Continuous casting production control method for sunken 1215MS casting blank
By adopting special protection slag, weak cooling system, enhanced electromagnetic stirring and small taper crystallizer in the 1215MS casting billet continuous casting process, the problem of casting billet is solved and high-quality casting is achieved The production of blanks meets the production requirements of the casting machine.
Patent Information
- Application Number
- CN202411181857.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
The 1215MS casting billet often has depression defects during the continuous casting of small square billets, which affects production stability and product quality. The high oxygen and high sulfur content of easy-to-cut steels lead to difficulty in separation of steel slag, which easily forms rolled slag and cracks.
Special protective slag for low-carbon, high-sulfur, easy-to-cut steel, weak cooling system, enhanced electromagnetic stirring, low-pull speed and stable casting, small taper crystallizer and Class D overall tundra are adopted to optimize the continuous casting process to improve the quality of the casting billet.
It effectively eliminates the quality problems such as slag, cracks, and bubbles of the casting blank, especially solves the depressed defects of the casting blank, meets the quality requirements of the casting machine production, and improves the surface and internal quality of the casting blank.
Smart Images

Figure CN119057031A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a 1215MS casting billet recessed continuous casting production control method. Background Art
[0002] Free-cutting steel is a type of steel developed for the purpose of reducing machining costs, improving cutting quality, reducing cutting resistance or improving cutting processability in automatic machining machines. 1215MS is an environmentally friendly low-carbon, high-sulfur free-cutting steel. It is one of the most difficult steels to produce. The product has high surface and internal quality. When the steel plant's small square billet continuous casting machine produced 1215MS, the quality defect problem caused by the concave surface of the billet was more serious, which had a great impact on the production and quality of the casting machine and became a problem that restricted production stability. With the vigorous development of machinery manufacturing and the automobile industry, the demand for free-cutting steel is increasing, and the product quality requirements are also getting higher and higher. Summary of the invention
[0003] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and to provide a 1215MS casting slab concave continuous casting production control method.
[0004] The present invention solves the technical problem by adopting the following technical solutions.
[0005] The present invention provides a 1215MS ingot concave continuous casting production control method, which comprises: using special protective slag for low-carbon high-sulfur free-cutting steel, a weak cooling system and a continuous casting process with enhanced electromagnetic stirring, low-speed steady casting, a small-taper crystallizer and a D-type integral tundish to improve the quality of the 1215MS ingot.
[0006] The present invention has the following beneficial effects:
[0007] The present invention provides a 1215MS casting billet concave continuous casting production control method, which includes: using special protective slag for low-carbon and high-sulfur free-cutting steel, weak cooling system and continuous casting process with enhanced electromagnetic stirring, low-speed steady casting, small-taper crystallizer and D-type integral tundish to improve the quality of 1215MS casting billet. The method can effectively prevent the quality of casting billet output slag, cracks, bubbles, etc., especially solves the quality problem of casting billet concave defects, and meets the production requirements of the casting machine. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0009] Figure 1 This is a flow chart of the 1215MS ingot recessed continuous casting production control method provided by the present invention. DETAILED DESCRIPTION
[0010] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out under normal conditions. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0011] The following is a specific description of a 1215MS ingot concave continuous casting production control method provided by an embodiment of the present invention.
[0012] An embodiment of the present invention provides a 1215MS ingot concave continuous casting production control method. Aiming at the problem that the quality concave defects of ingots produced by small square billet continuous casting at this stage are relatively serious, an embodiment of the present invention provides a 1215MS ingot concave continuous casting production control method. The method can effectively prevent the ingots from producing slag rolls, cracks, bubbles and other quality problems, especially solves the quality problem of ingots producing concave defects, and meets the production requirements of the casting machine.
[0013] The embodiment of the present invention provides a 1215MS casting slab concave continuous casting production control method, which mainly includes the following aspects:
[0014] (1) Use special protective slag for low-carbon, high-sulfur free-cutting steel.
