Composite sheet with gilded surface and preparation method thereof

By adopting a multi-layer structural design on the aluminum-plastic composite sheet, including a printing layer and an optimized glue layer, the problem of vulnerability to the gold stamping layer is solved, and the durability and visual effect are achieved, which improves the overall product. Performance and market value.

CN119058272APending Publication Date: 2024-12-03REGO PACKING GZ IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411176613.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03

Smart Images

  • Figure CN119058272A_ABST
    Figure CN119058272A_ABST
Patent Text Reader

Abstract

The invention relates to the field of gilded sheets, in particular to a surface gilded composite sheet and a preparation method thereof. A composite sheet with a gilded surface comprises a base sheet, a printing layer, a first glue layer, a gilding layer, a second glue layer and a protective film layer which are sequentially arranged. The second glue layer is composed of laminating glue and comprises a component A and a component B in parts by mass, and the mass ratio of the component A to the component B is (3-5): 1; the component A is prepared from the following components in parts by mass: 15 to 30 parts of vegetable oil polyol, 30 to 45 parts of polyester polyol, 0.5 to 3 parts of chain extender, 0.1 to 1 part of coupling agent, 0 to 1 part of rheological additive, 10 to 20 parts of calcium fluoride, 1 to 5 parts of zinc oxide, 1 to 5 parts of glass powder and 0.05 to 0.2 part of catalyst; and the component B is isocyanate. According to the composite sheet, the printing area and the gold stamping area are not prone to falling off or fading, and good durability is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of hot stamping sheets, and more specifically, to a composite sheet with hot stamping on the surface and a preparation method thereof. Background Art

[0002] In the packaging and decoration materials industry, aluminum-plastic laminate (ABL) is highly favored because it combines the corrosion resistance and aesthetics of aluminum with the flexibility and processability of plastic. ABL sheets are widely used in many fields such as food packaging, pharmaceutical packaging, and decorative panels, among which the hot stamping process adds a sense of luxury and refinement. However, although hot stamping can significantly enhance the visual effect of ABL sheets, the hot stamping area on its surface is often easily damaged due to the lack of effective protection measures.

[0003] The gold foil layer on the surface of ABL sheets faces a variety of potential damage factors during manufacturing and use. First, the bonding strength between the gold foil layer and the ABL substrate may be insufficient, resulting in easy peeling when subjected to external forces. Second, the gold foil layer itself is relatively fragile and easily eroded by mechanical friction, scratches or chemical solvents, which affects its appearance and durability. In addition, during transportation, storage and subsequent processing, the sheet may also be affected by environmental factors such as temperature changes and humidity fluctuations, further increasing the risk of damage to the gold foil area.

[0004] In order to overcome these technical difficulties, the industry has been exploring effective methods to protect the hot stamping area. Summary of the invention

[0005] In order to enhance the effective protection of the hot stamping area, the present application provides a composite sheet with hot stamping on the surface and a preparation method thereof.

[0006] In the first aspect, the present application provides a composite sheet with a surface hot stamping, which adopts the following technical solution: A composite sheet with a gold-stamped surface, comprising a base sheet, a printing layer, a first glue layer, a gold-stamping layer, a second glue layer, and a protective film layer arranged in sequence; The second glue layer is composed of a coating glue, which includes component A and component B in terms of mass fraction, and the mass ratio of component A to component B is (3-5):1; Component A comprises the following components in parts by mass: 15-30 parts of vegetable oil polyol, 30-45 parts of polyester polyol, 0.5-3 parts of chain extender, 0.1-1 parts of coupling agent, 0-1 parts of rheological additive, 10-20 parts of calcium fluoride, 1-5 parts of zinc oxide, 1-5 parts of glass powder, and 0.05-0.2 parts of catalyst; Component B is isocyanate.

[0007] The isocyanate includes a mixture of one or more of toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), liquefied MDI, isophorone diisocyanate (IPDI), and hexamethylene diisocyanate (HDI).

[0008] The base sheet is an ABL sheet.

[0009] The protective film layer is PE film.

