 2 The yield of catalytic acid can reach more than 80%, and the conversion rate of stearic acid is more than 95%, showing super high catalytic activity. Figure 4 (b) shows that, compared with N 2 Compared with the air, Ag / TiO 2 -3 in H 2 The yield of stearic acid converted to heptadecane in the presence of H 2 The atmosphere significantly affects the adsorption and decarboxylation of the acid.

[0139] Ag / TiO 2 Catalyst conversion activity for different fatty acids:

[0140] The Ag / TiO prepared in Example 1 2 -3 was used to test the conversion activity of five fatty acids, namely stearic acid, palmitic acid, arachidic acid, myristic acid, and lauric acid. The test conditions were as follows: 30 mg of a single fatty acid, 20 mg of a photocatalyst, and 10 mL of acetonitrile were placed in a stainless steel photoreactor; the stainless steel photoreactor was heated with H 2The hydrogen pressure in the stainless steel photoreactor was purged five times and pressurized to 0.1 MPa. When the temperature reached 28°C, the stainless steel photoreactor was irradiated with an LED light source (central wavelength of 365 nm, power of 40 W), the stirring rate was 1000 rpm, and the reaction time was 2 h.

[0141] like Figure 5 As shown in the figure, the conversion rates of the five fatty acids can reach more than 97%, and the yields are all greater than 78%, indicating that Ag / TiO 2 -3 has excellent fatty acid catalytic activity and is suitable for a variety of fatty acid decarboxylation reactions. 2 -3 catalyzed stearic acid conversion rate was 97.66%, and the yield was 84.12%; Ag / TiO 2 -3 catalyzed the conversion rate of palmitic acid to 97.02% and the yield to 83.24%; Ag / TiO 2 -3 catalyzed the conversion rate of arachidic acid to 98.92% and the yield to 78.27%; Ag / TiO 2 -3 catalyzed myristic acid conversion rate of 98.79%, the yield was 79.48%; Ag / TiO 2 -3 catalyzed the conversion rate of lauric acid to 98.94% and the yield to 79.81%.

[0142] Ag / TiO 2 -A Catalyst Stearic Acid Conversion Activity:

[0143] The photocatalyst TiO prepared in Example 2 2 -A, Ag / TiO 2 -A1, Ag / TiO 2 -A2, Ag / TiO 2 -A3, Ag / TiO 2 -A4, Ag / TiO 2 -A5, Ag / TiO 2 -A6 was used to test the stearic acid conversion activity. The test conditions were as follows: 30 mg of stearic acid, 20 mg of a single photocatalyst, and 10 mL of acetonitrile were placed in a stainless steel photoreactor; the stainless steel photoreactor was heated with H 2 The hydrogen pressure in the stainless steel photoreactor was purged five times and pressurized to 0.1 MPa. When the temperature reached 28°C, the stainless steel photoreactor was irradiated with an LED light source (central wavelength of 365 nm, power of 40 W), the stirring rate was 1000 rpm, and the reaction time was 2 h.

[0144] like Figure 6 As shown, Ag / TiO 2 -A3 and Ag / TiO 2 -A4 as a photocatalyst, the conversion rate of stearic acid reached more than 95%, and Ag / TiO2 -A1 as a photocatalyst has a much higher conversion rate of stearic acid than TiO 2 -A as a photocatalyst. Ag / TiO 2 -A3 achieved higher stearic acid conversion and heptadecane selectivity at lower metal loading, with the heptadecane selectivity reaching over 87%.

[0145] Ag / TiO 2 -R catalyst stearic acid conversion activity:

[0146] The photocatalyst TiO prepared in Example 3 2 -R、Ag / TiO 2 -R1, Ag / TiO 2 -R2, Ag / TiO 2 -R3, Ag / TiO 2 -R4, Ag / TiO 2 -R5, Ag / TiO 2 -R6 was used to test the stearic acid conversion activity. The test conditions were as follows: 30 mg of stearic acid, 20 mg of a single photocatalyst, and 10 mL of acetonitrile were placed in a stainless steel photoreactor; the stainless steel photoreactor was heated with H 2 The hydrogen pressure in the stainless steel photoreactor was purged five times and pressurized to 0.1 MPa. When the temperature reached 28°C, the stainless steel photoreactor was irradiated with an LED light source (central wavelength of 365 nm, power of 40 W), the stirring rate was 1000 rpm, and the reaction time was 2 h.

