Flotation method for silver-containing material with ultra-fine granularity

By using flocculant and lime milk and other agents to adjust the pH value during the flotation process, the problem of low flotation efficiency of extremely fine-grained silver-containing materials is solved, and efficient recycling and economic benefits of silver are achieved.

CN119056592APending Publication Date: 2024-12-03CHIFENG ZHONGSE ZINC IND CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411558574.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-04
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art is difficult to effectively flotation with extremely fine-grained silver-containing materials, which makes it difficult for the silver phase to float and be adsorbed, affecting the flotation efficiency.

Method used

Flocculant solution (polyacrylamide solution) is used to adsorb extremely fine-grained slags and grow up, and lime milk and activated carbon are added to the adjustment tank to adjust the pH value to 4-5.5 to improve the flotation effect.

Benefits of technology

The flocculant makes the silver-containing phase more easily float and adsorbed, which significantly improves the flotation efficiency, improves the silver recovery rate, and reduces the silver content of tailings, brings economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056592A_ABST
    Figure CN119056592A_ABST
Patent Text Reader

Abstract

The flotation method comprises the following steps that the superfine silver-containing material with the silver element content being 160-500 g / t is pulpified in a pulpifying tank, a flocculating agent solution is added, standing is conducted for 3-5 min, then the material is put into an adjusting tank, lime milk is added into the adjusting tank to adjust the pH value of the material to be 4-5.5, activated carbon is added, stirring is conducted for 3-5 min, and the superfine silver-containing material with the silver element content being 160-500 g / t is obtained. Stirring and mixing to obtain a mixed pulpified material, adding the mixed pulpified material and a flotation reagent into a flotation machine, and carrying out flotation through the flotation machine. Due to the fact that in the silver-containing materials with the ultra-fine granularity, the granularity of most materials is smaller than 0.078 mm, the granularity is too small, the argillization phenomenon is prone to being generated in the flotation process, and the silver-containing phase is difficult to float upwards and be adsorbed and is difficult to float. According to the method, the superfine-grained slag is mutually adsorbed and grows through the flocculating agent, the argillization phenomenon is not prone to being generated, the silver-containing phase floats upwards and is adsorbed more easily, and therefore the flotation efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a silver flotation method, in particular to a flotation method for extremely fine-grained silver-containing materials. Background Art

[0002] In the existing silver beneficiation production, flotation process is often used to extract and recover silver from silver-containing materials. Since different silver-containing materials have different compositions, and their compositions are complex and diverse, and the silver occurrence states are diverse, there are many factors that affect the flotation recovery rate of silver. The difficulty of silver flotation is mainly related to the occurrence form of silver in the slag, and secondly to the type of flotation reagents. Usually, the flotation process requires the mixing of different types of reagents, such as: flotation carriers, inhibitors, collectors, activators, and auxiliary collectors, to achieve the target flotation effect.

[0003] The existing silver flotation process can select elemental silver, silver oxide, silver chloride, silver sulfide, and sulfide minerals with conventional particle sizes from silver-containing materials by combining different flotation reagents, and the silver content of its tailings can be reduced to 75g / t at the lowest. However, for extremely fine-grained silver-containing materials, since most of the materials have a particle size of less than 0.078 mm, the flotation process is prone to mudification, which makes it difficult for the silver-containing phase to float and be adsorbed, and it is difficult to effectively select it through conventional flotation methods. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a flotation method for extremely fine-grained silver-containing materials.

[0005] The objective of the present invention is achieved through the following technical scheme: a flotation method for an extremely fine silver-containing material, comprising the following steps: slurrying an extremely fine silver-containing material with a silver content of 160-500 g / t in a slurrying tank, adding a flocculant solution and standing for 3-5 minutes, then placing the material in an adjustment tank, adding lime milk in the adjustment tank to adjust the pH value of the material to 4-5.5, adding activated carbon, stirring and mixing to obtain a mixed slurry, then adding the mixed slurry and a flotation agent into a flotation machine, and flotation by the flotation machine.

