Cable joint mold, method for preparing polypropylene layer and polypropylene layer
Through the thermoplastic molding technology of cable joint molds and polypropylene materials, a high-performance polypropylene layer is formed, which solves the problem of weak temperature performance and difficulty in recycling of crosslinked polyethylene materials during long-term operation, and improves the safety, stability and environmental protection of the cable characteristic.
Patent Information
- Application Number
- CN202410957711.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-12-03
AI Technical Summary
As a high-voltage insulating material, crosslinked polyethylene has problems such as weak temperature performance and significant accumulation of space charge during long-term operation, and is difficult to recycle and reuse, affecting the safety and environmental protection characteristics of cable operation.
The cable joint mold and polypropylene material are used to form a polypropylene layer through thermoplastic molding, and the mold sensor is used to control the temperature and pressure to form a high-performance polypropylene insulation or semiconductor shielding layer to meet the mechanical and electrical performance requirements of the cable.
It improves the safety, stability and performance at the middle joint of polypropylene cable, meets the voltage level requirements of the cable, reduces carbon emissions throughout the life cycle of the cable, and improves the mechanical and electrical insulation performance of the cable.
Smart Images

Figure CN119058031A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of power cables, and in particular, to a cable joint mold, a method for preparing a polypropylene layer, and a polypropylene layer. Background Art
[0002] With the rapid development of the power system, the scope of the power grid has also expanded rapidly. In power cables, research on the mechanical and electrical insulation properties of cross-linked polyethylene insulated power cables has also made certain progress. However, as a high-voltage insulating material, cross-linked polyethylene has problems such as low long-term operating temperature, weak high-temperature electrical properties, and significant space charge accumulation. In addition, during the cross-linking process of polyethylene, it is difficult to avoid the residue of cross-linking by-products in the insulating material. The cross-linking by-products further aggravate the accumulation of space charge during the operation of the cable, causing insulation aging or even breakdown, affecting the operation of the cable. In addition, cross-linked polyethylene is a thermosetting material, which cannot be recycled and reused, and does not have green and environmentally friendly characteristics. Therefore, further research on thermoplastic recyclable power cable insulation materials is still of great significance and practical need. Summary of the invention
[0003] In a first aspect of the present application, the present application proposes a cable connector mold, comprising: a mold body, the mold body is a through cylinder, the interior of the cylinder has a accommodating space, and the accommodating space is used to accommodate a semi-molded cable; a fixing part, the fixing part is arranged at both ends of the mold body to fix the semi-molded cable located in the cylinder; a first processing port, the first processing port is located between adjacent fixing parts, and the first processing port is connected to the accommodating space; a second processing port, the second processing port is located between adjacent fixing parts, and the second processing port is connected to the accommodating space.
[0004] The fixing part fixes the semi-molded cable to be processed with the cable joint mold. The part of the semi-molded cable to be jointed is placed in the accommodation space inside the mold body. The cable joint mold is connected to the extruder through one of the first processing port and the second processing port. Through the connected processing port, the material in the extruder can be injected into the accommodation space of the mold body, and the material flows and spreads in the accommodation space by utilizing the ductility of the material. The gas and redundant material in the mold body can be discharged through another processing port that is not connected to the extruder.
[0005] According to a specific embodiment of the present application, a sensor is further provided on the mold body, wherein the sensor includes at least one of a temperature sensor, a pressure sensor, and a temperature and pressure sensor.
[0006] The sensor arranged on the mold body can detect the pressure and temperature changes of the material entering the containing space of the mold body, so as to control the adding, molding and cooling processes of the material.
[0007] In the second aspect of the present application, the present application proposes a method for preparing a polypropylene layer using the cable joint mold, comprising: loading the middle joint of a semi-molded cable into a mold body; introducing nitrogen into the mold body through a first processing port or a second processing port to exhaust the air; injecting a polypropylene material into the mold body through the first processing port or the second processing port to form a polypropylene layer on the outer surface of the middle joint of the semi-molded cable.
[0008] By utilizing the thermoplasticity of polypropylene, polypropylene is melted at the middle joint of the semi-molded cable to form a polypropylene layer to wrap the middle joint of the semi-molded cable. The thickness and shape of the polypropylene layer formed by the coating are controlled by the cable joint mold to improve the safety and stability of the middle joint of the polypropylene cable.
