Lithium ion battery coating consistency control method
By setting key parameters and online detection, the problem of inconsistency in the capacity of lithium-ion battery cells is solved, the reliability and safety of the battery pack are improved, and the coating accuracy and consistency are achieved.
Patent Information
- Application Number
- CN202411084783.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-12-03
Smart Images

Figure CN119056709A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium-ion battery manufacturing, and in particular to a lithium-ion battery coating consistency control method. Background Art
[0002] Limited by the working principle and processing technology, the voltage and capacity of a single lithium-ion battery cannot directly meet the energy storage needs. Generally, multiple monomers are connected in series and parallel to form a module, and even multiple modules are further connected in series and parallel to form a battery pack to meet the voltage, power and energy requirements of the energy storage device. Therefore, the monomer is the core component of the module and directly determines the electrical performance, cycle life, safety and reliability of the module. Therefore, to improve the performance of lithium-ion battery modules, it is necessary to first improve the consistency of the monomer.
[0003] The weight of the positive electrode group directly determines the capacity of the single cell, and the weight accuracy directly determines the consistency of the capacity. The weight accuracy of the positive electrode group is jointly determined by the coating, sorting, and grouping processes. If the surface density of the positive active material is too high or the surface density of the negative active material is too low, it will cause insufficient residual negative electrode of the battery, which may cause lithium deposition in the battery, resulting in single cell capacity deviation and even safety problems. However, in the coating process, the coating accuracy and process capability index (Cpk) are currently low, resulting in a relatively discrete weight of the electrode and a large range. If there is no better method for selecting and grouping the electrode, the capacity of the single cell may be relatively discrete and the consistency may be poor, thereby reducing the reliability and safety of the battery pack. Summary of the invention
[0004] The present application provides a method for controlling the coating consistency of lithium-ion batteries. The method sets key parameters such as oven temperature, tape speed, coating length, and blank length, and detects items such as the appearance, surface density, thickness, size, and alignment of the mother sheet sample before formal coating. During the coating process, an online surface density detector is used to collect the coating surface density online, and measures to deal with abnormal situations are formulated, thereby improving the coating accuracy and process capability index, greatly reducing the weight discreteness and range of batch pole pieces, and thereby improving the reliability and safety of lithium-ion battery cells and battery packs.
[0005] In a first aspect, a lithium-ion battery coating consistency control method is provided, comprising:
[0006] Step 1), before the coating process begins, the oven temperature, belt speed, coating length, and blank length are set;
[0007] Step 2), before the first side of the master sheet is formally coated, the coating equipment is debugged and trial coating is carried out. During the coating process, the surface density is collected in real time using an online surface density detector, and the mother sheet sample of the trial coating is physically sampled and tested. The physical sampling test content includes appearance, surface density, surface density consistency, thickness, and size. If the test results meet the requirements, the first side coating is formally carried out. If not, the coating equipment is readjusted until it meets the requirements;
[0008] Step 3), after the test results meet the requirements, the first side coating is officially carried out, and the coating surface density is collected online using an online surface density detector during the coating process;
[0009] Step 4), according to the actual situation, the rolls are divided, and after the rolls are divided, a single-side mid-inspection is performed, and 3 to 5 mother sheet samples are cut at the winding place. The inspection content includes appearance, surface density, surface density consistency, thickness, and size;
[0010] Step 5), after the first side coating is completed, a final inspection is performed, and 3 to 5 mother sheet samples are cut at the winding place. The inspection contents include appearance, surface density, surface density consistency, thickness, and size;
[0011] Step 6), before the second side of the master sheet is formally coated, the coating equipment is debugged and trial coating is carried out. During the coating process, the surface density is collected in real time using an online surface density detector, and the master sheet samples tested on both sides are sampled and tested. The physical sampling test content includes alignment, appearance, surface density, surface density consistency, thickness, and size. If the test results meet the requirements, the second side coating is formally carried out. If not, the coating equipment is readjusted until it meets the requirements;
[0012] Step 7) After the test results meet the requirements, the second side coating is officially carried out, and the coating surface density is collected online using an online surface density detector during the coating process;
[0013] Step 8) The rolls are divided according to the actual situation. After the rolls are divided, a single-side mid-inspection is performed. 3 to 5 mother sheet samples are cut at the winding place. The inspection contents include alignment, appearance, surface density, surface density consistency, thickness, and size;
[0014] Step 9), after the second side coating is completed, a final inspection is carried out, and 3 to 5 mother sheet samples are cut at the winding place. The inspection contents include alignment, appearance, surface density, surface density consistency, thickness, and size.
[0015] In combination with the first aspect, in certain implementations of the first aspect, in step 1), the number of oven sections is 5 to 8, the temperature is 70 to 130° C., the belt speed is 6 to 10 m / min, the coating length is 90 to 170 mm, and the blank length is 40 to 60 mm.
[0016] In combination with the first aspect, in certain implementations of the first aspect, in step 2), the principle of the online surface density detector is to use the fact that when β rays penetrate the material to be measured, part of the rays are absorbed by the object, resulting in a certain attenuation of the intensity of the rays after penetration relative to the intensity of the incident rays, and the degree of this attenuation is related to the surface density of the penetrated object.
