Preparation method of ultra-large-thickness duplex stainless steel composite plate
Through two explosive welding technology and pretreatment steps, the problem of difficult control of the quality and proportion of ultra-large thickness duplex stainless steel composite panels is solved, and performance improvement and application standards are achieved, and it is suitable for high-end equipment manufacturing.
Patent Information
- Application Number
- CN202411244501.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-03
AI Technical Summary
The existing explosion welding technology is difficult to effectively control the explosion bonding quality of ultra-large thickness duplex stainless steel composite panels, and it is difficult to ensure proportion, which affects the performance of the material and the satisfaction of application standards.
Using two explosion welding technology, non-destructive testing and repair after one explosion welding, then secondary explosion welding, and pretreatment of substrate and cover plate and stress groove groove treatment before each welding, using specific types and The proportion of explosives and detonators is finally heat treated to improve bond strength and proportion.
It realizes efficient metallurgical combination of ultra-large thickness duplex stainless steel composite plates. The performance of bonding rate, tensile strength, yield strength and other properties meet or exceed national standards, avoids the problems of thick corrugation on the bonding surface and loose tooths, and is suitable for strict equipment manufacturing. environment.
Smart Images

Figure CN119057199A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of duplex steel composite plates, and in particular to a method for preparing a super-thick duplex stainless steel composite plate. Background Art
[0002] Explosive welding technology is a marginal subject between metal physics, explosion physics and welding science. It is a high-tech technology with great practical value that uses explosives as energy for metal-to-metal welding and production of metal composite materials. The most significant advantages of explosive welding technology are high welding strength, small heat-affected zone, high production efficiency, and theoretically applicable to various heterogeneous materials with impact toughness and elongation plasticity. Explosive welding has been widely used in petrochemical, marine engineering, aerospace, coal chemical and other industries with its core technical advantages. However, with the rapid development of domestic high-end equipment manufacturing industry, the requirements for the use of materials are becoming more and more stringent. Duplex stainless steel is increasingly favored by designers due to its excellent material mechanical properties and corrosion resistance. The yield strength of duplex stainless steel in the solution annealing state is more than twice that of standard austenitic stainless steel without nitrogen addition. At the same time, duplex stainless steel has shown strong advantages in acid corrosion resistance, alkali corrosion resistance, chloride pitting corrosion resistance, crevice corrosion resistance, and stress corrosion resistance.
[0003] Due to the characteristics of explosive welding, the thicker the coating material, the more difficult it is to achieve effective explosive welding, and the lower its bonding strength, and even problems such as composite interface delamination may occur in the later equipment manufacturing process. Especially for duplex stainless steel composite plates, since the coating duplex stainless steel contains two phases of austenite and ferrite, it is also an extremely important process to ensure that the phase ratio of ultra-thick duplex stainless steel meets the requirements of materials and related application standards while effectively achieving metallurgical bonding.
[0004] Therefore, it is of great significance to solve the technical problems of the existing explosive welding technology for ultra-thick duplex stainless steel composite plates, such as the difficulty in controlling the explosive bonding quality and ensuring the phase ratio. Summary of the invention
[0005] In view of this, the present invention provides a method for preparing an ultra-thick duplex stainless steel composite plate to solve the technical problems of the existing explosion welding technology for ultra-thick duplex stainless steel composite plates, such as difficulty in controlling the explosive bonding quality and ensuring the phase ratio.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] The present invention provides a method for preparing an ultra-thick duplex stainless steel composite plate, comprising the following steps:
[0008] S1. Pretreatment of the bonding surface between the substrate and the cover plate;
[0009] S2, parallel installation of base plate and cover plate;
[0010] S3. Arrange explosive frame above the covering plate;
[0011] S4, placing explosives in the explosive frame;
[0012] S5. Placement of detonators;
[0013] S6, perform explosion welding;
[0014] S7, non-destructive testing;
[0015] S8, repeating steps S1 to S6 to perform secondary explosion welding;
[0016] S9. Heat treatment of the composite plate obtained by secondary explosion welding.
[0017] Furthermore, in the step S1, the specific steps of pre-treating the bonding surface of the substrate and the cover plate are as follows: using an abrasive belt to treat the bonding surface of the substrate and the cover plate respectively;
[0018] The mesh number of the sanding belt used for the base plate is 50-60 mesh; the mesh number of the sanding belt used for the cover plate is 60-80 mesh;
[0019] The surface finish of the bonding surface of the substrate after pretreatment is ≤2μm; the surface finish of the bonding surface of the cover plate after pretreatment is ≤1.6μm;
[0020] Before pretreatment of the cladding plate, the non-bonding surface of the cladding plate is grooved with stress grooves; the depth of the stress groove is ≥ 1 / 2 of the thickness of the cladding plate, and the width of the stress groove is ≥ 1.5 mm; the stress groove is perpendicular to the cladding plate.
