Nickel-based superalloy laser welding heat affected zone liquefaction crack control method
By adopting laser reciprocating technology in nickel-based high-temperature alloy laser welding, the problem of liquefied crack control in the heat-affected zone of nickel-based high-temperature alloy laser welding is solved, and high-quality welding is achieved in a high-efficiency non-vacuum environment, reducing crack formation and welding cost.
Patent Information
- Application Number
- CN202310623781.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
AI Technical Summary
Liquefied cracks in the thermally affected zone of nickel-based high-temperature alloy laser welding are difficult to control. The existing methods have huge safety hazards for cracks under high temperature conditions, and often require vacuum environment and complex process parameters optimization.
The laser welding technology is adopted to perform linear reciprocating motion during the laser advancement process, and the nickel-based high-temperature alloy is docked or spliced with single-channel lasers to reduce the temperature of the heat-affected zone and reduce the formation of liquefied cracks. The specific steps include providing the laser beam to advance along the surface of the splicing seam and performing vertical reciprocating motion, ensuring that the weld is permeable and the single-pass weld depth is ≧4mm, setting a high welding speed and power, and controlling the laser parameters to reduce cracks.
It effectively suppresses liquefied cracks in the heat-affected zone of high-temperature alloy laser welding, improves welding structure density and joint quality, reduces welding costs, and achieves high-efficiency welding in a non-vacuum environment.
Smart Images

Figure CN119057243A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of laser welding, and in particular relates to a method for controlling liquefaction cracks in a heat-affected zone of laser welding of a nickel-based high-temperature alloy. Background Art
[0002] Nickel-based superalloys have good organization and thermal stability, oxidation resistance and corrosion resistance under high temperature (>650℃) conditions, and have been widely used in aerospace, aviation and nuclear power fields. Laser welding has the advantages of concentrated energy, narrow heat-affected zone, high welding efficiency, small deformation of joints after welding and no need for vacuum, and will be widely used in the field of superalloy welding. There are many types of nickel-based superalloys, mainly divided into solid solution-strengthened nickel-based superalloys and precipitation-strengthened nickel-based superalloys, and the strengthening mechanisms and organizational morphologies of the two are completely different.
[0003] The laser welded joint of nickel-based high-temperature alloy has high crack sensitivity and many types of cracks, such as solidification cracks, liquefaction cracks, strain aging cracks, and ductile penetration cracks, but the formation mechanism and formation area of these cracks are different. The weld in the welded joint (its temperature is ﹥1350~1380℃) and the heat-affected zone (its peak temperature is ≦1350~1380℃) belong to two areas of different nature, and their peak temperature, material heating and melting state, temperature gradient, microstructure evolution and stress strain are completely different. Liquefaction cracks occur in the heat-affected zone of laser welding (heat-affected zone: the peak temperature of this area is lower than the melting point of the material, and this area does not melt during the welding process, but the microstructure or performance will change under the action of welding thermal cycle), and the intergranular impurity elements under high temperature conditions are segregated and liquefied, and the components of the high melting point phase are liquefied and cracked along the grain under the action of tensile stress. Therefore, liquefaction cracks will bury a huge safety hazard for the high-temperature service of high-temperature alloy welded parts.
[0004] Compared with traditional welding methods such as melting welding (TIG and MAG) and brazing, laser welding has concentrated energy, narrow heat-affected zone, low heat input, and extremely fast heating and cooling, which leads to the formation of liquefaction cracks in the heat-affected zone of laser welding of nickel-based high-temperature alloys. At present, researchers control or inhibit liquefaction cracks in the heat-affected zone of laser welding of nickel-based high-temperature alloys by preheating before welding, heat treatment before and after welding, and optimizing process welding parameters.
[0005] Cui Haichao et al. (CN106077951) from Shanghai Jiaotong University used the laser wire-filling welding remelting process to control cracks in the heat-affected zone of high-temperature alloys based on the theory of stress distribution of laser joints and reducing the high-temperature residence time of the heat-affected zone at the overlap. Since this technology (CN106077951) controls cracks in the heat-affected zone by wire-filling remelting, it is difficult to control cracks in this method and is prone to new cracks.
[0006] Chen Bo et al. from Harbin Institute of Technology (CN 113977080) used scanning laser welding to connect nickel-based high-temperature alloys, achieving the regulation of continuous and coarse Laves phase inside the weld, and then obtaining fine and dispersed Laves phase, which helps to suppress the generation of microcracks inside the weld. The method of this invention (CN 113977080) is mainly aimed at regulating the Laves phase in the weld, and the temperature of this area is higher than 1380℃.