[0017] In combination with the first aspect, in certain implementations of the first aspect, in step 2), the mother sheet samples for physical sampling and testing are taken from 20 to 30 large sheets of trial coating, and 3 to 5 mother sheet samples are cut at the winding place;
[0018] Appearance inspection includes checking the adhesion of the coating material and visual drying. The active material coating is uniform without obvious color difference and no visible wet phenomenon. The sampled electrode is folded in half horizontally and vertically for inspection. There is no large piece of active material falling off.
[0019] Coating surface density = total weight of coated small pieces / (number of samples*small piece area)-foil surface density. The total weight of coated small pieces is the sum of the weights of multiple small pieces sampled by the sampler. The number of coated small pieces sampled is 10-12, and includes the left, middle, and right positions in the length direction of the mother sheet and the top and bottom positions in the width direction. The weight distribution of the coated small pieces cannot deviate from the center line in one direction or be distributed in a gradient from left to right. The single-sided coating surface density is 10-25 mg / cm 2 ;
[0020] The surface density consistency test compares the coating surface density value calculated by physical sampling with the coating surface density value collected by the online detector. If the difference does not meet the requirements, the online detector is calibrated; the difference requirement is not more than 0.1% to 0.2% of the center value of the surface density;
[0021] There are 4 to 8 thickness detection points, including the left, middle and right positions of the pole piece in the horizontal direction, and 2 to 4 points at the head and body positions in the longitudinal direction. The head thickness-body thickness in the vertical direction should be <4 to 8μm, and the body thickness-body thickness should be <3 to 7μm;
[0022] The size detection includes coating length and blank length detection, and the coating length and blank length meet the parameter requirements in step 1).
[0023] In combination with the first aspect, in certain implementations of the first aspect, in step 3) or step 7), if the surface density trend deviates from the center value by 1% to 3%, the coating equipment is adjusted in time; if the surface density exceeds the monomer process standard range for 3 to 6 consecutive points, the coating equipment is stopped for sampling and inspection and adjusted. When the sampling inspection fails, the unqualified section is marked and isolated, and the inspection is readjusted until the inspection results meet the requirements, and then formal coating can be resumed.
[0024] In combination with the first aspect, in certain implementations of the first aspect, in step 3) or step 7), if a tape connection or particle situation is encountered, the die head is pulled back at a low speed for processing without stopping the machine during the process; if a tape breakage situation is encountered, after stopping the machine for processing, the electrode piece staying in the oven section is marked as unqualified and isolated in time in the next process involving winding and unwinding.
[0025] In combination with the first aspect, in certain implementations of the first aspect, in step 4) or step 5), if the test results meet the requirements, the coated master sheet can be used for second-side coating; if the appearance, surface density, thickness or size does not meet the requirements, production is stopped and the reasons are analyzed and found, and the product is scrapped and isolated as appropriate.
[0026] In combination with the first aspect, in certain implementations of the first aspect, in step 6), 3 to 5 mother sheet samples are cut at the winding position;
[0027] The double-sided alignment sampling is cut by a sampler, including the junction area between the head of the coating area and the blank. The distance from the junction of the blank and the coating area on both sides to the blank cutting boundary is measured using a microscope, and the difference between the front and back distances is calculated, which is the alignment. The alignment is <0.4-0.7mm;
[0028] Appearance inspection includes checking the adhesion of the coating material and visual drying. The active material coating is uniform without obvious color difference and no visible wet phenomenon. The sampled electrode is folded in half horizontally and vertically for inspection. There is no large piece of active material falling off.
[0029] Coating surface density = total weight of coated small pieces / (number of samples*small piece area)-foil surface density. The total weight of coated small pieces is the sum of the weights of multiple small pieces sampled by the sampler. The number of coated small pieces sampled is 10-12, and includes the left, middle, and right positions in the length direction of the mother sheet and the top and bottom positions in the width direction. The weight distribution of the coated small pieces cannot deviate from the center line in one direction or be distributed in a gradient from left to right. The double-sided coating surface density is 20-50 mg / cm 2 ;
[0030] The surface density consistency test needs to compare the coating surface density value calculated by physical sampling with the coating surface density value collected by the online detector. If the difference does not meet the requirements, the online detector needs to be calibrated. The difference requirement is not more than 0.2% to 0.4% of the center value of the surface density.
[0031] There are 4 to 8 thickness detection points, including the left, middle and right positions of the pole piece in the horizontal direction, and 2 to 4 points at the head and body positions in the longitudinal direction. The head thickness-body thickness in the vertical direction should be <8 to 12μm, and the body thickness-body thickness should be <4 to 8μm;
[0032] The size detection includes the coating length and the blank length detection. The coating length and the blank length should meet the tolerance range of the parameters in step 1).
[0033] In combination with the first aspect, in certain implementations of the first aspect, in step 7), when the surface density trend deviates from the center value by 1%, the coating equipment is adjusted in time; if the surface density exceeds the monomer process standard range for 4 consecutive points, the machine is stopped for sampling and inspection and the coating equipment is adjusted.