[0021] Furthermore, in step S2, the specific steps of parallel installation of the base plate and the cover plate are as follows: V-shaped feet are arranged between the base plate and the cover plate to ensure that the base plate and the cover plate are horizontal and placed in parallel;
[0022] The interval between each V-shaped pad is 300-350mm;
[0023] The spacing between the bonding surfaces of the substrate and the cover plate is 12 to 16 mm.
[0024] Furthermore, in step S3, the specific arrangement steps of the explosive frame are as follows: using cardboard and tape to arrange the explosive frame at the boundary position of the covering plate, and the explosive frame is perpendicular to the covering plate;
[0025] The setting height of the explosive frame is ≥80mm.
[0026] Further, in step S4, the explosive comprises 55-65% of powdered emulsion explosive and 35-45% of inert material, and the inert material comprises one or more of calcium carbonate, mica sand and quartz sand;
[0027] The specific steps of laying the explosives are as follows: evenly lay the explosives with a height of 75 to 95 mm in the explosive frame, and ensure that the laying height of the explosives within a range of 140 to 160 mm from the edge of the explosive frame is 67 to 87 mm.
[0028] Furthermore, in step S5, the specific steps of placing the detonator are as follows: a conical groove is set at the explosive at the center of the cladding plate, and high-intensity explosive is added therein, so that the high-intensity explosive is 2 to 3 mm higher than the explosive, and then a digital electronic detonator is vertically placed at the center of the high-intensity explosive;
[0029] The diameter of the tapered groove is 30 to 50 mm;
[0030] High-strength explosives are 100% pure powdered emulsion explosives.
[0031] Furthermore, in step S6, a digital electronic detonator is detonated to complete one explosion welding.
[0032] Furthermore, in step S7, the nondestructive testing includes performing nondestructive testing and repairing on the semi-finished composite plate obtained by the primary explosion welding, and then leveling it, and finally cutting and removing the collapsed edge areas around it.
[0033] Furthermore, in step S8, in addition to repeating steps S1 to S6 for secondary explosion welding, the process further includes performing a groove processing on the non-bonding surface of the cover plate after performing a stress groove processing on the non-bonding surface for placing a detonator;
[0034] The groove is arranged at the center of the non-joining surface of the covering plate;
[0035] The diameter of the groove is 40-60 mm, and the depth of the groove is ≥ 1 / 2 of the thickness of the covering plate;
[0036] In the secondary explosion welding, the semi-finished composite plate obtained by the primary explosion welding after non-destructive testing is used as the base plate.
[0037] Furthermore, in step S9, the heat treatment temperature is 520-560° C., and the heat treatment time is 320-400 min.
[0038] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0039] 1. The ultra-thick duplex stainless steel composite plate produced by the present invention has been shown by non-destructive testing, mechanical property testing, and phase ratio testing to have a bonding rate, bonding strength, tensile strength, yield strength, elongation after fracture, impact absorption energy, ferrite content, and corrosion resistance that meet or even far exceed the requirements of national or relevant industry standards (GB / T8165, NB / T47002.1, etc.); and has been shown by large-scale applications in various large-scale chemical equipment manufacturing industries to have technical parameters and physical and chemical properties that fully meet the harsh service environment and service conditions of special equipment.
[0040] 2. The ultra-thick duplex stainless steel composite plate produced by the present invention effectively avoids the problem of coarse corrugations on the bonding surface and even loose corrugations caused by increasing the amount of explosives to achieve effective bonding of ultra-thick coatings. At the same time, it can better meet the design requirements of design units and personnel for ultra-thick coatings.
[0041] 3. The double explosion welding technology described in the present invention can realize the processing and forming of various ultra-thickness clad explosion-welded composite plates. The present invention only describes and introduces the composite plate with ultra-thickness duplex stainless steel as the cladding. After adjustment and optimization by technicians in this industry, this technology can also realize the metallurgical bonding of more other ultra-thickness clad explosion-welded composite plates, providing a basis for the metallurgical bonding of ultra-thickness clad explosion-welded composite plates. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0043] Figure 1 The schematic diagram of the structure of an explosive welding process in the preparation of an ultra-thick duplex stainless steel composite plate is shown in FIG. 1, wherein: 1-explosive bed; 2-base plate; 3-V-shaped foot; 4-covering plate; 5-stress groove; 6-explosive frame; 7-explosive; 8-high-intensity explosive; 9-digital electronic detonator;
[0044] Figure 2 It is a structural schematic diagram of secondary explosion welding in the preparation process of ultra-thick duplex stainless steel composite plates, wherein 1-explosion bed, 3-V-shaped foot, 4-covering plate, 5-stress groove, 6-explosive frame, 7-explosive, 8-high-intensity explosive, 9-digital electronic detonator, 10-semi-finished composite plate obtained by primary explosion welding after non-destructive testing, and 11-groove. DETAILED DESCRIPTION
[0045] The present invention provides a method for preparing an ultra-thick duplex stainless steel composite plate, comprising the following steps:
[0046] S1. Pretreatment of the bonding surface between the substrate and the cover plate;
[0047] S2, parallel installation of base plate and cover plate;
[0048] S3. Arrange explosive frame above the covering plate;
[0049] S4, placing explosives in the explosive frame;
[0050] S5. Placement of detonators;
[0051] S6, perform explosion welding;
[0052] S7, non-destructive testing;
[0053] S8, repeating steps S1 to S6 to perform secondary explosion welding;
[0054] S9. Heat treatment of the composite plate obtained by secondary explosion welding.