[0007] Chen Xi et al. (CN 114589403) of Harbin University of Technology Welding Technology Co., Ltd. used a welding device of swinging laser ultrasonic welding + accompanying condensation plate in a vacuum environment to control the heat affected zone of laser welding and refine the organization. The method of this invention (CN114589403) requires welding under vacuum conditions, and requires the accompanying condensation plate and ultrasonic device to be combined to achieve the purpose of controlling the heat affected zone and refining the organization. Its core principle is to increase the cooling speed and heat dissipation of the laser welding joint by controlling the flow rate and temperature of the coolant in the accompanying condensation plate, thereby achieving control of the heat affected zone. It is essentially different from the principle of the present invention.
[0008] Similarly, Zhao Mingjiu et al. (CN 104475960) from the Institute of Metal Research, Chinese Academy of Sciences, used scanning electron beam welding to connect iron-nickel-based superalloys, and there was no γ' zone and grain boundary liquefaction in the heat-affected zone of the welded joint. The method of this invention (CN 104475960) requires multiple passes of welding under vacuum conditions and is aimed at iron-nickel (Fe-Ni)-based superalloys, which increases the difficulty of operation. In addition, the heat dissipation coefficient of the material under vacuum conditions is completely different from that under non-vacuum conditions, and the microstructure, thermal conductivity and precipitation phase diffusion coefficient of iron-nickel (Fe-Ni)-based superalloys are essentially different from those of nickel-based superalloys.
[0009] The research of Dr. Ren Wenjie's thesis of Shanghai Jiaotong University shows that: under the conditions of welding speed (≧1.0m / min) and low welding heat input, there are many liquefaction cracks in the heat-affected zone of laser welding of nickel-based high-temperature alloys. The liquefaction cracks in the heat-affected zone of laser welding of high-temperature alloys can be suppressed by significantly reducing the welding speed or increasing the laser power (i.e. increasing the welding heat input), preheating before welding, heat treatment before welding and increasing the defocus. However, a significant increase in laser power is not conducive to weld formation and can easily lead to obvious collapse of the weld surface; a significant reduction in welding speed cannot reflect the advantage of high efficiency of laser welding. Increasing the defocus will reduce the weld penetration, resulting in incomplete weld penetration.
[0010] Lai Jing and others from Huazhong University of Science and Technology used a pulsed laser powder feeding process to control the generation of liquefaction cracks in nickel-based high-temperature alloy welding. However, the welding penetration of this method is relatively shallow and cannot reach a weld depth of more than 4mm, so it is not suitable for plate laser butt welding. Summary of the invention
[0011] In view of the difficulty of controlling liquefaction cracks in the temperature range of 1280°C to 1380°C of the heat affected zone of laser welding of solid solution strengthened nickel-based high-temperature alloys and the shortcomings of the above-mentioned existing crack control methods, the present invention proposes a method for controlling liquefaction cracks in the heat affected zone of laser welding of nickel-based high-temperature alloys (with a temperature range of 1280°C to 1380°C).
[0012] After extensive and in-depth research and numerous experiments, the inventors have found that lasers that move in a straight line and reciprocate (the direction of movement is perpendicular to the welding direction) are used to perform single-pass laser butt joint or splicing of nickel-based high-temperature alloys, thereby reducing liquefaction cracks in the 1280°C to 1380°C temperature range of the heat-affected zone of laser welding of high-temperature alloys. The present invention was completed on this basis.
[0013] In order to solve the above problems and shortcomings, the present invention provides a method for controlling liquefaction cracks in the heat-affected zone of laser welding of solid solution strengthened nickel-based high-temperature alloys, the steps of which are as follows:
[0014] A pair of nickel-based high-temperature alloys are provided, and the end faces of the high-temperature alloys are spliced, and the splicing seam forms a to-be-welded area; a laser welding light source provides at least one laser beam, and the laser beam irradiates the upper surface of the splicing seam continuously for a single time to form molten metal, and the laser beam is advanced along the upper surface of the splicing seam to melt and solidify the high-temperature alloy in the laser beam contact area to form a weld, thereby completing the laser single-sided welding and double-sided forming in one step;
[0015] The method comprises:
[0016] 1) The laser beam is moved back and forth in a straight line perpendicular to the welding direction during the welding process (welding direction) to perform laser deep penetration welding, so that the weld is fully melted and the depth of the single weld is ≥4 mm.
[0017] 2) The optical power of its laser welding power is ≧6000W, the welding speed is ≧2.1m / min, the laser reciprocating movement frequency is ≧250Hz, the laser vertical movement amplitude is 1.5~2.5mm, the focal spot diameter is 0.4mm~0.6mm, and the laser tilt angle is 0°~5°, which can greatly reduce the temperature of the heat affected zone of nickel-based high-temperature alloy laser welding in the 1280℃~1380℃ area and cause liquefaction cracks.