[0034] In combination with the first aspect, in certain implementations of the first aspect, in step 8) or step 9), if the test results meet the requirements, the coated master sheet can be used for subsequent production; if the alignment, appearance, surface density, thickness or size does not meet the requirements, production is stopped and the reasons are analyzed and found, and the product is scrapped and isolated as appropriate.
[0035] Compared with the prior art, the solution provided by the present application includes at least the following beneficial technical effects: by setting key parameters such as oven temperature, tape speed, coating length, blank length, etc., the appearance, surface density, thickness, size, alignment and other items of the mother sheet sample are tested before formal coating, and the coating surface density is collected online using an online surface density detector during the coating process. Abnormal situation response measures are formulated, which improves the coating accuracy and process capability index, greatly reduces the weight discreteness and range of batch pole pieces, and thereby improves the reliability and safety of lithium-ion battery cells and battery packs. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 Schematic diagram of sampling for coating samples.
[0037] Figure 2 Schematic diagram of thickness test points.
[0038] Figure 3 Schematic diagram of alignment calculation.
[0039] Figure 4 This is the process capability analysis chart of the coating process. DETAILED DESCRIPTION
[0040] The present application is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0041] The invention provides a lithium ion battery coating consistency control method, comprising the following steps.
[0042] Step 1), before the coating process begins, parameters such as oven temperature, belt speed, coating length, and blank length need to be set. The specific parameters can be selected according to different lithium-ion electrode materials and battery capacities.
[0043] In step 1), the number of oven sections is 5 to 8, the temperature is 70 to 130° C., the belt speed is 6 to 10 m / min, the coating length is 90 to 170 mm, and the blank length is 40 to 60 mm.
[0044] Step 2), before the first side of the mother sheet is formally coated, the coating equipment needs to be debugged and trial coating is carried out. During the coating process, the surface density is collected in real time using an online surface density detector, and the mother sheet sample for trial coating is physically sampled and tested. The physical sampling test content includes appearance, surface density, surface density consistency, thickness, size, etc. The specific parameters and index requirements can be selected according to different lithium-ion electrode materials and battery capacities. If the test results meet the requirements, the first side coating can be formally carried out. If it does not meet the requirements, the coating equipment is readjusted until it meets the requirements.
[0045] In step 2), the principle of the surface density online detector is that when β rays penetrate the measured material, part of the rays are absorbed by the object, resulting in a certain attenuation of the intensity of the rays after penetration relative to the intensity of the incident rays. The degree of this attenuation is related to the surface density of the penetrated object. Therefore, by measuring the intensity of the rays before and after penetration, the surface density of the penetrated object can be inferred.
[0046] In step 2), the master sheet samples to be tested are taken from 20 to 30 large sheets of test coating, and 3 to 5 master sheet samples are cut at the winding place.
[0047] In step 2), the appearance inspection includes checking the adhesion and visual drying of the coating material. The active material coating should be uniform without obvious color difference and no visible wetness. The sample electrode is folded in half horizontally and vertically to check that no large pieces of active material fall off.
[0048] In step 2), coating surface density = total weight of coated small pieces / (number of samples*small piece area)-foil surface density. The total weight of coated small pieces is the sum of the weights of multiple small piece samples taken by the sampler. The number of coated small pieces sampled is 10 to 12, and includes the left, middle, and right positions in the length direction of the mother sheet and the upper and lower positions in the width direction. The weight distribution of the coated small pieces cannot deviate from the center line in one direction or be distributed in a gradient from left to right. The single-sided coating surface density is 10 to 25 mg / cm 2 .
[0049] In step 2), the surface density consistency test needs to compare the coating surface density value calculated by physical sampling with the coating surface density value collected by the online detector. If the difference does not meet the requirements, the online detector needs to be calibrated. The difference requirement is, for example, no more than 0.1% to 0.2% of the center value of the surface density.
[0050] In step 2), there are 4 to 8 thickness detection points, including the left, middle and right positions of the pole piece in the horizontal direction, and 2 to 4 points are measured at the head and body positions in the longitudinal direction. The head thickness - body thickness in the vertical direction should be <4 to 8μm, and the body thickness - body thickness should be <3 to 7μm.
[0051] In step 2), the size detection includes coating length and blank length detection, and the coating length and blank length should meet the parameter requirements in step 1).
[0052] Step 3), after the test results meet the requirements, the first side coating is officially carried out, and the coating surface density is collected online using an online surface density detector during the coating process.
[0053] In step 3), if the surface density deviates from the center value by 1% to 3%, adjust the coating equipment in time; if the surface density exceeds the monomer process standard range for 3 to 6 points in a row, stop sampling and test and adjust the coating equipment. The sampling and testing method is the same as step 2). When the sampling test is unqualified, the unqualified section needs to be marked and isolated, and the test is readjusted until the test results meet the requirements before the formal first-side coating can be resumed.
[0054] In step 3), if there are problems such as tape splicing and particles, the die head is pulled back at a low speed for processing without stopping the machine during the process; if there are situations such as tape breakage that require stopping the machine, after processing, the electrode pieces staying in the oven section are marked as unqualified and isolated in time in the next process involving winding and unwinding.