[0009] According to a specific embodiment of the present application, the polypropylene layer is formed at a temperature of 160° C.-250° C., and at a pressure of 0.1 MPa-30 MPa.
[0010] The polypropylene pellets are injected into the cable joint mold by the extruder, and the temperature and pressure of the extruder head are adjusted so that the polypropylene reaches the aforementioned temperature and pressure range in the cable joint mold. Within the aforementioned stable and pressure range, the polypropylene can fully spread and tightly wrap the middle joint of the semi-molded cable to form a polypropylene layer.
[0011] According to a specific embodiment of the present application, the polypropylene layer is a polypropylene insulating layer, wherein the volume resistivity of the polypropylene material forming the polypropylene insulating layer is 10 11 Ω·m-10 17 Ω·m.
[0012] In power cables, polypropylene can be used as an insulating layer material. When the volume resistivity of the insulating layer polypropylene material is within the above range, it can meet the voltage level requirements of the cable.
[0013] According to a specific embodiment of the present application, the polypropylene material includes a polypropylene copolymer, and further includes: at least one of an elastomer and nanoparticles.
[0014] The material properties of polypropylene materials are adjusted through copolymerization, doping, etc., so that the mechanical properties, electrical insulation properties, etc. of polypropylene materials meet the requirements for use as the insulation layer of power cables.
[0015] According to a specific embodiment of the present application, the polypropylene layer is a polypropylene semi-conductive shielding layer, wherein the volume resistivity of the polypropylene material forming the polypropylene semi-conductive shielding layer is less than 500Ω·m.
[0016] In power cables, polypropylene can be used as a semi-conductive shielding layer material. When the polypropylene material is within the aforementioned volume resistivity range, the semi-conductive shielding layer formed by it can confine the electromagnetic field formed by the current in the cable within the cable.
[0017] According to a specific embodiment of the present application, the polypropylene material includes a polypropylene copolymer, a conductive filler and an additive.
[0018] A semi-conductive composite is made by adding conductive fillers and various additives to polypropylene through modification, so that its volume resistivity at room temperature meets the requirements for a semi-conductive shielding layer of a power cable.
[0019] According to a specific embodiment of the present application, the method further comprises: performing a cooling treatment on the polypropylene layer, wherein the cooling treatment comprises natural cooling or external contact mold cooling.
[0020] The properties of the formed polypropylene layer can be further controlled by cooling the polypropylene after molding.
[0021] In a third aspect of the present application, the present application proposes a polypropylene layer. The polypropylene layer is prepared by the above-mentioned method of preparing a polypropylene layer by using a cable connector mold.
[0022] The polypropylene layer proposed in this application has better insulation and shielding properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0024] Figure 1 This is a schematic structural diagram of a cable connector mold according to an embodiment of the present application.
[0025] Description of reference numerals:
[0026] The mold body 10 ; the accommodating space 20 ; the fixing member 30 ; the first processing opening 40 ; the second processing opening 50 ; and the sensor 60 . DETAILED DESCRIPTION
[0027] The embodiments of the present application are described in detail below. Examples of the embodiments are shown in the drawings, but unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of actually identical structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0028] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by technicians in the technical field to which this application belongs; the terms used in this application are only for the purpose of describing specific embodiments and are not intended to limit this application; unless otherwise specified, the numerical values of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the embodiments of this application).
[0029] The terms "including" and "having" in the specification and claims of the present application and any modifications thereof are open expressions, that is, including the contents specified in the present application but not excluding other contents.
[0030] In the description of this application, regardless of whether the words "about" or "approximately" are used, all the numbers disclosed herein are approximate values. The value of each number may differ by less than 10% or a reasonable difference considered by those skilled in the art, such as 1%, 2%, 3%, 4% or 5%.