[0015] The original mold protection slag used was low-carbon steel protection slag. The transverse sample of the defective part of the steel bar surface was taken for metallographic inspection. The defects under the metallographic structure of the sample were pits and cracks. Some cracks and pits were distributed together. There were gray inclusions in the cracks. The cracks extended gently inward. There was obvious tissue rheology on the side of the crack close to the surface. Under the electron microscope, the components of the micro-area at the bottom of the surface defect were mainly Fe and O. There were multiple granular slags at the bottom of the defect. The granular slag components mainly included Ca, O, Al, Na, K, Si, etc., which were residual protective slag. The high oxygen and high sulfur content in 1215MS free-cutting steel significantly reduced the surface tension of the molten steel, making it difficult to separate the steel slag during the casting process, which easily led to the crystallizer casting slag roll, resulting in internal defects of the ingot. The internal inclusions brought in by the slag roll failed to weld and form cracks during the rolling process. After subsequent drawing, the cracks further expanded to form surface pits and meat defects. The composition of the special protective slag for low-carbon and high-sulfur free-cutting steel used is shown in the following table:
[0016]
[0017] The solution provided by the embodiment of the present invention adopts a special protective slag for low-carbon and high-sulfur free-cutting steel, which improves the reducibility of protective slag basicity, reduces the sulfur and oxygen content at the steel slag interface through chemical reaction, increases the interfacial tension, reduces the formation of flocculent slag, and avoids quality accidents such as slag curling and pits in the casting.
[0018] (2) Adopt weak cooling system.
[0019] ①. The original crystallizer water flow rate is 130-135Nm 3 / h, the temperature difference between the inlet and outlet water of the crystallizer is between 5-6℃. When the temperature difference between the inlet and outlet water of the crystallizer is lower than 7℃, the liquid level of the crystallizer will fluctuate significantly. The water flow rate of the crystallizer is too large, and the billet is too strongly cooled. Since the molten steel is "overcooled" in the initial solidification stage of the crystallizer, the billet shell will grow unevenly, resulting in depressions in the billet.
[0020] The solution provided by the embodiment of the present invention adopts a weak cooling system for the crystallizer water, adjusts the crystallizer water distribution parameters, and increases the crystallizer water flow rate from the original 130-135Nm 3 / h, reduced to 110-115Nm 3 / h, the temperature difference between the inlet and outlet water of the crystallizer is controlled between 7-8℃, the heat flux intensity near the crystallizer liquid surface is reduced, the growth of the shell is slowed down, so as to promote the uniformity of the growth of the primary shell in the crystallizer copper tube, and reduce the crack sensitivity caused by the high S and P of this steel. Theory and practice have proved that weak cooling and slow cooling of the crystallizer water can effectively control the uneven growth of the primary shell in the crystallizer and inhibit the generation of crystallizer liquid surface fluctuations.
[0021] ②. In the production process of continuous casting machine, secondary cooling is a very important operation link. It has a significant impact on the normal production of casting machine and the internal and external quality of ingot. The key of secondary cooling is to ensure that the surface temperature of ingot is controlled within the process range. The original secondary cooling water distribution model is "Class B intermediate cooling", the pulling speed control range is 1.6-2.0m / min, the surface temperature of ingot out of the secondary cooling chamber is 850-880℃, and the surface temperature of ingot is not within the process control range. The secondary cooling water flow is too large, the cooling of ingot is too strong, the ingot shell thickens and hardens, the deformation force increases, and the surface temperature of ingot is too low. Under the action of the straightening machine, it is easy to cause the liquid level of the crystallizer to fluctuate. The fluctuation of the liquid level of the crystallizer is easy to cause slag curling and the ingot to form a depression.
[0022] The secondary cooling water adopts a weak cooling system, and the secondary cooling water distribution model is changed from "B-type medium cooling" to "C-type weak cooling". The water volume of the secondary cooling is controlled at 0.5-0.6L / Kg. By reducing the cooling intensity of the billet, the billet shell is produced evenly. The surface temperature of the billet leaving the secondary cooling chamber is 930-950℃, and the billet surface control temperature is within the process range.
[0023] Class C weak cooling water distribution table is as follows:
[0024]
[0025] (3) Enhance the electromagnetic stirring and end electric stirring of the crystallizer.
[0026] The original mold electromagnetic stirring (M-EMS) current is 250A, the frequency is 3Hz, and the end electromagnetic stirring (F-EMS) current is 200A, the frequency is 3Hz.