[0018] It should be understood that within the scope of the present invention, the above-mentioned technical features of the present invention and the technical features specifically described below (such as embodiments) can be combined with each other to form a new or preferred technical solution. Due to space limitations, they will not be described one by one here.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The nickel-based high-temperature alloy laser welding technology adopted in the present invention can effectively suppress the weld surface collapse caused by excessively high power density in ordinary laser welding, significantly improve the weld formation, and improve the density and joint quality of the nickel-based high-temperature alloy laser welded joint.
[0021] 2. The nickel-based high-temperature alloy laser welding technology adopted in the present invention, on the one hand, effectively inhibits the formation of eutectic phase in the heat-affected zone of the high-temperature alloy laser welding, and on the other hand, reduces the cooling rate of the heat-affected zone and reduces the formation of liquefaction cracks.
[0022] 3. The nickel-based high-temperature alloy laser welding technology adopted by the present invention can reduce the liquefaction cracks in the heat-affected zone of the nickel-based high-temperature alloy laser welding under the conditions of high welding speed and good weld formation.
[0023] 4. The nickel-based high-temperature alloy laser welding technology adopted in the present invention can greatly reduce welding spatter, does not require vacuum, does not require preheating before welding, heat treatment and slow cooling after welding, and can achieve welding in a conventional air environment, with low welding cost and high efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the concept, specific structure and technical effects of the present invention will be further described below in conjunction with the accompanying drawings to fully understand the purpose, features and effects of the present invention. The purpose of providing these descriptions is only to help explain the present invention and should not be used to limit the scope of the claims of the present invention.
[0025] Figure 1 A schematic diagram of the process developed for the present invention;
[0026] Figure 2 It is a schematic diagram of a common process not of the present invention;
[0027] Figure 3 (a) shows the liquefaction crack in the laser heat affected zone when the laser reciprocating motion frequency is 250 Hz; (b) shows the liquefaction crack in the laser heat affected zone when the laser reciprocating motion frequency is 300 Hz.
[0028] Figure 4 It is a liquefaction crack of the nickel-based high-temperature alloy laser welding head not according to the present invention. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, the accompanying drawings are schematic diagrams, so the device and apparatus of the present invention are not limited by the size or ratio of the schematic diagrams.
[0030] It should be noted that in the claims and description of this patent, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply. There is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "including one" do not exclude the presence of other identical elements in the process, method, article or device including the elements.
[0031] Example 1
[0032] Figure 1 The figure shows the specific implementation process of the method of the present invention, 11 and 12 are high temperature alloy substrates, 2 is a laser beam, 3 is a weld, 4 is molten metal, 5 is a region to be welded, 6 is a reciprocating motion trajectory of the embodiment, 7 is a welding direction arrow, and 8 is a laser reciprocating motion direction arrow. The specific implementation process of the method of the present invention includes the following steps:
[0033] (a) First, the welding area (end face and upper surface) of a pair of nickel-based high-temperature alloy test plates (plate thickness 4 mm) is polished and cleaned. The high-temperature alloy test plates are spliced (butted) after melting spot welding (such as laser welding, GTAW welding), and the misalignment and gap are less than 2% of the plate thickness.
[0034] (b) Further, a fiber laser is used as a laser emitting device. The spot diameter of the laser beam 2 is adjusted to 0.4 mm, and laser welding parameters such as laser beam power, welding speed, laser moving trajectory, laser vertical moving amplitude, and laser reciprocating motion frequency are set to ensure that the weld is fully melted and the depth of the single weld is ≥ 4 mm.
[0035] (c) Further, the laser beam 2 radiates and heats the surfaces of the high-temperature alloys 11 and 12, and under the heating effect of sufficiently high power density, the high-temperature alloys 11 and 12 evaporate and melt to form molten metal 4, and at the same time, the laser beam reciprocates in a straight line perpendicular to the welding direction during the welding process ( Figure 1 6). The laser beam moves toward the area to be welded 5 at a certain speed, and the molten metal 4 cools and solidifies to form a weld 3 until the welding is completed.
[0036] The preferred laser power in this embodiment is 6500W;
[0037] The preferred laser welding speed in this embodiment is 2.3 m / min;
[0038] In this embodiment, the laser reciprocating frequency is preferably 250 Hz;
[0039] In this embodiment, the preferred vertical movement amplitude of the laser is 1.5 mm.
[0040] The butt weld depth is ≧4 mm, and the laser welded joint in this embodiment is fully penetrated, that is, the joint penetration is 4 mm.
[0041] Example 2
[0042] The preferred laser power in this embodiment is 6700W;
[0043] The preferred laser welding speed in this embodiment is 2.1 m / min;
[0044] In this embodiment, the laser reciprocating frequency is preferably 300 Hz;
[0045] In this embodiment, the preferred vertical movement amplitude of the laser is 2.0 mm;
[0046] The rest is consistent with Example 1.