[0010] By introducing the first glue layer as a protective layer for the printing ink (printing layer), the long-term stability of the pattern and color on the surface of the ABL base sheet is ensured. This innovative design effectively resists damage to the printing effect caused by the external environment such as frequent friction, scratching and contact with chemicals, so that the printed pattern can remain clear even under harsh conditions of use, greatly reducing the risk of falling off or fading, thereby extending the visual appeal and service life of the product.

[0011] The combined application of the second glue layer and the protective film layer builds a solid protection system for the hot stamping layer. This double protection not only enhances the bonding strength between the hot stamping layer and the base sheet, but also effectively isolates the hot stamping layer from various pollutants such as contents, alcohol, sweat, etc. Therefore, no matter what usage scenario the product is in, the hot stamping area can maintain its original brilliant metal texture and exquisite visual effect, further enhancing the grade and beauty of the product.

[0012] The multi-layer structure design of this application takes into account the durability requirements of printing and hot stamping effects, and achieves all-round protection of the sheet surface through scientific stacking layout and material selection. This design not only enhances the physical properties of the product, such as wear resistance and scratch resistance, but also improves its resistance to chemical substances, thereby significantly improving the overall durability and reliability of the product and reducing the replacement cost caused by appearance damage.

[0013] Clear and lasting printing effects and stable and bright hot stamping effects together give the product excellent visual quality. This can not only attract consumers' attention and enhance the market competitiveness of products, but also show the professional image and brand value of the company through high-quality appearance. For consumers, this high-quality packaging experience will also enhance their trust and satisfaction with the product, thereby promoting the improvement of brand loyalty.

[0014] Furthermore, as the outer protection of the hot stamping layer, the second glue layer has the primary responsibility of protecting the hot stamping layer from the external environment, such as physical wear, chemical corrosion, and ultraviolet radiation. This protection mechanism requires that the glue layer must have strong adhesion and stable physical properties. Adhesion strength is one of the key indicators to measure the performance of the glue layer. High adhesion strength means that the glue layer can adhere tightly to the hot stamping layer and is not easy to fall off or separate, thereby ensuring the integrity and durability of the hot stamping pattern. This is crucial to improving the overall quality and market value of the product. In addition to adhesion strength, transparency is also a performance requirement that cannot be ignored for the second glue layer. Good transparency can ensure that the clarity and brightness of the hot stamping pattern are not affected, making the product look more beautiful and attractive. Therefore, when preparing the glue layer, it is necessary to balance the relationship between adhesion strength and transparency.

[0015] Generally speaking, the use of fillers in laminating glue will reduce the transparency of the laminating glue. However, the application specially selected calcium fluoride, zinc oxide, and glass powder to have a lower refractive index, which is close to the refractive index in the overall special system, and can reduce the reflection of light at the interface between the second glue layer and the substrate, thereby improving light transmittance. This refractive index matching effect helps to reduce scattered light and allows light to pass through the second glue layer more smoothly. The combination of the three can also fill the tiny pores and defects in the second glue layer, making the second glue layer denser and smoother. This dense structure helps to reduce the scattering and reflection of light in the second layer and improve transparency.

[0016] Zinc oxide can also absorb some ultraviolet rays, reducing the damage of ultraviolet rays to the second glue layer and the substrate, thereby maintaining long-term transparency. Calcium fluoride has good chemical stability and can resist the erosion of a variety of chemical substances. The combination of the three improves the stability of the second glue layer and ensures that the transparency will not be reduced due to chemical reactions during long-term use.

[0017] Moreover, the combination of calcium fluoride, zinc oxide and glass powder helps improve the fluidity of the laminating glue, allowing it to flow more quickly to the surface of the hot stamping layer and be evenly distributed, reducing the generation of bubbles and wrinkles. At the same time, its good fluidity ensures that the glue layer can fully penetrate into the fine structure of the hot stamping layer, forming a more solid bond. This uniform coverage and strong bond not only improves the aesthetics of the product, but also greatly enhances the bonding strength, thereby making it more firmly bonded to the hot stamping layer, improving the bonding quality and strength.

[0018] The optimal combination of the three and the limited dosage in the system can ensure the improvement of mechanical properties while maintaining a high transparency as much as possible to meet the visual effect requirements of the hot stamping layer.