[0027] In the solution provided by the embodiment of the present invention, the crystallizer electromagnetic stirring current is increased to 350A, and the frequency is 3Hz. The terminal electromagnetic stirring current is increased to 350A, and the frequency is 8Hz. Increasing the crystallizer electromagnetic stirring current and increasing the stirring intensity of the crystallizer molten steel and the terminal ingot liquid core can promote the floating of CO bubbles and prevent them from being captured by the solidification interface and remaining in the ingot to form subcutaneous bubbles.
[0028] (4) Use low pulling speed for smooth pouring.
[0029] The original pulling speed control range is 1.6-2.0m / min. The crystallizer liquid level fluctuation becomes more intense with the increase or decrease of pulling speed. The frequent changes in pulling speed affect the crystallizer liquid level fluctuation to a certain extent. In the production process, the pulling speed is frequently increased or decreased. The sudden increase or decrease in speed during the casting process makes the stopper rod flow control action frequent, and the flow state of the molten steel in the water inlet and the crystallizer changes rapidly, which easily causes the crystallizer liquid level fluctuation. In particular, the production of 1215MS requires a higher precision of liquid level fluctuation control. Therefore, the pulling speed is kept stable, which is the premise of stable casting and the prerequisite for maintaining the stability of the crystallizer liquid level.
[0030] The solution provided in the embodiment of the present invention adopts low drawing speed for smooth casting, expands the temperature acceleration range of the tundish, and reduces the production drawing speed control range to 1.7-1.8m / min, thereby reducing the frequent fluctuations in drawing speed caused by changes in the tundish temperature, and eliminating the crystallizer liquid level fluctuations, slag rolls and ingot interface billets caused by changes in the drawing speed.
[0031] (5) Use a small taper crystallizer.
[0032] The cross section of the original 1215MS crystallizer is 160mm*160mm, the upper size of the copper tube is 167m*167m, the lower size is 165*165mm, the copper tube is 900mm high, and the crystallizer taper is 2.6% / m. If the crystallizer taper is too large, it will cause the liquid steel flow in the crystallizer to move unstably, produce slip flow or rapid flow, cause friction inside the crystallizer, and form pits.
[0033] The solution provided in an embodiment of the present invention adopts a small-taper crystallizer with the following specifications: the upper opening size of the crystallizer copper tube is set to 166.6m*164.60m, the lower opening size is set to 165*163mm, the copper tube height is set to 900mm, the upper and lower opening difference is set to 1.6mm, and the crystallizer inverted taper is set to 2.1% / m.
[0034] (6) Use 1215MS to produce special Class D integral ladle.
[0035] The tundish nozzles of the billet continuous casting machine are mainly divided into split type and integral type. Among them, the split type nozzle can adjust the relative position of each nozzle in the crystallizer online to make it centered, but because the split type nozzle has a loose seal at the joint between the tundish upper nozzle and the immersion nozzle, this type of nozzle is prone to secondary oxidation of molten steel, affecting the quality of billet casting. The integral type nozzle can avoid such problems. Its upper end is fixed in the tundish base brick, and the lower end is immersed in the steel liquid level in the crystallizer when in use to protect the steel flow from oxidation. At the same time, it can block the radiation heat dissipation of the steel flow and prevent the molten steel from splashing, thereby improving the operating environment.
[0036] The solution provided by the embodiment of the present invention uses a Class D integral tundish dedicated to 1215MS production to replace a Class A common split nozzle tundish to improve the production stability of 1215MS. The Class D integral tundish has the following main features:
[0037] (1) The working layer of the D-type integral tundish is made of MgO material with a mass fraction of 82%-100%;
[0038] (2) using an improved stopper rod, wherein the binder in the rod head material of the stopper rod is a mixture of 0-25% solid thermosetting phenolic resin and 70%-100% liquid thermoplastic phenolic resin;
[0039] (3) The integral submerged nozzle is protected by argon gas to improve the purity of molten steel.
[0040] (4) An integral submerged nozzle is used. There is no connection gap between the nozzle on the tundish and the submerged nozzle. No air is inhaled during use, which is beneficial to the quality of the casting.
[0041] Compared with the prior art, the solution provided by the embodiment of the present invention has the following characteristics and advantages:
[0042] (1) The pulling speed is stable, the liquid level in the crystallizer is balanced, and the crystallizer liquid level fluctuation is less than 3 mm.
[0043] (2) The protective slag in the crystallizer is well slagging and has no agglomeration.
[0044] (3) The surface temperature of the ingot leaving the secondary cooling chamber is between 930-950℃.