[0047] Figure 3 The figure shows the liquefaction cracks (in the box) in the heat-affected zone of the nickel-based high-temperature alloy laser welding of this embodiment. Figure 3 (a) shows the liquefaction crack in the laser heat affected zone when the laser reciprocating frequency is 250 Hz. Figure 3 (b) is the liquefaction crack in the laser heat affected zone when the laser reciprocating motion frequency is 300 Hz. As can be seen from the figure, there are only a few liquefaction cracks in the heat affected zone.
[0048] Comparative Example
[0049] The liquefaction cracks on 8 cross sections of the high-temperature alloy laser welded joint were observed and counted. The total crack length of the liquefaction of the nickel-based high-temperature alloy laser weld of the technology of the present invention is reduced by 75% (frequency: 250Hz) and 70% (frequency: 300Hz) respectively compared with the technology of the non-invention, as shown in Table 1. It can also be seen from the table that compared with the traditional laser welding technology, the width of the welding heat-affected zone temperature 1280℃~1380℃ area of the method of the present embodiment invention has a significant decrease, that is, a decrease of 20% (250Hz) and 11% (300Hz) respectively. In this embodiment, due to the reduction of the reciprocating motion of the laser beam in the high-temperature alloy welding, the residence time of the 1280℃~1380℃ temperature area of the heat-affected zone per unit time is reduced, thereby reducing the degree of grain boundary liquefaction in the heat-affected zone and reducing the liquefaction cracks in the heat-affected zone of the high-temperature alloy laser welding.
[0050] Table 1 Statistics of liquefaction crack length of nickel-based high-temperature alloy laser welding joint
[0051]
[0052] Figure 2 The figure shows laser welding of nickel-based high-temperature alloy without using the method of the present invention, wherein the laser power value, welding speed value and defocus value are the same as those in Examples 1 and 2.
[0053] Figure 4 The figure shows the liquefaction cracks (in the square frame) of the laser welding of the nickel-based high-temperature alloy without using the present invention. As can be seen from the figure, there are a large number of liquefaction cracks in the heat-affected zone.
[0054] It can be seen from the method of the present invention and the comparative examples that the method of the present invention can significantly reduce the liquefaction cracks in the heat-affected zone of laser welding of nickel-based high-temperature alloys through single-pass laser welding. When using different laser reciprocating motion frequencies, the method of the present invention can still significantly reduce the liquefaction cracks in the laser welding of nickel-based high-temperature alloys.
[0055] Although the present invention has been shown as above with preferred embodiments, it is not intended to limit the present invention. Any equivalent changes or substitutions made by any person skilled in the art without departing from the spirit and scope of the present invention are within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be subject to the scope defined by the appended claims of the present application.
Claims
1. A method for controlling liquefaction cracks in the heat-affected zone of laser welding of nickel-based high-temperature alloys, comprising the following steps: Providing a pair of nickel-based high-temperature alloys, splicing the end faces of the high-temperature alloys, and forming a splicing seam into a welding area; The laser welding light source provides at least one laser beam, which continuously irradiates the upper surface of the joint to form molten metal, and advances the laser beam along the upper surface of the joint to melt and solidify the high-temperature alloy in the laser beam contact area to form a weld, thereby completing laser single-sided welding and double-sided forming in one go; the direction in which the laser beam advances along the joint is the welding direction, and is characterized in that while the laser beam advances along the welding direction, it reciprocates in a straight line perpendicular to the welding direction to perform laser deep penetration welding, achieving weld penetration and a single-pass weld depth of ≧4mm, thereby suppressing the generation of liquefaction cracks in the temperature region of 1280°C to 1380°C in the heat-affected zone of laser deep penetration welding of nickel-based high-temperature alloys.
2. The method for controlling liquefaction cracks in the heat-affected zone of laser welding of nickel-based high-temperature alloy according to claim 1, characterized in that: The optical power of the laser welding light source is ≥6000W, the welding speed is ≥2.1m / min, and the vertical movement amplitude of the laser beam is 1.5-2.5mm.
3. The method for controlling liquefaction cracks in heat-affected zone of laser welding of nickel-based high-temperature alloy according to claim 1, characterized in that: The reciprocating frequency of the laser beam is ≧250 Hz, the focal spot diameter of the laser beam is 0.4 mm to 0.6 mm, and the inclination angle of the laser beam is 0° to 5°.
4. The method for controlling liquefaction cracks in heat-affected zone of laser welding of nickel-based high-temperature alloy according to claim 1, characterized in that: The high temperature alloy is a solid solution strengthened nickel-based high temperature alloy.