Copper material CMP method for TGV bonding and semiconductor wafer

By using the copper material CMP method of different polishing liquids on the hard polishing pad, combined with real-time film thickness detection and optical laser endpoint detection, the problem of poor adhesion of glass surface smoothness and metal layer is solved, and efficient TGV bonding is achieved, ensuring that High quality and stability of wafer surface.

CN119057664APending Publication Date: 2024-12-03BEIJING SEMICORE MICROELECTRONICS EQUIPMENT CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411237533.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In advanced packaging technology, poor adhesion of glass surface smoothness and common metals lead to layering between the glass substrate and the metal layer, causing the metal layer to curl or fall off, damage the glass, and the existing TGV three-dimensional interconnection technology is difficult to be effective Solve these problems.

Method used

The copper material CMP method is adopted in non-grinding wheel method. The two types of polishing liquids are polished separately on the hard polishing pad. Combined with real-time film thickness detection and optical laser endpoint detection, the removal rate and thickness of the copper layer are controlled to avoid blockage of Cu chips. Ensure surface quality.

Benefits of technology

A better bonding interface state with wafer surface inhomogeneity less than 5% and surface roughness less than 0.5nm is achieved, which improves efficiency and surface quality and avoids curling and falling off of the metal layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057664A_ABST
    Figure CN119057664A_ABST
Patent Text Reader

Abstract

The invention is suitable for the technical field of semiconductor material processing, and provides a copper material CMP method for TGV bonding and a semiconductor wafer, and the method comprises the steps: removing a to-be-removed copper layer of the wafer on a first polishing disc, and controlling the residual thickness of the to-be-removed copper layer to be within a preset thickness range; the removal rate of the to-be-removed copper layer on the first polishing disc is 3-5 microns / min, and the preset thickness range is 2-3 microns; removing the residual to-be-removed copper layer on the second polishing disc until the lower layer material of the to-be-removed copper layer is exposed; the rate of removing the remaining copper layer to be removed on the second polishing disc is # imgabs0 #, and the abrasive diameter of the polishing solution selected on the first polishing disc is larger than that of the polishing solution selected on the second polishing disc. According to the invention, a better bonding interface state can be obtained, so that the surface non-uniformity of the wafer is 1t; 5%, the surface roughness of the wafer is lt; the wavelength is 0.5 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of semiconductor material processing, and in particular, relates to a copper material CMP method for TGV bonding and a semiconductor wafer. Background Art

[0002] The technology iteration of semiconductor integrated circuits has been developing along Moore's Law until now, and has almost reached the physical limit. The iteration speed of Moore's Law has slowed down. From the perspective of system application, the overall performance improvement depends on advanced packaging technology. The industry believes that system heterogeneous integration is one of the key technologies to improve system performance and reduce costs, and it needs to rely on advanced packaging technology.

[0003] Advanced packaging technology is a general term for a variety of packaging technology platforms. Advanced packaging mainly refers to flip chip, wafer level packaging (WLP), 2.5D packaging (Interposer), 3D packaging (TSV), etc. SiP (System in Package), WLP, and 2.5D / 3D are the three major development focuses.

[0004] In advanced packaging technology, glass is a possible alternative to silicon-based adapters, and through glass via (TGV) 3D interconnection technology is becoming a current research hotspot due to its many advantages. The main difficulty in the development of TGV 3D interconnection technology is that although existing methods can achieve TGV, some methods will damage the glass, resulting in an uneven surface; compared with silicon materials, the glass surface is smooth and has poor adhesion to common metals (such as Cu), which can easily cause delamination between the glass substrate and the metal layer, resulting in curling of the metal layer, or even falling off. Summary of the invention

[0005] To overcome the problems existing in the related art, the embodiments of the present application provide a copper material CMP method and a semiconductor wafer for TGV bonding, which can obtain a better bonding interface state, so that the surface unevenness of the wafer is <5% and the surface roughness of the wafer is <0.5nm.

[0006] This application is implemented through the following technical solutions:

[0007] In a first aspect, an embodiment of the present application provides a copper material CMP method for TGV bonding, comprising:

[0008] The copper layer to be removed from the wafer is removed on the first polishing disk, and the remaining thickness of the copper layer to be removed is controlled within a preset thickness range; wherein the rate of removing the copper layer to be removed on the first polishing disk is 3 to 5 μm / min, and the preset thickness range is 2 to 3 μm;

[0009] The remaining copper layer to be removed is removed on the second polishing plate until the underlying material of the copper layer to be removed is exposed; wherein the rate of removing the remaining copper layer to be removed on the second polishing plate is The abrasive diameter of the polishing liquid selected on the first polishing disc is greater than the abrasive diameter of the polishing liquid selected on the second polishing disc; both the first polishing disc and the second polishing disc use hard polishing pads.