[0055] In step S1 of the present invention, the specific steps of pre-treating the bonding surface of the substrate and the cover plate are as follows: using an abrasive belt to treat the bonding surface of the substrate and the cover plate respectively;
[0056] The mesh number of the sanding belt used for the substrate is preferably 50-60 mesh, more preferably 60 mesh; the mesh number of the sanding belt used for the cover plate is preferably 60-80 mesh, more preferably 80 mesh;
[0057] The surface finish of the bonding surface of the substrate after pretreatment is preferably ≤2 μm, more preferably ≤1.6 μm; the surface finish of the bonding surface of the cover plate after pretreatment is preferably ≤1.6 μm, more preferably ≤1.4 μm;
[0058] Before the pretreatment of the cladding plate, the non-bonding surface of the cladding plate is grooved with stress grooves; the depth of the stress groove is preferably ≥ 1 / 2 of the thickness of the cladding plate, and more preferably ≥ 2 / 3 of the thickness of the cladding plate; the width of the stress groove is preferably ≥ 1.5 mm, and more preferably ≥ 2.0 mm; the stress groove is perpendicular to the cladding plate.
[0059] In step S2 of the present invention, the specific steps of parallel installation of the base plate and the cover plate are as follows: V-shaped feet are arranged between the base plate and the cover plate to ensure that the base plate and the cover plate are horizontal and placed in parallel;
[0060] The interval between each V-shaped foot is preferably 300-350 mm, more preferably 320-340 mm;
[0061] The distance between the bonding surfaces of the substrate and the cover plate is preferably 12 to 16 mm, more preferably 14 to 15 mm.
[0062] In step S3 of the present invention, the specific arrangement steps of the explosive frame are as follows: using cardboard and tape to arrange the explosive frame at the boundary position of the covering plate, and the explosive frame is perpendicular to the covering plate;
[0063] The setting height of the explosive frame is preferably ≥80 mm, more preferably ≥90 mm, and even more preferably ≥100 mm.
[0064] In step S4 of the present invention, the explosive preferably comprises 55-65% of powdered emulsion explosive and 35-45% of inert material, more preferably 60-62% of powdered emulsion explosive and 38-40% of inert material, and the inert material preferably comprises one or more of calcium carbonate, mica sand and quartz sand;
[0065] The specific steps of laying the explosives are as follows: evenly lay the explosives with a height of 75 to 95 mm in the explosive frame, and ensure that the explosives within the range of 140 to 160 mm from the edge of the explosive frame are laid with a height of 67 to 87 mm;
[0066] The laying height of the explosive is preferably 78-82 mm, more preferably 80 mm; the laying height of the explosive within 140-160 mm from the edge of the explosive frame is preferably 70-85 mm, more preferably 72-75 mm, and more preferably 73-74 mm.
[0067] In step S5 of the present invention, the specific steps of placing the detonator are as follows: a conical groove is set at the explosive at the center of the cladding plate, and high-intensity explosive is added therein so that the high-intensity explosive is 2 to 3 mm higher than the explosive, and then a digital electronic detonator is vertically placed at the center of the high-intensity explosive;
[0068] The diameter of the tapered groove is preferably 30 to 50 mm, more preferably 35 to 45 mm, and more preferably 40 mm;
[0069] The high explosive is preferably a 100% pure powdered emulsion explosive.
[0070] In step S6 of the present invention, the digital electronic detonator is detonated to complete one explosion welding.
[0071] In step S7 of the present invention, the nondestructive testing includes performing nondestructive testing and repairing on the semi-finished composite plate obtained by the primary explosion welding, and then leveling it, and finally cutting and removing the collapsed edge areas around it.
[0072] In step S8 of the present invention, in addition to repeating steps S1 to S6 for secondary explosion welding, the process further includes performing a groove processing on the non-bonding surface of the cover plate after performing a stress groove processing on the non-bonding surface for placing a detonator;
[0073] The groove is arranged at the center of the non-joining surface of the covering plate;
[0074] The diameter of the groove is preferably 40 to 60 mm, more preferably 50 mm; the depth of the groove is preferably ≥ 1 / 2 of the thickness of the covering plate, more preferably ≥ 2 / 3 of the thickness of the covering plate;
[0075] In the secondary explosion welding, the semi-finished composite plate obtained by the primary explosion welding after non-destructive testing is used as the base plate.
[0076] In step S9 of the present invention, the temperature of the heat treatment is preferably 520-560° C., more preferably 540-550° C.; the time of the heat treatment is preferably 320-400 min, more preferably 360-380 min.