[0031] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0032] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0033] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0034] Power cables using cross-linked polyethylene as insulating materials can operate for a long time at 90°C. Power cables using thermoplastic polypropylene as insulating materials can operate for a long time at 110°C, which can increase the transmission capacity of the cable by more than 30% and reduce the carbon emissions of the cable over its entire life cycle by more than 50%, which can bring huge social and economic benefits. The middle joint where two power cables are connected can be coated using a polypropylene tape wrapping process. The wrapping process needs to go through the processes of wrapping, melting, cross-linking, and degassing, which can easily produce gaps and defects, reduce the performance of the formed polypropylene layer, and the performance of the polypropylene material will be reduced during the melting and re-solidification of the polypropylene tape, reducing the overall safety and stability of the cable operation. The cable joint mold proposed in this application and the method for preparing a polypropylene layer using the cable joint mold can improve the above-mentioned process defects, and the performance of the formed polypropylene layer meets the requirements of the power cable.
[0035] In a first aspect of the present application, the present application proposes a cable connector mold, comprising: a mold body 10, the mold body 10 is a through cylinder, the interior of the cylinder has a accommodating space 20, and the accommodating space 20 is used to accommodate a semi-molded cable; a fixing member 30, the fixing member 30 is arranged at both ends of the mold body 10 to fix the semi-molded cable located in the cylinder; a first processing port 40, the first processing port 40 is located between adjacent fixing members 30, and the first processing port 40 is communicated with the accommodating space 20; a second processing port 50, the second processing port 50 is located between adjacent fixing members 30, and the second processing port 50 is communicated with the accommodating space 20.
[0036] After the power cable is laid, the cables need to be connected front and back to form a continuous line, and the connection point is the middle joint. The extrusion die is wrapped around the outside of the middle joint of the semi-molded cable to be processed, and the first processing port 40 is connected to the extruder. After the modified polypropylene pellets that meet the requirements of the wrapping layer are extruded by the extruder, they enter the accommodating space 20 of the cable joint mold in a viscous flow state, and fill the gap between the accommodating space 20 in the cable joint mold and the middle joint of the semi-molded cable. Polypropylene material is a thermoplastic material, and its curing molding does not require the addition of a cross-linking agent, which reduces the introduction of chemical substances. By setting a suitable mold inner diameter and processing conditions, after the cable is connected, the formed polypropylene layer can smoothly transition with the polypropylene layer of the cable itself to form a continuous closed structure.
[0037] According to a specific embodiment of the present application, a sensor 60 is further provided on the mold body 10, wherein the sensor 60 includes at least one of a temperature sensor, a pressure sensor, and a temperature and pressure sensor.
[0038] After the polypropylene material enters the cable joint mold, its physical state will change with the flow distance and time. The sensor 60 arranged on the mold body 10 can provide information such as temperature and pressure in the cable joint mold during the joint processing. Appropriate pressure and temperature conditions are conducive to the moderate expansion and contraction, crystallization and molding of polypropylene to form a polypropylene layer with less voids and defects.
[0039] In a second aspect of the present application, the present application proposes a method for preparing a polypropylene layer using the cable joint mold, comprising:
[0040] S100: Insert the middle joint of the semi-molded cable into the mold body 10
[0041] The polypropylene layer can be used as an insulating layer or a semi-conductive shielding layer in a power cable. When connecting the polypropylene semi-conductive shielding layer at the intermediate joint, the conductor at the intermediate joint is electrically connected by a melting or precipitation process, and is polished and wrapped with a semi-conductive nylon tape. Subsequently, the intermediate joint of the cable wrapped with the semi-conductive nylon tape is placed in the mold body 10, and the polypropylene semi-conductive shielding layer is formed using the aforementioned cable joint mold; when connecting the polypropylene insulation layer of the intermediate joint, the semi-conductive shielding layer of the intermediate joint is polished and smooth, and an interface adhesive is applied as needed. The intermediate joint after the aforementioned treatment is placed in the mold body 10, and the polypropylene insulation layer is formed using the aforementioned cable joint mold. The size of the mold is matched according to the required thickness of the polypropylene layer.
[0042] S200: nitrogen is introduced into the mold body 10 through the first processing port 40 or the second processing port 50 to exhaust air.
[0043] Either the first processing port 40 or the second processing port 50 can be used as a nitrogen inlet, and the other can be used as a gas outlet. The air in the mold is discharged by nitrogen, which reduces the contact between oxygen in the air and the polypropylene material, reduces the probability of adverse side reactions during the molding process of the polypropylene material, and improves the quality of the formed polypropylene layer.