[0010] In one embodiment, the hardness of the hard polishing pad is 65-80.

[0011] In one embodiment, the diameter of the abrasive selected for the polishing liquid on the first polishing disk is 150-200 nm.

[0012] In one embodiment, the abrasive diameter of the polishing liquid selected for the second polishing disc is 50-150 nm.

[0013] In one embodiment, controlling the remaining thickness of the copper layer to be removed to be within a preset thickness range includes:

[0014] Real-time film thickness detection and real-time back pressure adjustment technology are used to control the remaining thickness of the copper layer to be removed within a preset thickness range.

[0015] In one embodiment, removing the remaining copper layer to be removed on the second polishing plate until the underlying material of the copper layer is exposed comprises:

[0016] The remaining copper layer to be removed is removed on the second polishing disc, and the removal thickness of the remaining copper layer to be removed is controlled by optical laser endpoint detection until the underlying material of the copper layer is exposed.

[0017] In one embodiment, the difference between the upper surface of the copper layer after the remaining copper layer to be removed is removed on the second polishing disk and the upper surface of the lower layer material of the copper layer to be removed is less than 5 nm.

[0018] In one embodiment, the thickness of the copper layer to be removed is 15-30 μm.

[0019] In one embodiment, the underlying material of the copper layer is titanium or oxide.

[0020] In a second aspect, an embodiment of the present application provides a semiconductor wafer obtained by applying the copper material CMP method for TGV bonding as in the first aspect.

[0021] Compared with the related art, the embodiments of the present application have the following beneficial effects:

[0022] In the embodiment of the present application, a non-grinding wheel method is adopted, a polishing liquid and a polishing pad are used, and two polishing liquids with different copper removal rates are used to polish on the polishing pad respectively, so as to solve the problem of Cu chip clogging, thereby achieving the effect of improving efficiency and controlling surface quality, and being able to obtain a better bonding interface state, so that the surface non-uniformity of the wafer is <5%, and the surface roughness of the wafer is <0.5nm.

[0023] The beneficial effects of the second aspect mentioned above refer to the beneficial effects of the copper material CMP method for TGV bonding in the first aspect, which will not be described in detail here.

[0024] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present specification. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or related technical descriptions will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0026] Figure 1 It is a schematic flow chart of a copper material CMP method for TGV bonding provided in one embodiment of the present application;

[0027] Figure 2 is a schematic cross-sectional view of a wafer before polishing provided in an embodiment of the present application;

[0028] Figure 3 is a schematic cross-sectional view of a wafer polished on a first polishing disk according to an embodiment of the present application;

[0029] Figure 4 is a schematic cross-sectional view of a wafer polished on a second polishing plate provided in an embodiment of the present application;

[0030] Figure 5 This is a schematic diagram of two concave wafers before bonding provided by an embodiment of the present application;

[0031] Figure 6 This is a schematic diagram of two protruding wafers before bonding provided in one embodiment of the present application. DETAILED DESCRIPTION

[0032] In the following description, specific details such as specific system structures and technologies are provided for the purpose of illustration rather than limitation, so as to provide a thorough understanding of the embodiments of the present application. However, it should be clear to those skilled in the art that the present application may also be implemented in other embodiments without these specific details. In other cases, detailed descriptions of well-known systems, devices, circuits, and semiconductor wafers are omitted to prevent unnecessary details from obstructing the description of the present application.

[0033] It should be understood that when used in the present specification and the appended claims, the term "comprising" indicates the presence of described features, wholes, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, wholes, steps, operations, elements, components and / or combinations thereof.

[0034] It should also be understood that the term “and / or” used in the specification and appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.

[0035] In addition, in the description of the present application specification and the appended claims, the terms "first", "second", "third", etc. are only used to distinguish the descriptions and cannot be understood as indicating or implying relative importance.

[0036] References to "one embodiment" or "some embodiments" etc. described in the specification of this application mean that one or more embodiments of the present application include specific features, structures or characteristics described in conjunction with the embodiment. Therefore, the statements "in one embodiment", "in some embodiments", "in some other embodiments", "in some other embodiments", etc. that appear in different places in this specification do not necessarily refer to the same embodiment, but mean "one or more but not all embodiments", unless otherwise specifically emphasized in other ways. The terms "including", "comprising", "having" and their variations all mean "including but not limited to", unless otherwise specifically emphasized in other ways.