[0055] Step 4), split the rolls according to the actual situation. After the rolls are split, a single-sided mid-test should be carried out. 3 to 5 mother sheet samples should be cut at the rewinding point. The testing method and requirements are the same as step 2).
[0056] In step 4), if the test results meet the requirements, the coated mother sheet can be used for the second side coating. If the appearance, surface density, thickness or size do not meet the requirements, production should be stopped and the reasons should be analyzed and found, and the product should be scrapped and isolated as appropriate.
[0057] Step 5), after the first side coating is completed, a final inspection is performed, and 3 to 5 mother sheet samples are cut at the winding place, and the inspection method is the same as step 2).
[0058] In step 5), if the test results meet the requirements, the coated mother sheet can be used for the second side coating. If the appearance, surface density, thickness or size do not meet the requirements, production should be stopped and the reasons should be analyzed and found, and the product should be scrapped and isolated as appropriate.
[0059] Step 6), before the second side of the mother sheet is formally coated, the coating equipment needs to be debugged and trial coating is carried out. During the coating process, the surface density online detector is used to collect the coating surface density in real time, and the alignment, appearance, surface density, surface density consistency, thickness, etc. of the mother sheet sample of the double-sided trial coating are tested. The specific parameters and index requirements can be selected according to different lithium-ion electrode materials and battery capacities. If the test results meet the requirements, the second side coating can be formally carried out. If it does not meet the requirements, the coating equipment is readjusted until it meets the requirements.
[0060] In step 6), 3 to 5 mother sheet samples are cut at the winding position.
[0061] In step 6), the double-sided alignment sampling is cut using a sampler, which should include the junction area between the head of the coated area and the blank. A microscope is used to measure the distance from the junction of the blank and the coated area on both sides to the blank cutting boundary, and the difference between the front and back distances is calculated, i.e. the alignment. The alignment is <0.4-0.7mm.
[0062] In step 6), the appearance inspection includes checking the adhesion of the coating material and visual drying. The active material coating should be uniform without obvious color difference and no visible wetness. The sample electrode is folded in half horizontally and vertically to check that no large pieces of active material fall off.
[0063] In step 6), coating surface density = total weight of coated small pieces / (number of samples*small piece area)-foil surface density. The total weight of coated small pieces is the sum of the weights of multiple small piece samples taken by the sampler. The number of coated small pieces sampled is 10 to 12, and includes the left, middle, and right positions in the length direction of the mother sheet and the upper and lower positions in the width direction. The weight distribution of the coated small pieces cannot deviate from the center line in one direction or be distributed in a gradient from left to right. The double-sided coating surface density is 20 to 50 mg / cm 2 .
[0064] In step 6), the surface density consistency test requires comparing the coating surface density value calculated by physical sampling with the coating surface density value collected by the online detector. If the difference does not meet the requirements, the online detector needs to be calibrated. The difference is required to be no more than 0.2% to 0.4% of the center value of the surface density.
[0065] In step 6), there are 4 to 8 thickness detection points, including the left, middle and right positions of the pole piece in the horizontal direction, and 2 to 4 points are measured at the head and body positions in the longitudinal direction. The head thickness - body thickness in the vertical direction should be <8 to 12μm, and the body thickness - body thickness should be <4 to 8μm.
[0066] In step 6), the size detection includes coating length and blank length detection, and the coating length and blank length should meet the tolerance range of the parameters in step 1).
[0067] Step 7) After the test results meet the requirements, the second side coating is officially carried out. During the coating process, the surface density online detector is used to collect the coating surface density online.
[0068] In step 7), if the surface density deviates from the center value by 1% to 3%, adjust the coating equipment in time; if the surface density exceeds the monomer process standard range for 3 to 6 points in a row, stop sampling and test and adjust the coating equipment. The sampling and testing method is the same as step 6). When the sampling test is unqualified, the unqualified section needs to be marked and isolated, and the test is readjusted until the test result meets the requirements before the formal second side coating can be resumed; if there are situations such as splicing and particles, pull back the die head at a low speed for processing, and do not stop during the process; if there are situations such as broken belts that require shutdown, after processing, mark the pole piece staying in the oven section as unqualified, and isolate it in time in the next winding and unwinding process. In this embodiment, when the surface density deviates from the center value by 1%, adjust the coating equipment in time; when the surface density exceeds the monomer process standard range for 4 points in a row, stop sampling and test and adjust the coating equipment.
[0069] Step 8) Divide the rolls according to the actual situation. After the division is completed, a single-sided mid-test should be carried out. 3 to 5 mother sheet samples should be cut at the rewinding point. The inspection method and requirements are the same as step 6).
[0070] In step 8), if the test results meet the requirements, the coated mother sheet can be used for subsequent production. If the alignment, appearance, surface density, thickness or size do not meet the requirements, production should be stopped and the reasons should be analyzed and found, and the product should be scrapped and isolated as appropriate.
[0071] Step 9), after the second side coating is completed, a final inspection is performed, and 3 to 5 mother sheet samples are cut at the winding place, and the inspection method is the same as step 6).