[0077] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0078] Example 1
[0079] 1. Material selection:
[0080] Substrate: The substrate is made of Q345R container steel plate, with specific specifications and dimensions: thickness 96mm, width 2160mm, length 5200mm;
[0081] Cover plate: The cover plate used for primary explosion welding is made of duplex stainless steel S22053, with specific specifications and dimensions: thickness 12mm, width 2210mm, length 5250mm;
[0082] The covering plate used for secondary explosion welding is made of duplex stainless steel S22053, with specific specifications and dimensions: thickness 10mm, width 2150mm, and length 5190mm.
[0083] 2. Specific preparation method:
[0084] (1) Place the substrate evenly on the cover plate used for primary explosion welding, mark along the substrate boundary size, and then use a handheld cutting machine to dig a stress groove with a width of 2 mm on the explosion surface of the cover plate used for primary explosion welding along the inner side of the marked line. The depth of the stress groove is 1 / 2 of the thickness of the cover plate to ensure that the stress groove is relatively straight.
[0085] (2) Use an 80-mesh hand-pushed belt sander to remove the surface oxides of the cover plate used for primary explosive welding to expose the metallic luster, so that the surface finish meets the requirement of 1.6μm, and at the same time, there shall be no other surface defects such as oil, debris, pits, etc. on the surface of the bonding surface; use a 60-mesh fully automatic belt sander to remove the surface oxides of the substrate to expose the metallic luster, so that the surface finish meets the requirement of 2.0μm, and there shall be no surface defects such as wrinkles, excessive pitting, etc.
[0086] (3) Place the substrate horizontally on the explosion bed, clean the joint surface with acetone, and then evenly place V-shaped pads with a height of 14 mm. The V-shaped pads are placed parallel to the horizontal and vertical coordinates of the substrate, with a spacing of 300 mm between each other. The four edges should be placed no more than 5 mm away from the edge. Then clean the joint surface of the cover plate used for the first explosion welding with acetone, and then place it horizontally with the joint surface facing down on top of the V-shaped pads. When placing, the stress groove of the explosion surface of the cover plate used for the first explosion welding should be perpendicular to the lower substrate and correspond to the boundary of the lower substrate. At the same time, pay attention that no other debris should be brought into the joint surface between the substrate and the cover plate used for the first explosion welding.
[0087] (4) A 90mm high explosive frame is set up around the parallel-placed cover plate for primary explosive welding using 3mm thick cardboard and tape. The cardboard is required to be perpendicular to the cover plate for primary explosive welding, and the range of the explosive frame is consistent with the boundary of the cover plate for primary explosive welding. The cardboard interface position should also be sealed with tape. Then, 100% pure powdered emulsion explosive is evenly placed in the explosive frame with a height of 82mm, and the explosive placement height within 150mm from the edge of the cover plate for primary explosive welding is appropriately reduced to 72-74mm.
[0088] (5) A conical groove of φ=30 mm is cut out at the center of the cover plate used for primary explosive welding, and then high-intensity explosives are added to make the high-intensity explosives 2-3 mm higher than the surrounding explosives, and then the high-intensity explosives are gently flattened, and then a digital electronic detonator is vertically placed at the center of the high-intensity explosives. The digital electronic detonator is then detonated to obtain a semi-finished composite plate.
[0089] (6) The semi-finished composite plate is transported back to the production area for non-destructive testing and repair, and then leveled. At the same time, the edge collapse area is cut and removed to obtain a composite plate blank with a specification size of (12+160)×2100×5140mm. Subsequently, an 80-mesh sand belt is used to grind the cladding surface of the composite plate blank to remove the surface oxide layer formed by the primary explosive welding. The local slight scratches and pits are polished and removed by a straight grinder, so that the surface finish of the entire plate is ≤1.6μm, and there are no local pits and pits. Then the explosion surface of the cover plate used for secondary explosion welding is marked according to the size of the composite slab, and then a hand-held cutter is used to dig a stress groove with a width of 2mm on the explosion surface of the cover plate used for secondary explosion welding along the inner side of the marking line. The depth of the stress groove is 1 / 2 of the thickness of the cover plate, and then an angle grinder and a grinding cone are used to grind a groove with a depth of φ=50mm and a depth of 1 / 2 of the thickness of the cover plate used for secondary explosion welding at the center of the cover plate used for secondary explosion welding for placing detonators. Subsequently, an 80-mesh hand-pushed sanding machine is used to remove the surface oxide of the cover plate used for secondary explosion welding, exposing the metallic luster, so that the smoothness of the joint surface meets the requirement of 1.6μm, and at the same time, there shall be no other surface defects such as oil stains, debris, and pits on the joint surface.
[0090] (7) Place the composite slab horizontally on the prepared blasting bed, clean the bonding surface with acetone, and evenly place V-shaped pads with a height of 12 mm in accordance with the requirements of the above step (3). Then, place the cover plate used for secondary explosion welding, which has been cleaned with acetone, horizontally on the V-shaped pads with the bonding surface facing downward. The stress groove of the cover plate used for secondary explosion welding is required to be perpendicular to the composite slab below and correspond to the boundary of the composite slab below. At the same time, it should be noted that no other debris should be brought into the bonding surface between the base plate and the cover plate used for secondary explosion welding.