[0037] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present application will be clearly and completely described below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0038] Compared with silicon substrates, the advantages of TGV are mainly reflected in its excellent high-frequency electrical properties. Glass material is an insulator material with a dielectric constant of only about 1 / 3 of that of silicon material, and a loss factor 2 to 3 orders of magnitude lower than that of silicon material. The substrate loss and parasitic effects are reduced, ensuring the integrity of the transmission signal, and large-size ultra-thin glass substrates are easy to obtain.

[0039] However, as mentioned in the background technology, the glass surface is smooth and has poor adhesion to the commonly used metal Cu. When the thick Cu film is processed by the grinding and CMP process, the diamond on the surface of the grinding wheel will soon be blocked by Cu chips due to the soft Cu material, which will reduce the removal efficiency of the Cu surface. Sometimes, the Cu film will be lifted due to the high mechanical force of the grinding wheel. TGV chemical mechanical polishing (CMP) has two applications, one is blind via and the other is through via. The materials of both vias are copper, but the Cu in the blind via penetrates the substrate, while the Cu in the through via does not penetrate the substrate. The CMP solution of this application is mainly aimed at blind via TGV technology. Through precise polishing liquid selection and equipment process parameter setting, in conjunction with various detection systems and endpoint control functions, the Cu CMP requirements can be met, the phenomenon of Cu chip clogging and Cu film being lifted can be avoided, and the conditions for direct bonding after CMP can be met.

[0040] Figure 1 1 is a schematic flow chart of a copper material CMP method for TGV bonding provided in one embodiment of the present application. Figure 2 is a schematic diagram of the wafer cross section before polishing. Figure 3 is a schematic diagram of the cross section of a wafer polished on the first polishing plate. Figure 4 is a schematic diagram of the cross section of the wafer polished on the second polishing plate; refer to Figures 1 to 4 The details of the copper material CMP method for TGV bonding are as follows:

[0041] Step 101, removing the copper layer to be removed from the wafer on a first polishing disk, and controlling the remaining thickness of the copper layer to be removed to be within a preset thickness range; wherein the removal rate of the copper layer to be removed on the first polishing disk is 3 to 5 μm / min, and the preset thickness range is 2 to 3 μm.

[0042] Exemplarily, a thicker copper layer is removed in bulk on a first polishing pad, such as Figure 2 to Figure 3 shown.

[0043] Step 102, removing the remaining copper layer to be removed on the second polishing plate until the underlying material of the copper layer to be removed is exposed; wherein the rate of removing the remaining copper layer to be removed on the second polishing plate is The abrasive diameter of the polishing liquid selected on the first polishing disc is greater than the abrasive diameter of the polishing liquid selected on the second polishing disc; both the first polishing disc and the second polishing disc use hard polishing pads.

[0044] Exemplarily, the thickness of the copper layer removed on the second polishing plate is less than the thickness of the copper layer removed on the first polishing plate, and a small amount of the copper layer is removed on the second polishing plate, such as Figure 3 to Figure 4 As shown. The lower layer material of the copper layer is generally oxide, and the lower layer here means that compared with the copper layer before polishing, a part of the actual copper layer is between the lower layer materials. The remaining copper layer to be removed refers to the upper surface of the lower layer material to the upper surface of the copper layer.

[0045] This embodiment adopts a non-grinding wheel method, uses two polishing discs for segmented control, and a polishing liquid plus a polishing pad method. The abrasive diameter of the polishing liquid selected on the first polishing disc is larger than the abrasive diameter of the polishing liquid selected on the second polishing disc. Two high and low polishing liquids with different copper removal rates are used to polish on the polishing pad respectively. The removal rate of the first polishing disc is greater than the removal rate of the second polishing disc. Therefore, when the rate is slower and close to the final thickness control, it is necessary to control the polishing parameters more finely to avoid over-polishing or copper chips residue. Then, by setting various specific polishing parameters, the problem of Cu chip clogging is further solved, thereby achieving the effect of improving efficiency and controlling surface quality, and being able to obtain a better bonding interface state.

[0046] In one embodiment, the hardness of the hard polishing pad is 65-80, in Shore A hardness.

[0047] In one embodiment, the abrasive diameter of the polishing liquid selected on the first polishing disc can be 150-200 nm. The abrasive in the selected diameter range is relatively large, and can generate a strong cutting force during the polishing process, effectively remove the rough layer and large unevenness on the surface of the material, and provide a good foundation for the subsequent polishing steps. If the abrasive diameter is too large, the abrasive particles may not be able to effectively remove the rough layer and deep scratches on the surface of the material, and may also generate unnecessary surface roughness during the polishing process.