[0072] In step 9), if the test results meet the requirements, the coated master sheet can be used for subsequent production. If the alignment, appearance, surface density, thickness or size do not meet the requirements, production should be stopped and the reasons should be analyzed and found, and the product should be scrapped and isolated as appropriate.
[0073] Optionally, the method further includes step 10), performing process capability analysis on the surface density during the coating process, calculating the Cpk value, and evaluating the production process capability.
[0074] Example 1
[0075] The lithium-ion battery coating consistency control method proposed by the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0076] Taking a batch of positive electrode coating as an example, the method of the present invention includes the following steps:
[0077] 1) Before the coating process begins, parameters such as oven temperature, tape speed, coating length, and blank length need to be set. The specific parameters can be selected according to different lithium-ion electrode materials and battery capacities; the number of oven sections is 5 to 8, the temperature is 70 to 130°C, the tape speed is 6 to 10 m / min, the coating length is 90 to 170 mm, and the blank length is 40 to 60 mm; in this embodiment, the number of oven sections is 6, the temperature is 80 to 120°C, the specific temperature settings are shown in Table 1 below, the tape speed is 7 m / min, the coating length is 160 mm, and the blank length is 55 mm.
[0078] Table 1
[0079]
[0080] 2) Before the first side of the mother sheet is formally coated, the coating equipment needs to be debugged and trial coating is carried out. During the coating process, the surface density is collected in real time using an online surface density detector, and the appearance, surface density, surface density consistency, thickness, size, etc. of the mother sheet sample of the trial coating are tested. The specific parameters and index requirements can be selected according to different lithium-ion electrode materials and battery capacities. If the test results meet the requirements, the first side coating can be formally carried out. If it does not meet the requirements, the coating equipment is readjusted until it meets the requirements.
[0081] 2.a) The principle of the surface density online detector is that when β rays penetrate the measured material, part of the rays are absorbed by the object, resulting in a certain attenuation of the intensity of the rays after penetration relative to the intensity of the incident rays. The degree of this attenuation is related to the surface density of the penetrated object. Therefore, by measuring the intensity of the rays before and after penetration, the surface density of the object can be inferred.
[0082] 2.b) The mother sheet samples to be tested are taken from 20 to 30 large sheets after trial coating, and 3 to 5 mother sheet samples are cut at the winding position; in this embodiment, after 25 large sheets are trial coated, 5 mother sheet samples are taken for testing.
[0083] 2.c) Appearance inspection includes checking the adhesion of the coating material and visual drying. The coating of the active material should be uniform without obvious color difference and no visible wetness. The sample electrode should be folded in half horizontally and vertically to check that no large pieces of active material have fallen off.
[0084] 2.d) Wherein, coating surface density = total weight of coated small pieces / (number of samples*small piece area)-foil surface density. The total weight of coated small pieces is the sum of the weights of multiple small pieces sampled by the sampler. The number of coated small pieces sampled is 10-12, and includes the left, middle, and right positions in the length direction of the mother sheet and the upper and lower positions in the width direction. The weight distribution of the coated small pieces cannot deviate from the center line in one direction or be distributed in a gradient from left to right. The single-sided coating surface density is 10-25 mg / cm2 In this embodiment, the number of weight samples is 12, and the single-sided coating surface density is 22.5±0.5mg / cm 2 .
[0085] 2.e) The surface density consistency test requires comparing the coating surface density value calculated by physical sampling with the coating surface density value collected by the online detector. If the difference does not meet the requirements, the online detector needs to be calibrated. The difference is required to be no more than 0.1% to 0.2% of the center value of the surface density; in this embodiment, the difference is required to be no more than 0.1% of the center value of the surface density.
[0086] 2.f) There are 4 to 8 thickness detection points, including the left, middle and right positions of the pole piece in the horizontal direction, and 2 to 4 points are measured at the head and main body positions in the longitudinal direction. The head thickness-main body thickness in the vertical direction should be <4 to 8 μm, and the main body thickness-main body thickness should be <3 to 7 μm; in this embodiment, there are 6 thickness detection points, 3 points are measured at the head and main body positions in the longitudinal direction, and the head thickness-main body thickness in the vertical direction should be <5 μm, and the main body thickness-main body thickness should be <4 μm.
[0087] 2.g) The size detection includes coating length and blank length detection, and the coating length and blank length should meet the tolerance range of the parameters in step 1); in this embodiment, the coating length is 160±1mm and the blank length is 55±1mm.
[0088] 3) After the test results meet the requirements, the first side coating is officially carried out. During the coating process, the surface density online detector is used to collect the coating surface density online. If the surface density deviates from the center value by 1% to 3%, the coating equipment is adjusted in time; if the surface density exceeds the monomer process standard range by 3 to 6 points in a row, the machine is stopped for sampling and testing and the coating equipment is adjusted. The sampling and testing method is the same as step 2). When the sampling test is unqualified, the unqualified section needs to be marked and isolated, and the test is readjusted until the test results meet the requirements before the formal first side coating can be resumed; if there are situations such as splicing and particles, the die head is pulled back at a low speed for processing, and the machine should not be stopped during the process; if there are situations such as broken tapes that require shutdown, after processing, the pole piece staying in the oven section is marked as unqualified and isolated in time in the next winding and unwinding process. In this embodiment, when the surface density deviates from the center value by 1%, the coating equipment is adjusted in time. If the surface density exceeds the monomer process standard range by 4 points in a row, the machine is stopped for sampling and testing and the coating equipment is adjusted.