[0044] S300: injecting a polypropylene material into the mold body 10 through the first processing port 40 or the second processing port 50 to form a polypropylene layer on the outer surface of the middle joint of the semi-molded cable
[0045] Either the first processing port 40 or the second processing port 50 can be used as an injection inlet for the polypropylene material, and the other can be used as an outlet for the gas and redundant materials in the mold body 10. When adding the polypropylene material, the sensor 60 on the mold body 10 can be used to continuously monitor the temperature and pressure in the mold body 10. When the pressure value reaches the preset value, the extruder head is evacuated, and the first processing port 40 and the second processing port 50 are closed to maintain the cavity pressure in the joint module. Opening or closing the processing port at the appropriate time can control the changes in temperature and pressure in the mold body 10 to be relatively stable, which is conducive to forming a polypropylene layer with uniform thickness and high consistency of component distribution. The mold is used to define the morphology of the polypropylene layer. Compared with the polypropylene layer formed by the traditional wrapping process, the consistency of the polypropylene material in the polypropylene layer is higher, and the internal space charge accumulation is less, which can improve the electrical properties of the formed polypropylene layer.
[0046] According to a specific embodiment of the present application, the polypropylene layer is formed at a temperature of 160° C.-250° C., and at a pressure of 0.1 MPa-30 MPa.
[0047] Compared with cross-linked polyethylene, polypropylene has higher breakdown field strength and volume resistivity, and polypropylene molding does not require cross-linking or degassing, but there is a certain volume difference between the solid state and the molten state. Within the aforementioned temperature and pressure ranges, the polypropylene material can flow and fill the gaps between the cable connector mold and the intermediate connector. The pressure conditions control the volume shrinkage before and after the molding process, reduce the formation of structural defects in the polypropylene layer, and improve the mechanical and electrical properties of the formed polypropylene layer.
[0048] According to a specific embodiment of the present application, the polypropylene layer is a polypropylene insulating layer, wherein at 25°C, the volume resistivity of the polypropylene material forming the polypropylene insulating layer is 10 11 Ω·m-10 17 Ω·m.
[0049] Polypropylene material has good mechanical properties and high elastic modulus. The conductivity of the insulating material is affected by temperature and electric field. In order to meet the requirements of polypropylene material as an insulating layer material, when its volume resistivity is within the aforementioned range at room temperature, the electrical properties, mechanical properties, thermal properties and aging properties of the polypropylene insulation layer formed at the middle joint are all higher than 60% of the performance indicators of the cable body insulation layer.
[0050] According to a specific embodiment of the present application, the polypropylene material includes a polypropylene copolymer, and further includes: at least one of an elastomer and nanoparticles.
[0051] The electrical properties of polypropylene materials can be improved through blending, copolymerization and nano-doping technology, while retaining the material advantages of polypropylene itself, such as good mechanical properties, wear resistance and corrosion resistance.
[0052] According to a specific embodiment of the present application, the polypropylene layer is a polypropylene semi-conductive shielding layer, wherein, at room temperature, the volume resistivity of the polypropylene material forming the polypropylene semi-conductive shielding layer is less than 500Ω·m.
[0053] The semi-conductive shielding layer can make the cable conductor and the insulating layer have better contact, eliminate the increase of the surface electric field strength caused by the rough structure of the conductor surface and the insulating layer surface, effectively reduce the surface defects, and make the surface electric field uniform. When the volume resistivity of the polypropylene material is within the aforementioned volume resistivity range, the semi-conductive shielding layer formed by the polypropylene material has a suitable conductive path distribution, which plays a role in uniform interface electric field distribution, suppressing excessive local field strength, and preventing local discharge.
[0054] According to a specific embodiment of the present application, in order to adapt to the subsequent production of the insulating layer, the semi-conductive shielding layer is polished as needed.
[0055] The surface smoothness of the semiconductor shielding layer is one of its important indicators. Condition control during the molding process can improve the uniformity of the polypropylene layer. Further polishing after molding can also eliminate micropores and protrusions on the surface, improve surface smoothness, and facilitate a uniform electric field.