[0147] like Figure 7 As shown, Ag / TiO 2 -R3 and Ag / TiO 2 -R4 as a photocatalyst, the conversion rate of stearic acid reached more than 95%, and Ag / TiO 2 -R1 as a photocatalyst has a much higher conversion rate of stearic acid than TiO 2 -R as a photocatalyst. Ag / TiO 2 -R3 achieved higher stearic acid conversion and heptadecane selectivity at lower metal loading, with the heptadecane selectivity reaching over 87%.

[0148] Stearic acid conversion activity of catalysts loaded with different metals:

[0149] The Ag / TiO prepared in Example 1 2 -3. Pt / TiO prepared in Example 4 2 , Au / TiO prepared in Example 5 2The stearic acid conversion activity test was carried out under the following test conditions: 30 mg of stearic acid, 20 mg of a single photocatalyst, and 10 mL of acetonitrile were placed in a stainless steel photoreactor; the stainless steel photoreactor was heated with H 2 The hydrogen pressure in the stainless steel photoreactor was purged five times and pressurized to 0.1 MPa. When the temperature reached 28°C, the stainless steel photoreactor was irradiated with an LED light source (central wavelength of 365 nm, power of 40 W), the stirring rate was 1000 rpm, and the reaction time was 2 h.

[0150] like Figure 8 As shown in Figure 2, compared with other noble metal-loaded catalysts, Ag / TiO 2 -3 has the highest yield of heptadecane under the same reaction conditions, among which 0.25wt%Ru / TiO 2 The yield of 0.25wt% Pt / TiO was 55.42%. 2 The yield of heptadecane was 72.21% with 0.25wt% Au / TiO 2 The yield of heptadecane was 71.04% and the yield of 0.25wt% Ag / TiO 2 The yield of heptadecane was 84.12%, indicating that Au / TiO 2 It has excellent photocatalytic activity.

[0151] Photocurrent and impedance test:

[0152] The Ag / TiO prepared in Example 1 2 -1. Ag / TiO 2 -2. Ag / TiO 2 -3. Ag / TiO 2 -4 (10 mg each) were dispersed in ethanol (1 mL), then Nafion solution (30 μL) was added and ultrasonicated for 30 minutes to form a uniform suspension. 200 μL of the suspension was dropped on ITO (indium tin oxide) glass and dried at room temperature for photoelectric testing. The photochemical properties were tested using an electrochemical workstation (CHI660E) and a three-electrode quartz cell system (counter electrode: Pt electrode; reference electrode: Ag / AgCl; working electrode: ITO).

[0153] Use 0.5M Na 2 SO 4 The solution was used as electrolyte and the xenon lamp was used as light source to measure the Ag / TiO 2 -1. Ag / TiO 2 -2. Ag / TiO 2 -3. Ag / TiO 2 -4 It and EIS to study the efficiency of photogenerated charge separation and transfer. Compared with other catalysts, Ag / TiO 2-3 showed the strongest photocurrent intensity ( Fig. 9 a), indicating that the transfer and separation efficiency of interface electrons is higher and the recombination at the catalyst interface is smaller. Fig. 9 As shown in b, the EIS trends of the four catalysts are as follows: Ag / TiO 2 -3 <Ag / TiO 2 -4 <Ag / TiO 2 -2 <Ag / TiO 2 -1, which is consistent with the trend of photocurrent. The above results show that Ag / TiO 2 -3 exhibits excellent photogenerated charge transfer and separation efficiency, which is beneficial to the reduction of H+ to H· and promotes the coupling of alkyl radicals and H· atoms to generate alkanes.