[0091] (8) Use 3mm thick cardboard and tape to set up a 80mm high explosive frame around the parallel-placed secondary explosive welding cover plate. The cardboard must be perpendicular to the secondary explosive welding cover plate, and the range of the explosive frame must be consistent with the boundary of the secondary explosive welding cover plate. The cardboard interface must also be sealed with tape. Then evenly place 100% pure powdered emulsion explosive with a height of 75mm in the explosive frame, and appropriately reduce the explosive placement height within 150mm from the edge of the secondary explosive welding cover plate to 67-70mm.
[0092] (9) Dig out a conical groove of φ=50mm in the center groove of the cover plate used for secondary explosive welding, then add a small amount of high-intensity explosive to make the high-intensity explosive 2-3mm higher than the surrounding explosives, gently flatten it, and then place the digital electronic detonator vertically in the center of the high-intensity explosive, and the digital electronic detonator must be perpendicular to the center of the groove of the cover plate used for secondary explosive welding.
[0093] (10) The digital electronic detonator is detonated to complete the secondary explosion welding, and a composite plate with a specification size of (22+96)×2100×5140 mm is obtained.
[0094] (11) The composite plate after secondary explosion welding is placed in a heat treatment furnace for stress relief treatment at 540°C and kept warm for 260 minutes to obtain an ultra-thick duplex stainless steel composite plate.
[0095] After inspection, the mechanical and chemical properties of the ultra-thick duplex stainless steel composite plates meet the relevant requirements of the industry standard NB / T47002.1-2019.
[0096] Example 2
[0097] 1. Material selection:
[0098] Substrate: The substrate is made of ASME SA516Gr70N American standard container steel plate, with specific specifications and dimensions: thickness 125mm, width 2380mm, length 4390mm;
[0099] Cover plate: The cover plate used for primary explosion welding is made of ASME SA-240 / SA-240M American standard duplex stainless steel 2205, with specific specifications and dimensions: thickness 14mm, width 2440mm, length 4450mm;
[0100] The covering plate used for secondary explosion welding is made of ASME SA240 American standard duplex stainless steel 2205, with specific specifications and dimensions: thickness 12mm, width 2360mm, and length 4370mm.
[0101] 2. Specific preparation method:
[0102] (1) Place the substrate evenly on the cover plate used for primary explosion welding, mark along the substrate boundary size, and then use a handheld cutting machine to dig a stress groove with a width of 2 mm on the explosion surface of the cover plate used for primary explosion welding along the inner side of the marked line. The depth of the stress groove is 1 / 2 of the thickness of the cover plate to ensure that the stress groove is relatively straight.
[0103] (2) Use an 80-mesh hand-pushed belt sander to remove the surface oxides of the cover plate used for primary explosive welding to expose the metallic luster, so that the surface finish meets the requirement of 1.6μm, and at the same time, there shall be no other surface defects such as oil, debris, pits, etc. on the surface of the bonding surface; use a 60-mesh fully automatic belt sander to remove the surface oxides of the substrate to expose the metallic luster, so that the surface finish meets the requirement of 2.0μm, and there shall be no surface defects such as wrinkles, excessive pitting, etc.
[0104] (3) Place the substrate horizontally on the explosion bed, clean the joint surface with acetone, and then evenly place V-shaped pads with a height of 16 mm. The V-shaped pads are placed parallel to the horizontal and vertical coordinates of the substrate, with a spacing of 300 mm between each other. The four edges should be placed no more than 5 mm away from the edge. Then clean the joint surface of the cover plate used for the first explosion welding with acetone, and then place it horizontally with the joint surface facing down on top of the V-shaped pads. When placing, the stress groove of the explosion surface of the cover plate used for the first explosion welding should be perpendicular to the lower substrate and correspond to the boundary of the lower substrate. At the same time, pay attention that no other debris should be brought into the joint surface between the substrate and the cover plate used for the first explosion welding.
[0105] (4) A 100mm high explosive frame is set up around the parallel-placed cover plate for primary explosive welding using 3mm thick cardboard and adhesive tape. The cardboard is required to be perpendicular to the cover plate for primary explosive welding, and the range of the explosive frame is consistent with the boundary of the cover plate for primary explosive welding. The cardboard interface position should also be sealed with adhesive tape. Then, 100% pure powdered emulsion explosive is evenly placed in the explosive frame with a height of 95mm. The explosive placement height within the range of 150mm from the edge of the cover plate for primary explosive welding is appropriately reduced to 85-87mm.
[0106] (5) A conical groove of φ=30 mm is cut out at the center of the cover plate used for primary explosive welding, and then high-intensity explosives are added to make the high-intensity explosives 2-3 mm higher than the surrounding explosives, and then the high-intensity explosives are gently flattened, and then a digital electronic detonator is vertically placed at the center of the high-intensity explosives. The digital electronic detonator is then detonated to obtain a semi-finished composite plate.