[0048] The abrasive diameter of the polishing liquid selected on the second polishing disc can be 50 to 150 nm. The abrasive in the selected diameter range can penetrate deeper into the tiny pits and scratches on the surface of the material, perform fine grinding, and improve the surface finish and smoothness.

[0049] The polishing liquid provides more liquid flow channels to reduce the accumulation of copper chips on the surface of the polishing pad. Of course, the appropriate pH value can also be adjusted to optimize the polishing chemical reaction, reduce the accumulation of copper chips, and promote the dissolution or dispersion of copper chips.

[0050] In one embodiment, controlling the remaining thickness of the copper layer to be removed to be within a preset thickness range includes:

[0051] Real-time film thickness detection and real-time back pressure adjustment technology are used to control the remaining thickness of the copper layer to be removed within a preset thickness range.

[0052] Real-time film thickness detection technology is mainly used to measure the thickness of films, coatings or other thin material layers in real time and accurately during the manufacturing or processing process. Common real-time film thickness detection technologies, such as optical methods, use the optical properties of thin films to measure the thickness and refractive index of thin films through the state changes during reflection or transmission of polarized light, and can measure films from a few nanometers to a few microns. Back pressure adjustment technology is used to control the pressure of the polishing liquid while measuring the remaining thickness of the copper layer to be removed within a preset thickness range. Real-time film thickness detection and real-time back pressure adjustment technology to ensure the uniformity and quality of the film can ensure that the uniformity of the Cu film thickness and the remaining copper layer to be removed after the first polishing disk is completed is controllable and within the specified range, and the non-uniformity is <5%.

[0053] In one embodiment, removing the remaining copper layer to be removed on the second polishing plate until the underlying material of the copper layer is exposed comprises:

[0054] The remaining copper layer to be removed is removed on the second polishing disk, and the removal thickness of the remaining copper layer to be removed is controlled by optical laser endpoint detection (Lazer EPD) until the underlying material of the copper layer is exposed.

[0055] Optical Lazer EPD is an advanced online monitoring technology that uses a laser beam to illuminate the surface of the material being polished, and detects the changes in the optical signal generated by the interaction between the laser and the material surface to determine the status and end point of the polishing process in real time. This technology can accurately measure small changes in material thickness and automatically stop the polishing process when the preset remaining thickness is reached, ensuring polishing accuracy and consistency.

[0056] The system emits a beam of laser, which passes through a specific optical system and irradiates the surface of the polished Cu material at a certain angle and power. After the laser interacts with the material surface, it will generate light signals such as reflection, scattering or absorption. These light signals are received by the photodetector in the system and converted into electrical signals. After amplification, filtering and other processing, the received electrical signals are sent to the computer for analysis. The computer calculates the change in the thickness of Cu in real time according to the preset algorithm and model, and compares it with the target thickness. When the calculated material thickness approaches or reaches the preset remaining thickness, the system automatically adjusts the polishing parameters (such as polishing pressure, rotation speed, etc.) through a feedback mechanism to maintain a stable removal rate, and stops the polishing process when the end point is reached.

[0057] The size of the depression or protrusion of the surface Cu is controlled by combining the polishing liquid and time, thereby controlling the total CMP time of Cu on the second polishing disk. The difference between the upper surface of the copper layer after the remaining copper layer to be removed on the second polishing disk and the upper surface of the lower material of the copper layer to be removed is less than 5nm, thereby achieving the Cu smoothness and depression (or protrusion) <5nm, and the Cu surface and the lower material (tungsten / Oxide) Ra <0.5nm.

[0058] This embodiment uses the optical Lazer EPD to assist in controlling the remaining thickness of the copper layer to be removed, and then controls the total CMP time of Cu on the second polishing plate, which can uniformly control the height difference between the Cu layer on the wafer surface and the underlying material to be less than 5nm, and the roughness of the Cu surface and the underlying material is <0.5nm. There are two forms of height difference between the copper layer and the underlying material: concave and convex, such as Figure 5 and Figure 6 As shown, the height difference between the Cu layer on the wafer surface and the underlying material is uniformly controlled so that the height difference between materials of different qualities is uniform. Combined with the above-mentioned good roughness, an ideal surface state for wafer-level bonding is achieved.

[0059] In one embodiment, the present application performs polishing for a thick Cu film electroplating, and the thickness of the copper layer to be removed is 15-30 μm, and the copper layer to be removed refers to the material from the upper surface of the lower material to the upper surface of the copper layer. Since the surface roughness of the copper layer before polishing is relatively large, the thickness deviation of the copper layer to be removed is generally 3-5 μm.

[0060] The width of the copper layer to be removed is Figure 2 The width between the two portions of the underlying material shown ranges from 12 to 20 μm.