[0154] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A photocatalyst for catalyzing the conversion of carboxylic acids into alkanes, characterized in that: include: A carrier, wherein the carrier is titanium dioxide; An active component, wherein the active component is Ag, which is uniformly dispersed in the carrier and has a particle size of 0.3 to 1 nm; The average particle size of the photocatalyst is 1 μm; The proportion of the active component in the photocatalyst is X, 0.1wt%≤X≤1wt%.

2. The photocatalyst for catalyzing the conversion of carboxylic acids into alkanes according to claim 1, characterized in that: The proportion of the active component in the photocatalyst is X, 0.25wt%≤X≤1.0wt%.

3. A method for preparing the photocatalyst for catalyzing the conversion of carboxylic acid into alkane according to claim 1 or 2, comprising the following steps: A titanium source is added dropwise to acetic acid, and then a soluble precursor of the active component is added, and the mixture is stirred at room temperature until the solution turns white to obtain a precursor liquid; The precursor liquid is kept at 120-150°C for 10-30 hours, cooled naturally and centrifuged, the white precipitate is collected, washed, dried and crushed; The crushed material is fully calcined in an oxygen atmosphere at 400-650°C, and the calcined product is cooled to room temperature and then placed in a hydrogen-containing atmosphere at 350-500°C for full reduction to obtain the photocatalyst for catalyzing the conversion of carboxylic acid into alkane as claimed in claim 1 or 2.

4. A method for preparing the photocatalyst for catalyzing the conversion of carboxylic acid into alkane according to claim 1 or 2, comprising the following steps: dispersing TiO2 nanoparticles in deionized water to obtain a TiO2 suspension; Adding a soluble precursor of the active component to the TiO2 suspension, mixing thoroughly, drying, and crushing; The crushed material is fully calcined in an oxygen atmosphere at 400-650°C, and the calcined product is cooled to room temperature and then placed in a hydrogen-containing atmosphere at 350-500°C for full reduction to obtain the photocatalyst for catalyzing the conversion of carboxylic acid into alkane as claimed in claim 1 or 2.

5. The method for preparing a photocatalyst for catalyzing the conversion of carboxylic acids into alkanes according to claim 3 or 4, characterized in that: The soluble precursor of the active component is silver nitrate or silver ammonia solution.

6. Use of the photocatalyst for catalyzing the conversion of carboxylic acids into alkanes according to claim 1 or 2 in the production of alkanes.

7. A method for producing alkanes from carboxylic acids by photocatalysis, characterized in that: The following steps are involved: Place a carboxylic acid, the photocatalyst for catalyzing the conversion of carboxylic acid into alkanes according to claim 1 or 2, and an organic solvent in a photoreactor; The reaction is stirred at room temperature, in an oxygen-free atmosphere and under ultraviolet light irradiation to obtain an alkane.

8. The method for producing alkanes from carboxylic acids using photocatalysis according to claim 7, characterized in that: The oxygen-free atmosphere is one of hydrogen, nitrogen, an inert gas, nitrogen containing hydrogen, and an inert gas containing hydrogen; and / or, The air pressure is 0.1~4MPa.

9. The method for producing alkanes from carboxylic acids using photocatalysis according to claim 7, characterized in that: The carboxylic acid includes one or more of stearic acid, palmitic acid, arachidic acid, myristic acid, and lauric acid.

10. The method for producing alkanes from carboxylic acids using photocatalysis according to claim 7, characterized in that: The organic solvent is C8-C16 alkane or acetonitrile; and / or, The ultraviolet light adopts an LED light source with a power of 10 to 40W.

Citation Information

Patent Citations

  • Preparation method of Cu / Pd alloy modified TiO2 catalyst for reductive dechlorination materials

    CN107224982A

  • Preparation method of air purification photocatalyst with extra-small precious metal loaded on titanium dioxide surface

    CN107930620A

  • Preparation method of Pd / TiO2 catalyst and application of Pd / TiO2 catalyst to Ullmann reaction

    CN108620066A

  • Method for preparing alkane by hydrogenating and photo-catalyzing fatty acid decarboxylation

    CN111233603A

  • Method for preparing alkane through photo-thermal catalysis of fatty acid decarboxylation by using silver nano-catalyst