[0107] (6) The semi-finished composite plate is transported back to the production area for non-destructive testing and repair, and then leveled. At the same time, the edge collapse area is cut and removed to obtain a composite plate blank with a specification size of (14+125)×2300×4310mm. Subsequently, an 80-mesh sand belt is used to grind the cladding surface of the composite plate blank to remove the surface oxide layer formed by the primary explosive welding. The local slight scratches and pits are polished and removed by a straight grinder, so that the surface finish of the entire plate is ≤1.6μm, and there are no local pits and pits. Then the explosion surface of the cover plate used for secondary explosion welding is marked according to the size of the composite slab, and then a hand-held cutter is used to dig a stress groove with a width of 2mm on the explosion surface of the cover plate used for secondary explosion welding along the inner side of the marking line. The depth of the stress groove is 1 / 2 of the thickness of the cover plate, and then an angle grinder and a grinding cone are used to grind a groove with a depth of φ=50mm and a depth of 1 / 2 of the thickness of the cover plate used for secondary explosion welding at the center of the cover plate used for secondary explosion welding for placing detonators. Subsequently, an 80-mesh hand-pushed sanding machine is used to remove the surface oxide of the cover plate used for secondary explosion welding, exposing the metallic luster, so that the smoothness of the joint surface meets the requirement of 1.6μm, and at the same time, there shall be no other surface defects such as oil stains, debris, and pits on the joint surface.
[0108] (7) Place the composite slab horizontally on the prepared blasting bed, clean the bonding surface with acetone, and evenly place V-shaped pads with a height of 14 mm in accordance with the requirements of the above step (3). Then, place the cover plate used for secondary explosion welding, which has been cleaned with acetone, horizontally on the V-shaped pads with the bonding surface facing downward. The stress groove of the cover plate used for secondary explosion welding is required to be perpendicular to the composite slab below and correspond to the boundary of the composite slab below. At the same time, it should be noted that no other debris should be brought into the bonding surface between the base plate and the cover plate used for secondary explosion welding.
[0109] (8) Use 3mm thick cardboard and tape to set up a 90mm high explosive frame around the parallel-placed secondary explosive welding cover plate. The cardboard must be perpendicular to the secondary explosive welding cover plate, and the range of the explosive frame must be consistent with the boundary of the secondary explosive welding cover plate. The cardboard interface must also be sealed with tape. Then evenly place 100% pure powdered emulsion explosive with a height of 80mm in the explosive frame, and appropriately reduce the explosive placement height within 150mm from the edge of the secondary explosive welding cover plate to 72-75mm.
[0110] (9) Dig out a conical groove of φ=50mm in the center groove of the cover plate used for secondary explosive welding, then add a small amount of high-intensity explosive to make the high-intensity explosive 2-3mm higher than the surrounding explosives, gently flatten it, and then place the digital electronic detonator vertically in the center of the high-intensity explosive, and the digital electronic detonator must be perpendicular to the center of the groove of the cover plate used for secondary explosive welding.
[0111] (10) The digital electronic detonator is detonated to complete the secondary explosion welding, and a composite plate with a specification size of (26+125)×2300×4310 mm is obtained.
[0112] (11) The composite plate after secondary explosion welding is placed in a heat treatment furnace for stress relief treatment at 550°C and kept warm for 315 minutes to obtain an ultra-thick duplex stainless steel composite plate.
[0113] After inspection, the physical and chemical properties of the ultra-thick duplex stainless steel composite plate fully meet the relevant requirements of ASME SA-264 / SA-264M.
[0114] Example 3
[0115] 1. Material selection:
[0116] Substrate: The substrate is made of Q345B low alloy steel plate, with specific specifications and dimensions: thickness 160mm, width 1920mm, length 2360mm;
[0117] Cover plate: The cover plate used for primary explosion welding is made of duplex stainless steel 2205, with specific specifications and dimensions: thickness 12mm, width 1980mm, length 2420mm;
[0118] The covering plate used for secondary explosion welding is made of duplex stainless steel 2205, with specific specifications and dimensions: thickness 12mm, width 1920mm, and length 2360mm.
[0119] 2. Specific preparation method:
[0120] (1) Place the substrate evenly on the cover plate used for primary explosion welding, mark along the substrate boundary size, and then use a handheld cutting machine to dig a stress groove with a width of 2 mm on the explosion surface of the cover plate used for primary explosion welding along the inner side of the marked line. The depth of the stress groove is 1 / 2 of the thickness of the cover plate to ensure that the stress groove is relatively straight.
[0121] (2) Use an 80-mesh hand-pushed belt sander to remove the surface oxides of the cover plate used for primary explosive welding to expose the metallic luster, so that the surface finish meets the requirement of 1.6μm, and at the same time, there shall be no other surface defects such as oil, debris, pits, etc. on the surface of the bonding surface; use a 60-mesh fully automatic belt sander to remove the surface oxides of the substrate to expose the metallic luster, so that the surface finish meets the requirement of 2.0μm, and there shall be no surface defects such as wrinkles, excessive pitting, etc.