[0045] (4) The produced ingots are free of slag, cracks, bubbles and depressions.
[0046] The present invention will be further described below in conjunction with the embodiments.
[0047] Original process
[0048] (1) Carbon steel protective slag was originally used, and transverse samples of the surface defect parts of the rolled steel bars were taken for metallographic inspection. The defects of the samples were pits and cracks. Some cracks and pits were distributed together. There were gray inclusions in the cracks. The cracks extended gently inward. There was obvious tissue rheology on the side of the crack close to the surface. Under the electron microscope, the micro-region components at the bottom of the surface defect were mainly Fe and O. There were multiple granular slags at the bottom of the defect. The granular slag components mainly included Ca, O, Al, Na, K, Si, etc., which were residual protective slag. The high oxygen and high sulfur content in 1215 free-cutting steel significantly reduced the surface tension of the molten steel, making it difficult to separate the slag during the casting process, which easily led to the casting of slag in the crystallizer, resulting in internal defects of the ingot. The internal inclusions brought in by the slag could not be welded during the rolling process to form cracks. After subsequent drawing, the cracks further expanded to form surface pits and meat defects.
[0049] (2) The crystallizer water flow rate of the original crystallizer is 130-135Nm 3 / h, the inlet and outlet water temperatures of the crystallizer are 5-6℃. When the inlet and outlet water temperature difference of the crystallizer is lower than 7℃, the liquid level of the crystallizer will fluctuate significantly. The water flow of the crystallizer is too large, and the billet is too strongly cooled. Since the molten steel is "overcooled" in the initial solidification stage of the crystallizer, the billet shell will grow unevenly, resulting in depressions in the billet.
[0050] (3) The secondary cooling water distribution model is medium cooling, the casting speed control range is 1.6-2.0m / min, the surface temperature of the billet out of the secondary cooling chamber is 850-880℃, and the secondary cooling water cooling is too strong, resulting in the billet surface temperature being too low.
[0051] Class B intercooler water distribution table is as follows:
[0052]
[0053] (4) The cross-section of the original 1215MS crystallizer is 160mm*160mm, the upper size of the copper tube is 167m*167m, the lower size is 164*164mm, the copper tube is 900mm high, and the crystallizer taper is 2.6% / m. The crystallizer taper is too large, which will cause the liquid steel flow in the crystallizer to move unstably, produce slip flow or rapid flow, cause internal friction of the crystallizer, and form pits.
[0054] For improved process, see Figure 1 ,include:
[0055] (1) Use special protective slag for low-carbon, high-sulfur free-cutting steel.
[0056] Use special protective slag for low-carbon, high-sulfur free-cutting steel. Improve the reducibility of protective slag basicity, reduce the sulfur and oxygen content at the slag interface through chemical reaction, increase the interfacial tension, reduce the formation of flocculent slag, and avoid quality accidents such as slag curling and pits in the casting. The composition of the special protective slag for low-carbon, high-sulfur free-cutting steel used is shown in the following table:
[0057]
[0058] (2) Adopt weak cooling system.
[0059] ①. The crystallizer water adopts weak cooling system, adjusts the crystallizer water distribution parameters, and increases the crystallizer water flow from the original 130-135Nm 3 / h, reduced to 110-115Nm 3 / h, the temperature difference between the inlet and outlet water of the crystallizer is controlled between 7-8℃, the heat flux intensity near the crystallizer liquid surface is reduced, the growth of the shell is slowed down, so as to promote the uniformity of the growth of the primary shell in the crystallizer copper tube, and reduce the crack sensitivity caused by the high S and P of this steel. Theory and practice have proved that weak cooling and slow cooling of the crystallizer water can effectively control the uneven growth of the primary shell in the crystallizer and inhibit the generation of crystallizer liquid surface fluctuations.
[0060] ②. The secondary cooling water adopts a weak cooling system, and the secondary cooling water distribution model is changed from "Class B intermediate cooling" to "Class C weak cooling". The water volume of the secondary cooling is controlled at 0.5-0.6L / Kg. By reducing the cooling intensity of the billet, the billet shell is produced evenly, the surface temperature of the billet leaving the secondary cooling chamber is 930-950℃, and the billet surface control temperature is within the process range.