[0089] 4) The rolls are divided according to the actual situation. After the rolls are divided, a single-side mid-inspection should be carried out. 3 to 5 mother sheet samples are cut at the winding place. The inspection method and requirements are the same as step 2). If the inspection result meets the requirements, the coated mother sheet can be used for the second side coating. If the appearance, surface density, thickness or size does not meet the requirements, the production should be stopped and the reasons should be analyzed and found. The product should be scrapped and isolated as appropriate. In this embodiment, 5 mother sheet samples are taken for inspection;
[0090] 5) After the first side coating is completed, a final inspection is performed, and 3 to 5 mother sheet samples are cut off at the winding place. The detection method is the same as step 2). If the detection result meets the requirements, the coated mother sheet can be used for the second side coating. If the appearance, surface density, thickness or size does not meet the requirements, the production should be stopped and the reasons should be analyzed and found. The product should be scrapped and isolated as appropriate; in this embodiment, 5 mother sheet samples are taken for detection;
[0091] 6) Before the second side of the mother sheet is formally coated, the coating equipment needs to be debugged and trial coating is carried out. During the coating process, the surface density is collected in real time using an online surface density detector. The alignment, appearance, surface density, surface density consistency, thickness, size, etc. of the mother sheet samples tested on both sides are tested. The specific parameters and index requirements can be selected according to different lithium-ion electrode materials and battery capacities. If the test results meet the requirements, the second side coating can be formally carried out. If not, the coating equipment is readjusted until it meets the requirements.
[0092] 6.a) 3 to 5 mother sheet samples are cut off at the winding position; in this embodiment, 5 mother sheet samples are taken for testing.
[0093] 6.b) The double-sided alignment sampling is cut by a sampler, which should include the junction area between the head of the coating area and the blank. A microscope is used to measure the distance from the junction of the blank and the coating area on both sides to the blank cutting boundary, and the difference between the front and back distances is calculated, i.e., the alignment. The alignment is <0.4-0.7mm. In this embodiment, the alignment is <0.4mm.
[0094] 6.c) Appearance inspection includes checking the adhesion of the coating material and visual drying. The coating of the active material should be uniform without obvious color difference and no visible wetness. The sample electrode should be folded in half horizontally and vertically to check that no large pieces of active material have fallen off.
[0095] 6.d) Wherein, coating surface density = total weight of coated small pieces / (number of samples*small piece area)-foil surface density. The total weight of coated small pieces is the sum of the weights of multiple small piece samples taken by the sampler. The number of coated small pieces sampled is 10 to 12, and includes the left, middle, and right positions in the length direction of the mother sheet and the upper and lower positions in the width direction. The weight distribution of the coated small pieces cannot deviate from the center line in one direction or be distributed in a gradient from left to right. The single-sided coating surface density is 20 to 50 mg / cm 2 In this embodiment, the weight sampling number is 12, and the double-sided coating surface density is 45±1mg / cm 2 .
[0096] 6.e) The surface density consistency test requires comparing the coating surface density value calculated by physical sampling with the coating surface density value collected by the online detector. If the difference does not meet the requirements, the online detector needs to be calibrated. The difference is required to be no more than 0.2% to 0.4% of the center value of the surface density. In this embodiment, the difference is required to be no more than 0.2% of the center value of the surface density.
[0097] 6.f) The number of thickness detection points is 4 to 8, including the left, middle and right positions of the pole piece in the horizontal direction, and 2 to 4 points are measured at the head and body positions in the longitudinal direction. The head thickness - body thickness in the vertical direction should be <8 to 12 μm, and the body thickness - body thickness should be <4 to 8 μm. In this embodiment, the number of thickness detection points is 6, including the left, middle and right positions of the pole piece in the horizontal direction, and 3 points are measured at the head and body positions in the longitudinal direction. The head thickness - body thickness in the vertical direction should be <9 μm, and the body thickness - body thickness should be <5 μm.
[0098] 6.g) The size detection includes coating length and blank length detection, and the coating length and blank length should meet the parameter requirements in step 1); in this embodiment, the coating length is 160±1mm and the blank length is 55±1mm.
[0099] 7) After the test results meet the requirements, the second side coating is officially carried out. During the coating process, the surface density online detector is used to collect the coating surface density online. If the surface density deviates from the center value by 1% to 3%, the coating equipment is adjusted in time; if the surface density exceeds the monomer process standard range by 3 to 6 points in a row, the machine is stopped for sampling and testing and the coating equipment is adjusted. The sampling and testing method is the same as step 6). When the sampling test is unqualified, the unqualified section needs to be marked and isolated, and the test is readjusted until the test results meet the requirements before the formal second side coating can be resumed; if there are situations such as splicing and particles, the die head is pulled back at a low speed for processing, and the machine should not be stopped during the process; if there are situations such as broken tapes that require shutdown, after processing, the pole piece staying in the oven section is marked as unqualified and isolated in time in the next winding and unwinding process. In this embodiment, when the surface density deviates from the center value by 1%, the coating equipment is adjusted in time. If the surface density exceeds the monomer process standard range by 4 points in a row, the machine is stopped for sampling and testing and the coating equipment is adjusted.