[0019] Preferably, based on the mass fraction of the component A, calcium fluoride is 13-18 parts, zinc oxide is 1-3 parts, and glass powder is 3.5-5 parts.

[0020] By adopting the above technical solution, the dosage of the three in the system is further limited, so that the three can give full play to their special coordination effect, thereby improving transparency, bonding strength and stability.

[0021] Preferably, the particle size of calcium fluoride is 30-40 nm, that of zinc oxide is 60-80 nm, and that of glass powder is 50-60 nm.

[0022] By adopting the above technical solution, the particle sizes of calcium fluoride, zinc oxide and glass powder are further limited, and the transparency of nano-scale calcium fluoride, zinc oxide and glass powder can be further improved.

[0023] Preferably, the vegetable oil polyol includes one or more of soybean oil, palm oil, castor oil, and rapeseed oil, and the polyester polyol includes one or more of polyhexanediol adipate, poly1,4-butylene adipate, and polyethylene adipate.

[0024] Preferably, the vegetable oil polyol is rapeseed oil, and the polyester polyol is poly(1,4-butylene adipate).

[0025] By adopting the above technical solution, the types of vegetable oil polyols and polyester polyols are further limited, providing a system that is more suitable for calcium fluoride, zinc oxide, and glass powder to play their roles, and further giving full play to the effects of the three.

[0026] Preferably, the preparation of the laminating glue comprises the following steps: Step a: mixing vegetable oil polyol and polyester polyol at 100-120° C. to obtain a first mixture; Step b: cooling to 60-70° C., mixing the catalyst, chain extender, rheological additive, calcium fluoride, zinc oxide, glass powder, coupling agent and the first mixture until uniform, to obtain component A; Step c: Mix component A and component B until they are uniform to obtain a laminating glue.

[0027] Preferably, the calcium fluoride, zinc oxide and glass powder are mixed with a silane coupling agent in a solvent by ultrasonic oscillation, filtered, washed and dried to obtain a modified filler.

[0028] Preferably, the preparation of the modified filler comprises the following steps: Step A: mixing the silane coupling agent and the solvent until uniform to obtain a basic solution; Step B: Mix calcium fluoride, zinc oxide, glass powder and the base solution, and ultrasonically oscillate for 20-45 minutes at 30-35kHz; the mass ratio of the total mass of calcium fluoride, zinc oxide and glass powder to the mass ratio of the silane coupling agent is 1:(0.01-0.03); Step C: solid-liquid separation of the material in step B, washing and drying the solid part to obtain a modified filler.

[0029] By adopting the above technical scheme, calcium fluoride, zinc oxide and glass powder are further processed to prepare modified fillers, which effectively reduce the free energy and polarity of the surface of calcium fluoride, zinc oxide and glass powder particles, thereby having better compatibility with the system. The modified fillers are not easy to agglomerate in the system and are more fully dispersed, which is further beneficial to improve transparency, bonding strength and stability.

[0030] In a second aspect, the present application provides a method for preparing a composite sheet with a surface hot stamping, which adopts the following technical solution: A method for preparing a composite sheet with a gold-stamped surface comprises the following steps: Step 1: Printing on the surface of the base sheet to form a printing layer; Step 2: Apply cold stamping glue on the surface of the printed layer to form a first glue layer; Step 3: Cover the surface of the first glue layer with a hot stamping film and transfer it to the surface of the first glue layer to form a hot stamping layer; Step 4: Apply laminating glue on the surface of the hot stamping layer to form a second glue layer; Step 5: Press the protective film layer and the surface of the second glue layer to obtain a composite sheet.

[0031] In summary, this application has the following beneficial effects: 1. Since the present application uses the first glue layer, the second glue layer, and the protective film layer to protect the printing layer and the hot stamping layer, it effectively isolates the erosion of the printing layer and the hot stamping layer by various pollutants such as contents, alcohol, sweat, etc., thereby extending the visual appeal and service life of the product and improving product quality.

[0032] 2. The present application further optimizes the composition of the second glue layer so that the laminating glue can quickly cover the surface of the hot stamping layer and firmly bond with it, thereby reducing defects such as bubbles and improving bonding strength and quality; moreover, the transparency and stability of the second glue layer can be ensured, and a good effect can be exerted for a long time. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is the composite sheet prepared in Example 1 of the present application.