[0061] Class C weak cooling water distribution table is as follows:
[0062]
[0063] (3) Enhance the electromagnetic stirring of the crystallizer and the end battery stirring.
[0064] The crystallizer electromagnetic stirring current is increased to 350A, and the frequency is 3Hz. The terminal electromagnetic stirring current is increased to 350A, and the frequency is 8Hz. Increasing the crystallizer electromagnetic stirring current and increasing the stirring intensity of the crystallizer molten steel and the terminal ingot liquid core can promote the floating of CO bubbles and prevent them from being captured by the solidification interface and remaining in the ingot to form subcutaneous bubbles.
[0065] (4) Use low pulling speed for smooth pouring.
[0066] The casting is smooth with low casting speed, the temperature acceleration range of the tundish is expanded, and the production casting speed control range is narrowed to 1.7-1.8m / min, so as to reduce the frequent fluctuation of casting speed caused by the temperature change of the tundish, and eliminate the crystallizer liquid level fluctuation, slag roll and ingot interface caused by the casting speed change.
[0067] (5) Use a small taper crystallizer.
[0068] A small-taper crystallizer is used, with the upper opening size of the crystallizer copper tube set to 166.6m*164.60m, the lower opening size set to 165*163mm, the copper tube height set to 900mm, the upper and lower opening difference set to 1.6mm, and the crystallizer inverted taper set to 2.1% / m.
[0069] (6) Use 1215MS to produce special Class D integral ladle.
[0070] Use the D-type integral tundish dedicated to 1215MS production to replace the A-type common split nozzle tundish to improve the production stability of 1215MS. The D-type tundish has the following main features:
[0071] (1) The working layer of the D-type integral tundish is made of MgO material with a mass fraction of 82%-100%;
[0072] (2) using an improved stopper rod, wherein the binder in the rod head material of the stopper rod is a mixture of 0-25% solid thermosetting phenolic resin and 70%-100% liquid thermoplastic phenolic resin;
[0073] (3) The integral submerged nozzle is protected by argon gas to improve the purity of molten steel.
[0074] Comparative Example 1
[0075] The crystallizer water flow setting value is 120-125Nm 3 / h, the results are: the temperature difference between the inlet and outlet water of the crystallizer is between 5-6℃, and the temperature difference between the inlet and outlet water of the crystallizer is lower than 7℃. Temperature fluctuations are likely to occur inside the crystallizer, which will lead to excessive crystallization at the inlet of the crystallizer, affecting the effect of the crystallization process. The liquid level of the crystallizer will fluctuate significantly, which will lead to cracks on the surface of the ingot or internal defects.
[0076] Comparative Example 2
[0077] The steps are similar to those in Example 1, except that the secondary cooling water distribution model is "Class B intermediate cooling", the drawing speed control range is 2.0-2.3m / min, and the surface temperature of the billet out of the secondary cooling chamber is 860-890℃. The result is that the surface temperature of the billet is not within the process control range. The secondary cooling water flow is too large, the billet is cooled too strongly, the billet shell thickens and hardens, and the deformation force increases, causing the billet surface temperature to be too low. Under the action of the straightening machine, it is easy to cause the crystallizer liquid level to fluctuate. On the other hand, the local overcooling of the secondary cooling is easy to cause the billet longitudinal depression.
[0078] Comparative Example 3
[0079] The steps are similar to those in Example 1, except that the drawing speed control parameter is in the range of 1.5-2.3 m / min. Since the secondary cooling water distribution is currently controlled by a water meter, the secondary cooling water volume is quadratically related to the billet drawing speed to set the water volume in each zone, and the water flow rate is set according to the drawing speed. When the drawing speed changes frequently, the result is that the frequency of the cooling water valve adjustment, the response speed of the cooling water valve and the proportion of each opening adjustment, the water volume adjustment speed is difficult to track the change of the upper drawing speed, which directly affects the stability of the secondary cooling water volume. The frequent increase or decrease of the drawing speed and the sudden increase or decrease of the speed during the casting process make the stopper rod control flow action frequent, and the flow state of the molten steel in the water inlet and the crystallizer changes rapidly, which is easy to cause frequent fluctuations in the crystallization liquid level, increase the probability of slag rolling in the crystallizer, and the probability of slag rings, pits, cracks, and pores on the surface of the billet will increase. The subcutaneous slag inclusions of the slag billet will increase, affecting the internal and surface quality of the billet.