[0100] 8) The rolls are divided according to the actual situation. After the rolls are divided, a single-sided mid-inspection should be carried out. 3 to 5 mother sheet samples are cut at the reeling place. The inspection method and requirements are the same as step 6); if the inspection results meet the requirements, the coated mother sheet can be used for subsequent production. If the alignment, appearance, surface density, thickness or size do not meet the requirements, the production should be stopped and the reasons should be analyzed and found. The products should be scrapped and isolated as appropriate; in this embodiment, 5 mother sheet samples are taken for inspection.
[0101] 9) After the second side coating is completed, a final inspection is performed, and 3 to 5 mother sheet samples are cut off at the winding place. The detection method is the same as step 6). If the detection result meets the requirements, the coated mother sheet can be used for subsequent production. If the alignment, appearance, surface density, thickness or size do not meet the requirements, the production should be stopped and the reasons should be analyzed and found. The product should be scrapped and isolated as appropriate; in this embodiment, 5 mother sheet samples are taken for detection;
[0102] 10) Perform process capability analysis on the surface density during the coating process, calculate the Cpk value, and evaluate the production process capability; in this embodiment, the Cpk value is 1.67, indicating that the production process is stable.
[0103] Figure 1 This is a schematic diagram of sampling of coated small pieces. The number of coated small pieces sampled is 12, and includes the left, middle, and right positions in the length direction of the mother piece and the top and bottom positions in the width direction.
[0104] Figure 2 This is a schematic diagram of thickness test points. There are 6 thickness test points, including the left, middle and right positions of the pole piece in the horizontal direction, and 3 points each at the head and body positions in the longitudinal direction.
[0105] Figure 3This is a schematic diagram of alignment calculation. The double-sided alignment sampling is cut using a sampler, which should include the junction area between the head of the coated area and the blank space. A microscope is used to measure the distance from the junction of the blank space and the coated area on both sides to the blank space cutting boundary, and the difference between the front and back distances is calculated, which is the alignment.
[0106] Figure 4 This is the process capability analysis chart of the coating process. The Cpk value reaches 1.67, indicating that the production process is stable.
[0107] Although the present invention is disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Any person skilled in the art may make possible changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the scope defined by the claims of the present invention.
Claims
1. A lithium-ion battery coating consistency control method, characterized in that: include: Step 1), before the coating process begins, the oven temperature, belt speed, coating length, and blank length are set; Step 2), before the first side of the master sheet is formally coated, the coating equipment is debugged and trial coating is carried out. During the coating process, the surface density is collected in real time using an online surface density detector, and the mother sheet sample of the trial coating is physically sampled and tested. The physical sampling test content includes appearance, surface density, surface density consistency, thickness, and size. If the test results meet the requirements, the first side coating is formally carried out. If not, the coating equipment is readjusted until it meets the requirements; Step 3), after the test results meet the requirements, the first side coating is officially carried out, and the coating surface density is collected online using an online surface density detector during the coating process; Step 4), according to the actual situation, the rolls are divided, and after the rolls are divided, a single-side mid-inspection is performed, and 3 to 5 mother sheet samples are cut at the winding place. The inspection content includes appearance, surface density, surface density consistency, thickness, and size; Step 5), after the first side coating is completed, a final inspection is performed, and 3 to 5 mother sheet samples are cut at the winding place. The inspection contents include appearance, surface density, surface density consistency, thickness, and size; Step 6), before the second side of the master sheet is formally coated, the coating equipment is debugged and trial coating is carried out. During the coating process, the surface density is collected in real time using an online surface density detector, and the master sheet samples tested on both sides are sampled and tested. The physical sampling test content includes alignment, appearance, surface density, surface density consistency, thickness, and size. If the test results meet the requirements, the second side coating is formally carried out. If not, the coating equipment is readjusted until it meets the requirements; Step 7) After the test results meet the requirements, the second side coating is officially carried out, and the coating surface density is collected online using an online surface density detector during the coating process; Step 8) The rolls are divided according to the actual situation. After the rolls are divided, a single-side mid-inspection is performed. 3 to 5 mother sheet samples are cut at the winding place. The inspection contents include alignment, appearance, surface density, surface density consistency, thickness, and size; Step 9), after the second side coating is completed, a final inspection is carried out, and 3 to 5 mother sheet samples are cut at the winding place. The inspection contents include alignment, appearance, surface density, surface density consistency, thickness, and size.
2. The method according to claim 1, characterized in that In step 1), the number of oven sections is 5 to 8, the temperature is 70 to 130° C., the belt speed is 6 to 10 m / min, the coating length is 90 to 170 mm, and the blank length is 40 to 60 mm.
3. The method according to claim 1, characterized in that In step 2), the principle of the surface density online detector is that when β rays penetrate the measured material, part of the rays are absorbed by the object, resulting in a certain attenuation of the intensity of the rays after penetration relative to the intensity of the incident rays. The degree of this attenuation is related to the surface density of the penetrated object.