[0122] (3) Place the substrate horizontally on the explosion bed, clean the joint surface with acetone, and then evenly place V-shaped pads with a height of 14 mm. The V-shaped pads are placed parallel to the horizontal and vertical coordinates of the substrate, with a spacing of 300 mm between each other. The four edges should be placed no more than 5 mm away from the edge. Then clean the joint surface of the cover plate used for the first explosion welding with acetone, and then place it horizontally with the joint surface facing down on top of the V-shaped pads. When placing, the stress groove of the explosion surface of the cover plate used for the first explosion welding should be perpendicular to the lower substrate and correspond to the boundary of the lower substrate. At the same time, pay attention that no other debris should be brought into the joint surface between the substrate and the cover plate used for the first explosion welding.
[0123] (4) A 90mm high explosive frame is set up around the parallel-placed cover plate for primary explosive welding using 3mm thick cardboard and tape. The cardboard is required to be perpendicular to the cover plate for primary explosive welding, and the range of the explosive frame is consistent with the boundary of the cover plate for primary explosive welding. The cardboard interface position should also be sealed with tape. Then, 100% pure powdered emulsion explosive is evenly placed in the explosive frame with a height of 82mm, and the explosive placement height within 150mm from the edge of the cover plate for primary explosive welding is appropriately reduced to 72-74mm.
[0124] (5) A conical groove of φ=30 mm is cut out at the center of the cover plate used for primary explosive welding, and then high-intensity explosives are added to make the high-intensity explosives 2-3 mm higher than the surrounding explosives, and then the high-intensity explosives are gently flattened, and then a digital electronic detonator is vertically placed at the center of the high-intensity explosives. The digital electronic detonator is then detonated to obtain a semi-finished composite plate.
[0125] (6) The semi-finished composite plate is transported back to the production area for non-destructive testing and repair, and then leveled. At the same time, the edge collapse area is cut and removed to obtain a composite plate blank with a specification size of (12+160)×1860×2300mm. Subsequently, an 80-mesh sand belt is used to grind the cladding surface of the composite plate blank to remove the surface oxide layer formed by the primary explosive welding. A straight grinder is used to polish and remove local slight scratches and pits, so that the surface finish of the entire plate is ≤1.6μm, and there are no local pits and pits. Then the explosion surface of the cover plate used for secondary explosion welding is marked according to the size of the composite slab, and then a hand-held cutter is used to dig a stress groove with a width of 2mm on the explosion surface of the cover plate used for secondary explosion welding along the inner side of the marking line. The depth of the stress groove is 1 / 2 of the thickness of the cover plate, and then an angle grinder and a grinding cone are used to grind a groove with a depth of φ=50mm and a depth of 1 / 2 of the thickness of the cover plate used for secondary explosion welding at the center of the cover plate used for secondary explosion welding for placing detonators. Subsequently, an 80-mesh hand-pushed sanding machine is used to remove the surface oxide of the cover plate used for secondary explosion welding, exposing the metallic luster, so that the smoothness of the joint surface meets the requirement of 1.6μm, and at the same time, there shall be no other surface defects such as oil stains, debris, and pits on the joint surface.
[0126] (7) Place the composite slab horizontally on the prepared blasting bed, clean the bonding surface with acetone, and evenly place V-shaped pads with a height of 14 mm in accordance with the requirements of the above step (3). Then, place the cover plate used for secondary explosion welding, which has been cleaned with acetone, horizontally on the V-shaped pads with the bonding surface facing downward. The stress groove of the cover plate used for secondary explosion welding is required to be perpendicular to the composite slab below and correspond to the boundary of the composite slab below. At the same time, it should be noted that no other debris should be brought into the bonding surface between the base plate and the cover plate used for secondary explosion welding.
[0127] (8) Use 3mm thick cardboard and tape to set up a 80mm high explosive frame around the parallel-placed secondary explosive welding cover plate. The cardboard must be perpendicular to the secondary explosive welding cover plate, and the range of the explosive frame must be consistent with the boundary of the secondary explosive welding cover plate. The cardboard interface must also be sealed with tape. Then evenly place 100% pure powdered emulsion explosive with a height of 78mm in the explosive frame, and appropriately reduce the explosive placement height within 150mm from the edge of the secondary explosive welding cover plate to 70-73mm.
[0128] (9) Dig out a conical groove of φ=50mm in the center groove of the cover plate used for secondary explosive welding, then add a small amount of high-intensity explosive to make the high-intensity explosive 2-3mm higher than the surrounding explosives, gently flatten it, and then place the digital electronic detonator vertically in the center of the high-intensity explosive, and the digital electronic detonator must be perpendicular to the center of the groove of the cover plate used for secondary explosive welding.
[0129] (10) The digital electronic detonator is detonated to complete the secondary explosion welding, and a composite plate with a specification size of (24+160)×1860×2300 mm is obtained.