[0056] According to a specific embodiment of the present application, the polypropylene material includes a polypropylene copolymer, a conductive filler and an additive.
[0057] Adding conductive fillers to the polypropylene matrix can make the polypropylene material obtain semi-conductive properties, and its conductive performance is closely related to the type and filling amount of the conductive filler, the type of polymer matrix, and the dispersion of the filler in the polymer matrix. The polypropylene material can meet the performance requirements of the semi-conductive shielding layer of the power cable. The electrical performance, mechanical performance, thermal performance and aging performance of the semi-conductive shielding layer formed at the middle joint by the extrusion process are all higher than 60% of the performance indicators of the semi-conductive shielding layer of the cable body.
[0058] According to a specific embodiment of the present application, it further includes:
[0059] The polypropylene layer is subjected to a cooling process, wherein the cooling process comprises natural cooling or external contact mold cooling.
[0060] After the polypropylene material is formed in the mold body 10, the formation process of the polypropylene layer can be controlled by cooling treatment to regulate the transition of the polypropylene to the polymer glass state.
[0061] For example, when the temperature in the mold body 10 reaches a preset value, the cable connector mold can be removed. The cooling process can be natural heat dissipation, or it can be controlled by external condensation water, etc., to adjust the cooling rate to further control the formation process of the polypropylene layer and regulate the process of polypropylene transition to the polymer glass state.
[0062] In a third aspect of the present application, the present application proposes a polypropylene layer. The polypropylene layer is prepared by using the method for preparing a polypropylene layer using the cable connector mold.
[0063] The polypropylene layer proposed in this application is formed by an extrusion die. Compared with the insulating layer or semi-conductive shielding layer formed by the wrapping process, its interface is smoother and the electric field distribution is more uniform, thereby improving the overall performance of the cable.
[0064] The scheme of the present application is described below by specific examples. It should be noted that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this area or the product instructions are used. The reagents or instruments used are not specified by the manufacturer, and are all conventional products that can be obtained commercially.
[0065] Example 1
[0066] Connect the first processing port to the extruder, and use nitrogen to evacuate the air in the cable joint mold; add polypropylene material to the extruder as needed, adjust the temperature of the extruder head to 200°C and the pressure to 1MPa. Squeeze the polypropylene material into the cable joint mold through the extruder head, and open the mold outlet first during extrusion so that the internal nitrogen can be discharged; when a small amount of polypropylene material escapes from the mold outlet, close the mold outlet; continuously monitor the temperature and pressure in the mold, and when the pressure value reaches 1MPa, evacuate the extruder head and close the mold inlet, cool it for 30 minutes, remove the mold, and obtain the intermediate joint connected with the polypropylene insulation layer.
[0067] The polypropylene material is an ethylene-propylene copolymer. At room temperature, the volume resistivity of a 1 mm thick sample of the ethylene-propylene copolymer is 10 15 Ω·m, the AC breakdown of the 1mm thick sample at room temperature is 40kV / mm, and the power frequency dielectric loss of the 1mm thick sample at room temperature is 1×10 -4 .
[0068] Example 2
[0069] Example 2 is consistent with Example 1, except that the temperature of the extruder head is adjusted to 190° C., the pressure is 10 MPa, and the circulating cooling is carried out at a pressure of 10 MPa for 10 min.
[0070] The polypropylene material used is PP / SEBS. The volume resistivity of the 1mm thick sample of the PP / SEBS blend is 10 15 Ω·m, the AC breakdown of the 1mm thick sample at room temperature is 35kV / mm, and the power frequency dielectric loss of the 1mm thick sample at room temperature is 2×10 -4 .
[0071] Example 3
[0072] Example 3 is consistent with Example 2, except that the polypropylene material used is PP / POE, and the volume resistivity of the 1 mm thick sample of the PP / POE blend is 10 15 Ω·m, the AC breakdown of the 1mm thick sample at room temperature is 35kV / mm, and the power frequency dielectric loss of the 1mm thick sample at room temperature is 2×10 -4 .