[0061] In one embodiment, the underlying material of the copper layer is titanium or oxide.

[0062] The copper material CMP method for TGV bonding proposed in the present invention achieves a lower surface roughness of <0.5nm and a smaller height difference between PI and the underlying material of <5nm through the matching of consumables and the setting of process parameters, so as to obtain a better bonding interface state, a greater bonding strength, a more stable and reliable device, and a faster data transmission speed and lower power consumption of the prepared chip.

[0063] An embodiment of the present application provides a semiconductor wafer obtained by applying the copper material CMP method for TGV bonding as in the above embodiment.

[0064] It should be understood that the execution order of the above processes should be determined by their functions and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0065] It should be noted that the information interaction, execution process and other contents between the above-mentioned devices are based on the same concept as the method embodiment of the present application. Their specific functions and technical effects can be found in the method embodiment part and will not be repeated here.

[0066] The technicians in the relevant field can clearly understand that for the convenience and simplicity of description, only the division of the above-mentioned functional units and modules is used as an example for illustration. In practical applications, the above-mentioned function allocation can be completed by different functional units and modules as needed, that is, the internal structure of the device can be divided into different functional units or modules to complete all or part of the functions described above. The functional units and modules in the embodiment can be integrated in a processing unit, or each unit can exist physically separately, or two or more units can be integrated in one unit. The above-mentioned integrated unit can be implemented in the form of hardware or in the form of software functional units. In addition, the specific names of the functional units and modules are only for the convenience of distinguishing each other, and are not used to limit the scope of protection of this application. The specific working process of the units and modules in the above-mentioned system can refer to the corresponding process in the aforementioned method embodiment, which will not be repeated here.

[0067] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

Claims

1. A copper material CMP method for TGV bonding, characterized in that: include: The copper layer to be removed from the wafer is removed on a first polishing disk, and the remaining thickness of the copper layer to be removed is controlled to be within a preset thickness range; wherein the rate of removing the copper layer to be removed on the first polishing disk is 3 to 5 μm / min, and the preset thickness range is 2 to 3 μm; The remaining copper layer to be removed is removed on the second polishing disc until the underlying material of the copper layer to be removed is exposed; wherein the rate of removing the remaining copper layer to be removed on the second polishing disc is The abrasive diameter of the polishing liquid selected for the first polishing disc is greater than the abrasive diameter of the polishing liquid selected for the second polishing disc; both the first polishing disc and the second polishing disc use hard polishing pads.

2. The copper material CMP method for TGV bonding according to claim 1, characterized in that: The hardness of the hard polishing pad is 65-80.

3. The copper material CMP method for TGV bonding according to claim 1, characterized in that: The abrasive diameter of the polishing liquid selected for the first polishing disc is 150-200 nm.

4. The copper material CMP method for TGV bonding according to claim 1, characterized in that; The abrasive diameter of the polishing liquid selected for the second polishing disc is 50-150 nm.

5. The copper material CMP method for TGV bonding according to claim 1, characterized in that: The controlling the remaining thickness of the copper layer to be removed to be within a preset thickness range comprises: The film thickness real-time detection and real-time back pressure adjustment technology is used to control the remaining thickness of the copper layer to be removed to be within a preset thickness range.

6. The copper material CMP method for TGV bonding according to claim 1, characterized in that: The step of removing the remaining copper layer to be removed on the second polishing plate until the underlying material of the copper layer is exposed comprises: The remaining copper layer to be removed is removed on the second polishing disk, and the removal thickness of the remaining copper layer to be removed is controlled by optical laser endpoint detection until the underlying material of the copper layer is exposed.

7. The copper material CMP method for TGV bonding according to claim 1, characterized in that: The difference between the upper surface of the copper layer after the remaining copper layer to be removed is removed on the second polishing disk and the upper surface of the lower layer material of the copper layer to be removed is less than 5 nm.

8. The copper material CMP method for TGV bonding according to claim 1, characterized in that: The thickness of the copper layer to be removed is 15-30 μm.

9. The copper material CMP method for TGV bonding according to claim 1, characterized in that: The lower layer material of the copper layer is titanium or oxide.

10. A semiconductor wafer, characterized in that: The method is obtained by using the copper material CMP method for TGV bonding as claimed in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Chemical mechanical polishing method capable of enhancing polishing performance

    CN101376232A

  • Chemical-mechanical polishing method in copper interconnection process

    CN101992421A

  • Chemical-mechanical polishing method

    CN108257863A

  • Polishing composition and method for polishing a conductive material

    CN1842577A

  • Two-stage chemical-mechanical polishing method

    JP3099002B1