[0130] (11) The composite plate after secondary explosion welding is placed in a heat treatment furnace for stress relief treatment at 530°C and kept warm for 375 minutes to obtain an ultra-thick duplex stainless steel composite plate.
[0131] After inspection, the mechanical and chemical properties of the ultra-thick duplex stainless steel composite plates meet the relevant requirements of the industry standard NB / T47002.1-2019.
[0132] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing an ultra-thick duplex stainless steel composite plate, characterized in that: The steps include: S1. Pretreatment of the bonding surface between the substrate and the cover plate; S2, parallel installation of base plate and cover plate; S3. Arrange explosive frame above the covering plate; S4, placing explosives in the explosive frame; S5. Placement of detonators; S6, perform explosion welding; S7, non-destructive testing; S8, repeating steps S1 to S6 to perform secondary explosion welding; S9. Heat treatment of the composite plate obtained by secondary explosion welding.
2. The method for preparing the ultra-thick duplex stainless steel composite plate according to claim 1, characterized in that: In the step S1, the specific steps of pre-treating the bonding surface of the substrate and the cover plate are as follows: using an abrasive belt to treat the bonding surface of the substrate and the cover plate respectively; The mesh number of the sanding belt used for the base plate is 50-60 mesh; the mesh number of the sanding belt used for the cover plate is 60-80 mesh; The surface finish of the bonding surface of the substrate after pretreatment is ≤2μm; the surface finish of the bonding surface of the cover plate after pretreatment is ≤1.6μm; Before pretreatment of the cladding plate, the non-bonding surface of the cladding plate is grooved with stress grooves; the depth of the stress groove is ≥ 1 / 2 of the thickness of the cladding plate, and the width of the stress groove is ≥ 1.5 mm; the stress groove is perpendicular to the cladding plate.
3. The method for preparing the ultra-thick duplex stainless steel composite plate according to claim 1 or 2, characterized in that: In step S2, the specific steps of parallel installation of the base plate and the cover plate are as follows: V-shaped feet are arranged between the base plate and the cover plate to ensure that the base plate and the cover plate are placed horizontally and in parallel; The interval between each V-shaped pad is 300-350mm; The spacing between the bonding surfaces of the substrate and the cover plate is 12 to 16 mm.
4. The method for preparing the ultra-thick duplex stainless steel composite plate according to claim 3, characterized in that: In step S3, the specific arrangement steps of the explosive frame are as follows: using cardboard and tape to arrange the explosive frame at the boundary position of the covering plate, and the explosive frame is perpendicular to the covering plate; The setting height of the explosive frame is ≥80mm.
5. The method for preparing the ultra-thick duplex stainless steel composite plate according to claim 1, 2 or 4, characterized in that: In step S4, the explosive comprises 55-65% of powdered emulsion explosive and 35-45% of inert material, and the inert material comprises one or more of calcium carbonate, mica sand and quartz sand; The specific steps of laying the explosives are as follows: evenly lay the explosives with a height of 75 to 95 mm in the explosive frame, and ensure that the laying height of the explosives within a range of 140 to 160 mm from the edge of the explosive frame is 67 to 87 mm.
6. The method for preparing the ultra-thick duplex stainless steel composite plate according to claim 5, characterized in that: In step S5, the specific steps of placing the detonator are as follows: a conical groove is set at the explosive at the center of the cladding plate, and high-intensity explosive is added therein, so that the high-intensity explosive is 2 to 3 mm higher than the explosive, and then a digital electronic detonator is vertically placed at the center of the high-intensity explosive; The diameter of the tapered groove is 30 to 50 mm; High-strength explosives are 100% pure powdered emulsion explosives.
7. The method for preparing the ultra-thick duplex stainless steel composite plate according to claim 6, characterized in that: In step S6, the digital electronic detonator is detonated to complete one explosion welding.
8. The method for preparing the ultra-thick duplex stainless steel composite plate according to claim 7, characterized in that: In step S7, the nondestructive testing includes performing nondestructive testing and repairing on the semi-finished composite plate obtained by the primary explosion welding, and then leveling it, and finally cutting and removing the collapsed edge areas around it.
9. The method for preparing the ultra-thick duplex stainless steel composite plate according to claim 2, characterized in that: In the step S8, in addition to repeating the steps S1 to S6 for secondary explosion welding, the step further includes, after the stress grooves are grooved on the non-bonding surface of the cover plate, grooves are grooved on the non-bonding surface for placing detonators; The groove is arranged at the center of the non-joining surface of the covering plate; The diameter of the groove is 40-60 mm, and the depth of the groove is ≥ 1 / 2 of the thickness of the covering plate; In the secondary explosion welding, the semi-finished composite plate obtained by the primary explosion welding after non-destructive testing is used as the base plate.
10. The method for preparing the ultra-thick duplex stainless steel composite plate according to any one of claims 6 to 9, characterized in that: In the step S9, the heat treatment temperature is 520-560° C., and the heat treatment time is 320-400 min.