4. The method according to claim 1, characterized in that: In step 2), the mother sheet samples for physical sampling and testing are taken from 20 to 30 large sheets of test coating, and 3 to 5 mother sheet samples are cut at the winding place; Appearance inspection includes checking the adhesion of the coating material and visual drying. The active material coating is uniform without obvious color difference and no visible wet phenomenon. The sampled electrode is folded in half horizontally and vertically for inspection. There is no large piece of active material falling off. Coating surface density = total weight of coated small pieces / (number of samples*small piece area)-foil surface density. The total weight of coated small pieces is the sum of the weights of multiple small pieces sampled by the sampler. The number of coated small pieces sampled is 10-12, and includes the left, middle, and right positions in the length direction of the mother sheet and the top and bottom positions in the width direction. The weight distribution of the coated small pieces cannot deviate from the center line in one direction or be distributed in a gradient from left to right. The single-sided coating surface density is 10-25 mg / cm 2 ; The surface density consistency test compares the coating surface density value calculated by physical sampling with the coating surface density value collected by the online detector. If the difference does not meet the requirements, the online detector is calibrated; the difference requirement is not more than 0.1% to 0.2% of the center value of the surface density; There are 4 to 8 thickness detection points, including the left, middle and right positions of the pole piece in the horizontal direction, and 2 to 4 points at the head and body positions in the longitudinal direction. The head thickness-body thickness in the vertical direction should be <4 to 8μm, and the body thickness-body thickness should be <3 to 7μm; The size detection includes coating length and blank length detection, and the coating length and blank length meet the parameter requirements in step 1).
5. The method according to claim 1, characterized in that In step 3) or step 7), if the surface density deviates from the center value by 1% to 3%, adjust the coating equipment in time; if the surface density exceeds the monomer process standard range for 3 to 6 points in a row, stop sampling and test and adjust the coating equipment. If the sampling test fails, mark and isolate the unqualified section, and readjust the test until the test results meet the requirements, then resume formal coating.
6. The method according to claim 5, characterized in that In step 3) or step 7), if there are tape splicing or particle problems, pull the die head back at a low speed for processing without stopping the machine during the process; if there is a tape breakage, after stopping the machine for processing, mark the electrode remaining in the oven section as unqualified and isolate it in time in the next process involving winding and unwinding.
7. The method according to claim 1, characterized in that In step 4) or step 5), if the test results meet the requirements, the coated mother sheet can be used for second-side coating. If the appearance, surface density, thickness or size do not meet the requirements, production is stopped and the reasons are analyzed and found, and the product is scrapped and isolated as appropriate.
8. The method according to claim 1, characterized in that In step 6), 3 to 5 mother sheet samples are cut at the winding position; The double-sided alignment sampling is cut by a sampler, including the junction area between the head of the coating area and the blank. The distance from the junction of the blank and the coating area on both sides to the blank cutting boundary is measured using a microscope, and the difference between the front and back distances is calculated, which is the alignment. The alignment is <0.4-0.7mm; Appearance inspection includes checking the adhesion of the coating material and visual drying. The active material coating is uniform without obvious color difference and no visible wet phenomenon. The sampled electrode is folded in half horizontally and vertically for inspection. There is no large piece of active material falling off. Coating surface density = total weight of coated small pieces / (number of samples*small piece area)-foil surface density. The total weight of coated small pieces is the sum of the weights of multiple small pieces sampled by the sampler. The number of coated small pieces sampled is 10-12, and includes the left, middle, and right positions in the length direction of the mother sheet and the top and bottom positions in the width direction. The weight distribution of the coated small pieces cannot deviate from the center line in one direction or be distributed in a gradient from left to right. The double-sided coating surface density is 20-50 mg / cm 2 ; The surface density consistency test needs to compare the coating surface density value calculated by physical sampling with the coating surface density value collected by the online detector. If the difference does not meet the requirements, the online detector needs to be calibrated. The difference requirement is not more than 0.2% to 0.4% of the center value of the surface density. There are 4 to 8 thickness detection points, including the left, middle and right positions of the pole piece in the horizontal direction, and 2 to 4 points at the head and body positions in the longitudinal direction. The head thickness-body thickness in the vertical direction should be <8 to 12μm, and the body thickness-body thickness should be <4 to 8μm; The size detection includes the coating length and the blank length detection. The coating length and the blank length should meet the tolerance range of the parameters in step 1).
9. The method according to claim 8, characterized in that In step 7), when the surface density deviates from the central value by 1%, the coating equipment is adjusted in time; when the surface density exceeds the monomer process standard range for 4 consecutive points, the machine is stopped for sampling and testing and the coating equipment is adjusted.
10. The method according to claim 1, characterized in that In step 8) or step 9), if the test results meet the requirements, the coated master sheet can be used for subsequent production. If the alignment, appearance, surface density, thickness or size do not meet the requirements, production is stopped and the reasons are analyzed and found, and the product is scrapped and isolated as appropriate.
Citation Information
Cited By
Membrane abnormal position identification method, system and equipment and storage medium
CN119408325A