[0073] Example 4
[0074] Example 4 is consistent with Example 2, except that the polypropylene material used is polypropylene grafted with styrene groups, and the volume resistivity of the 1 mm thick sample is 10 16 Ω·m, the AC breakdown of the 1mm thick sample at room temperature is 45kV / mm, and the power frequency dielectric loss of the 1mm thick sample at room temperature is 1×10 -4 .
[0075] Example 5
[0076] Example 5 is consistent with Example 1, except that the polypropylene pellets selected are semi-conductive shielding materials with a volume resistivity of 15Ω·cm at room temperature.
[0077] Example 6
[0078] Example 6 is consistent with Example 2, except that the polypropylene pellets selected are semi-conductive shielding materials with a volume resistivity of 10Ω·cm at room temperature.
[0079] A test was conducted on a polypropylene thermoplastic cable that had been connected at the middle joint using a cable joint mold. The test results showed that the cable could be used normally, met the cable operation and maintenance requirements of the cable line, and passed the engineering inspection and testing.
[0080] In the description of the present application, it should be understood that the terms "length", "width", "thickness", "up", "down", "front", "back", "left", "right", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0081] In the description of the present application, a first feature being “on” or “under” a second feature may include that the first and second features are directly in contact with each other, or may include that the first and second features are not in direct contact with each other but are in contact with each other via another feature therebetween.
[0082] In the description of the present application, “above”, “over” and “above” a first feature to a second feature includes the first feature being directly above and obliquely above the second feature, or simply means that the first feature is horizontally higher than the second feature.
[0083] In the description of the present application, "A and / or B" may include the case of A alone, the case of B alone, or any of the cases of A and B, where A and B are only used for examples and may be any technical feature connected by "and / or" in the present application.
[0084] In the present application, the writing order of each step does not mean a strict execution order and does not constitute any limitation on the implementation process. The specific execution order of each step should be determined by its function and possible internal logic. If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) can be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0085] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A cable connector mold, characterized in that: include: A mold body, wherein the mold body is a through cylinder, and the interior of the cylinder has a receiving space, and the receiving space is used to receive the semi-molded cable; Fixing members, the fixing members being arranged at both ends of the mold body to fix the semi-molded cable in the cylinder; a first processing opening, wherein the first processing opening is located between adjacent fixing members and communicates with the accommodating space; A second processing opening is located between adjacent fixing members and is communicated with the accommodating space.
2. The cable connector mold according to claim 1, characterized in that: The mold body is also provided with a sensor, wherein the sensor includes at least one of a temperature sensor, a pressure sensor, and a temperature and pressure sensor.
3. A method for preparing a polypropylene layer using the cable connector mold according to claim 1 or 2, characterized in that: include: The middle joint of the semi-molded cable is installed into the mold body; Passing nitrogen into the mold body through the first processing port or the second processing port to exhaust air; A polypropylene material is injected into the mold body through the first processing port or the second processing port to form a polypropylene layer on the outer surface of the intermediate joint of the semi-molded cable.
4. The method according to claim 3, characterized in that: The polypropylene layer is formed at a temperature of 160° C.-250° C. and a pressure of 0.1 MPa-30 MPa.
5. The method according to claim 4, characterized in that The polypropylene layer is a polypropylene insulating layer, wherein the volume resistivity of the polypropylene material forming the polypropylene insulating layer is 10 11 Ω·m-10 17 Ω·m.
6. The method according to claim 5, characterized in that The polypropylene material includes modified polypropylene modified by at least one of copolymerization modification, mixed polymerization modification, grafting modification and nano-doping modification.
7. The method according to claim 4, characterized in that The polypropylene layer is a polypropylene semi-conductive shielding layer, wherein the volume resistivity of the polypropylene material forming the polypropylene semi-conductive shielding layer is less than 500Ω·m.
8. The method according to claim 7, characterized in that The polypropylene material comprises modified polypropylene modified by at least one of copolymerization modification, co-polymerization modification, grafting modification and nano-doping modification, conductive filler and additives.
9. The method according to any one of claims 4 to 6, characterized in that: Further including: The polypropylene layer is subjected to a cooling process, wherein the cooling process comprises natural cooling or external contact mold cooling.
10. A polypropylene layer, characterized in that The method is prepared by any one of claims 3 to 9.