[0080] Comparative Example 4
[0081] The steps are similar to those in Example 1, except that the upper opening size of the copper tube of the crystallizer is set to 166.2m*164.20m, the lower opening size is set to 164.4*162.4mm, the copper tube height is set to 900mm, the upper and lower opening difference is set to 1.8mm, and the inverted taper of the crystallizer is set to 2.7% / m. The results are as follows: excessive taper will result in a thicker crystal shell, excessively large and irregular grains, and defects such as cracks, looseness and pores are prone to appear in the ingot.
[0082] As can be seen from the above, the embodiment of the present invention provides a 1215MS casting slab concave continuous casting production control method. It adopts special protective slag for low-carbon and high-sulfur free-cutting steel, adopts weak cooling system, strengthens electromagnetic stirring and end electric stirring of crystallizer, adopts low pulling speed and stable casting, adopts small taper crystallizer and adopts Class D integral tundish dedicated to 1215MS production. By optimizing the production process, it can effectively prevent the casting slag, cracks, bubbles and other quality problems, especially solves the quality problem of the casting slab producing concave defects.
[0083] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A 1215MS casting slab concave continuous casting production control method, characterized in that: It includes: The quality of 1215MS ingots is improved by using special protective slag for low-carbon and high-sulfur free-cutting steel, weak cooling system, continuous casting process with enhanced electromagnetic stirring, low-speed steady pouring, small-taper crystallizer and Class D integral tundish.
2. The 1215MS casting slab concave continuous casting production control method according to claim 1 is characterized in that: The composition of the special protective slag for low-carbon and high-sulfur free-cutting steel is shown in the following table:
3. The 1215MS casting slab concave continuous casting production control method according to claim 1 is characterized in that: The weak cooling system includes: reducing the water flow rate of the crystallizer and adopting a weak cooling system for secondary cooling.
4. The 1215MS casting slab concave continuous casting production control method according to claim 3 is characterized in that: Reducing the crystallizer water flow includes: adjusting the crystallizer water flow to 110-115Nm 3 / h, the temperature difference of the inlet and outlet water of the crystallizer is controlled between 7-8℃.
5. The 1215MS casting slab concave continuous casting production control method according to claim 3 is characterized in that: The secondary cooling adopts a weak cooling system including: adjusting the secondary cooling water distribution model to Class C weak cooling, controlling the water volume of the secondary cooling at 0.5-0.6L / Kg, and controlling the surface temperature of the ingot out of the secondary cooling chamber at 930-950°C, so that the surface temperature of the ingot is controlled within the process range.
6. The 1215MS casting slab concave continuous casting production control method according to claim 5 is characterized in that: The Class C weak cooling water distribution table is as follows:
7. The 1215MS casting slab concave continuous casting production control method according to claim 1 is characterized in that: Enhanced electromagnetic stirring includes: the crystallizer electromagnetic stirring current is enhanced to 350A, the frequency is 3Hz, and the end electromagnetic stirring current is enhanced to 350A, the frequency is 8Hz.
8. The 1215MS casting slab concave continuous casting production control method according to claim 1 is characterized in that: Smooth casting at low pulling speed includes: adjusting the production pulling speed control range to 1.7-1.8m / min.
9. The 1215MS casting slab concave continuous casting production control method according to claim 1, characterized in that: The specifications of the small-taper crystallizer include: the upper opening size of the crystallizer copper tube is set to 166.6m*164.60m, the lower opening size is set to 165*163mm, the copper tube height is set to 900mm, the upper and lower opening difference is set to 1.6mm, and the crystallizer inverted taper is set to 2.1% / m.
10. The 1215MS casting slab concave continuous casting production control method according to claim 1, characterized in that: The Class D integral tundish has at least one of the following characteristics: (1) The working layer of the D-type integral tundish is made of MgO material with a mass fraction of 82%-100%; (2) using an improved stopper rod, wherein the binder in the rod head material of the stopper rod is a mixture of 0-25% solid thermosetting phenolic resin and 70%-100% liquid thermoplastic phenolic resin; (3) The integral submerged nozzle is protected by argon gas to improve the purity of molten steel; (4) An integral submerged nozzle is used. There is no connection gap between the tundish upper nozzle and the submerged nozzle. No air is inhaled during use, which is beneficial to improving the quality of the casting.