[0006] The ultra-fine silver-containing material is a silver-containing material in which more than 79% of the material has a particle size less than 0.078 mm, more than 10% of the material has a particle size of 0.078-0.15 mm, and the remaining material has a particle size greater than 0.15 mm.

[0007] The flocculant solution is a polyacrylamide solution.

[0008] The added amount of the flocculant solution is 6-12.5 g / t, and the mass concentration of the flocculant solution is 1 / 10000-1 / 2000.

[0009] The slurrying is to stir and mix the extremely fine silver-containing material and water in a slurrying tank at a liquid-to-solid ratio of 1:1-2:1.

[0010] The beneficial effect of the present invention is that since most of the extremely fine-grained silver-containing materials have a particle size of less than 0.78 mm, the particle size is too small, and the flotation process is prone to mudification, and the silver-containing phase is difficult to float and be adsorbed, and difficult to be floated. The present invention uses a flocculant to make the extremely fine-grained slag adsorb and grow together, and is not prone to mudification. The silver-containing phase is more likely to float and be adsorbed, thereby improving the flotation efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 It is a flowchart of the present invention; Figure 2 is the particle size composition of the very fine silver-containing material used in Example 1; Figure 3 The figure is a comparison of the silver flotation effects of the present invention and the conventional process. DETAILED DESCRIPTION

[0012] The present invention is described in detail below with reference to the accompanying drawings. Example

[0013] like Figure 2 As shown, among the silver-containing materials used in this test, 79.4% of the materials have a particle size less than 0.078 mm, 13% of the materials have a particle size of 0.078-0.15 mm, and 7.6% of the materials have a particle size greater than 0.15 mm, which are extremely fine-grained silver-containing materials. The silver content in this material is 185g / t-195g / t.

[0014] 30 portions of the above-mentioned ultra-fine-grained silver-containing material were used, 15 portions of which were subjected to flotation tests using the method of the present invention, and 15 portions were subjected to control flotation tests. The specific processing steps are as follows.

[0015] Treatment steps for test groups 1-5: Figure 1 As shown, the ultrafine silver-containing material and water are mixed and stirred in a slurry tank at a liquid-solid ratio of 1:1, and a flocculant solution is added and allowed to stand for 3 minutes. The material is then placed in an adjustment tank, and lime milk is added to the adjustment tank to adjust the pH value of the material to 4. Activated carbon is added and stirred to obtain a mixed slurry. The mixed slurry and flotation reagent are then added to a flotation machine, and flotation is performed by the flotation machine. The flocculant solution used is a polyacrylamide solution, the amount of the flocculant solution added is 6g / t, and the mass concentration of the flocculant solution is 1 / 5000.

[0016] Treatment steps for test groups 6-10: Figure 1As shown, the ultrafine silver-containing material and water are mixed and stirred in a slurry tank at a liquid-solid ratio of 1:1.5, and a flocculant solution is added and allowed to stand for 5 minutes. The material is then placed in an adjustment tank, and lime milk is added to the adjustment tank to adjust the pH value of the material to 4.8. Activated carbon is added and stirred to obtain a mixed slurry. The mixed slurry and flotation reagent are then added to a flotation machine, and flotation is performed by the flotation machine. The flocculant solution used is a polyacrylamide solution, the amount of the flocculant solution added is 10g / t, and the mass concentration of the flocculant solution is 1 / 5000.

[0017] Treatment steps for test groups 11-15: Figure 1 As shown, the ultrafine silver-containing material and water are mixed and stirred in a slurry tank at a liquid-solid ratio of 2:1, a flocculant solution is added and allowed to stand for 5 minutes, and then the material is placed in an adjustment tank, lime milk is added to the adjustment tank to adjust the pH value of the material to 5.5, activated carbon is added, and mixed and stirred to obtain a mixed slurry, and then the mixed slurry and flotation reagent are added to a flotation machine, and flotation is performed by the flotation machine. The flocculant solution used is a polyacrylamide solution, the amount of the flocculant solution added is 12.5g / t, and the mass concentration of the flocculant solution is 1 / 5000.

[0018] The treatment steps of the control group 1-5 groups are as follows: the extremely fine silver-containing material and water are mixed and slurried in a slurry tank at a liquid-solid ratio of 1:1, and then the material is placed in an adjustment tank, and lime milk is added to the adjustment tank to adjust the pH value of the material to 4, and then the slurry and flotation reagent are added to the flotation machine, and flotation is performed by the flotation machine. The flocculant solution used is a polyacrylamide solution, the amount of the flocculant solution added is 6g / t, and the mass concentration of the flocculant solution is 1 / 5000.

[0019] Treatment steps for control group 6-10: Mix the extremely fine silver-containing material and water in a slurry tank at a liquid-solid ratio of 1:1.5, and then put the material into an adjustment tank, add lime milk to adjust the pH value of the material to 4.8, and then add the slurry material and flotation reagent into the flotation machine for flotation. The flocculant solution used is polyacrylamide solution, the amount of flocculant solution added is 10g / t, and the mass concentration of the flocculant solution is 1 / 5000.

[0020] Treatment steps for control group 11-15: Mix the extremely fine silver-containing material and water in a slurry tank at a liquid-solid ratio of 2:1, and then put the material into an adjustment tank, add lime milk to adjust the pH value of the material to 5.5, and then add the slurry material and flotation reagent into the flotation machine for flotation. The flocculant solution used is polyacrylamide solution, the amount of flocculant solution added is 12.5g / t, and the mass concentration of the flocculant solution is 1 / 5000.

[0021] Test results Figure 3As shown in the figure, the first 15 groups are the flotation results of the control group, and the experimental results of the control group 1-15 are arranged from left to right. The silver content of the tailings after flotation is used as an indicator of the flotation capacity of silver. The lower the silver content of the tailings, the more silver is selected into the silver concentrate, and the better the flotation effect. The silver content of the raw ore is 185-195g / t. After flotation production of the control group, the silver content in the tailings is reduced to 75-85g / t.

[0022] exist Figure 3 The last 15 groups are the flotation results of the test group, and the experimental results of the test groups 1-15 are arranged from left to right. After flotation production, the silver content in the tailings was reduced to 60-65g / t, and the silver recovery rate was significantly improved, bringing significant economic benefits.

[0023] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.

Claims

1. A flotation method for extremely fine-grained silver-containing materials, characterized in that The method comprises the following steps: slurrying an extremely fine silver-containing material with a silver content of 160-500 g / t in a slurrying tank, adding a flocculant solution and standing for 3-5 minutes, then putting the material into an adjustment tank, adding lime milk in the adjustment tank to adjust the pH value of the material to 4-5.5, adding activated carbon, stirring and mixing to obtain a mixed slurry, then adding the mixed slurry and a flotation agent into a flotation machine, and performing flotation by the flotation machine.

2. The flotation method of the ultrafine-grained silver-containing material according to claim 1, characterized in that: The ultra-fine silver-containing material is a silver-containing material in which more than 79% of the material has a particle size less than 0.078 mm, more than 10% of the material has a particle size of 0.078-0.15 mm, and the remaining material has a particle size greater than 0.15 mm.

3. The flotation method of the ultrafine-grained silver-containing material according to claim 1, characterized in that: The flocculant solution is a polyacrylamide solution.

4. The flotation method of the ultrafine-grained silver-containing material according to claim 3, characterized in that: The added amount of the flocculant solution is 6-12.5 g / t, and the mass concentration of the flocculant solution is 1 / 10000-1 / 2000.

5. The flotation method of the ultrafine-grained silver-containing material according to claim 2, characterized in that: The slurrying is to stir and mix the extremely fine silver-containing material and water in a slurrying tank at a liquid-to-solid ratio of 1:1-2:1.

Citation Information

Patent Citations

  • Method for extracting metal indium from waste residues generated from lead and zinc smelting

    CN101660054A

  • Method for floating and recycling gold and silver by lead and silver slag ultrasonic treatment in zinc electrolysis plant

    CN101914686A

  • Method for increasing recovery rate of silvers from high leaching residues by flotation

    CN102205280A

  • Method for increasing grade and recovery rate of flotation silver separated from high leaching residues

    CN102225373A

  • Pretreatment process before silver flotation of highly leached residues

    CN103540754A