[0034] Figure 2 This is a diagram of the condition of the conventional composite sheet after the toothpaste water test in Test 5(1).

[0035] Figure 3 This is a diagram of the composite sheet of Example 1 after undergoing the toothpaste water test in Test 5 (1). DETAILED DESCRIPTION

[0036] The present application is further described in detail below with reference to the accompanying drawings and embodiments.

[0037] The raw materials used in the following examples and comparative examples are all commercially available products. Example

[0038] Example 1 A composite sheet with a gold-stamped surface comprises a base sheet, a printing layer, a first glue layer, a gold-stamped layer, a second glue layer and a protective film layer which are arranged in sequence.

[0039] In this embodiment, the base sheet includes an outer film, a first adhesive layer, a barrier layer, a second adhesive layer, and an inner film which are fixedly arranged in sequence.

[0040] The outer film and the inner film are both polyethylene films.

[0041] The first adhesive layer and the second adhesive layer are both formed by dry compound glue. The first adhesive layer is used to connect the inner film and the barrier layer, and the second adhesive layer is used to connect the outer film and the barrier layer.

[0042] The barrier layer is aluminized EVOH film, which is commercially available.

[0043] The first glue layer is formed by commercially available cold perm glue.

[0044] The second glue layer is composed of coating glue, including component A and component B, and the mass ratio of component A to component B is 4:1.

[0045] Component A includes the following components: vegetable oil polyol, polyester polyol, chain extender, coupling agent, rheological additive, calcium fluoride, zinc oxide and glass powder.

[0046] The particle size of calcium fluoride is 35 nm, that of zinc oxide is 70 nm, and that of glass powder is 55 nm.

[0047] The plant polyol is rapeseed oil, and the polyester polyol is poly(1,4-butylene adipate).

[0048] The chain extender is pentaerythritol.

[0049] The coupling agent is a silane coupling agent.

[0050] The rheological additive is organic bentonite.

[0051] The catalyst is dibutyltin dilaurate.

[0052] The specific amount of each raw material is shown in Table 1.

[0053] Component B is toluene diisocyanate (TDI).

[0054] The preparation of laminating glue includes the following steps: Step a: Mix vegetable oil polyol and polyester polyol at 110° C. for 2 hours to obtain a first mixture.

[0055] Step b: Cooling to 65° C., mixing the catalyst, chain extender, rheological additive, calcium fluoride, zinc oxide, glass powder, coupling agent and the first mixture for reaction for 1.5 hours to obtain component A.

[0056] Step c: Mix component A and component B until they are uniform to obtain a laminating glue.

[0057] The protective film layer is a commercially available PE film.

[0058] The present application also provides a method for preparing a composite sheet with a surface hot stamping, comprising the following steps: Step 1: Use a flexographic printing machine to print the UV curing oil film on the surface of the base sheet according to the settings to form a printing layer.

[0059] Step 2: Apply cold stamping glue on the surface of the printed layer to form the first glue layer.

[0060] Step 3: Cover the surface of the first glue layer with a hot stamping film, and use a flexographic printing machine to transfer the pattern of the hot stamping film to the surface of the first glue layer to form a hot stamping layer.

[0061] Step 4: Apply laminating glue on the surface of the hot stamping layer to form a second glue layer.

[0062] Step 5: Laminate the protective film layer and the surface of the second glue layer to obtain a composite sheet, refer to Figure 1 .

[0063] Example 2 A composite sheet with a gold-stamped surface, which is different from Example 1 in that: The second glue layer is composed of coating glue, including component A and component B, and the mass ratio of component A to component B is 3:1.

[0064] Component A includes the following components: vegetable oil polyol, polyester polyol, chain extender, coupling agent, rheological additive, calcium fluoride, zinc oxide and glass powder.

[0065] The particle size of calcium fluoride is 30 nm, that of zinc oxide is 60 nm, and that of glass powder is 50 nm.

[0066] The plant polyol is soybean oil, and the polyester polyol is poly(hexanediol adipate).

[0067] The chain extender is glycerol.

[0068] The coupling agent is a silane coupling agent.

[0069] The rheological additive is organic bentonite.

[0070] The catalyst is dibutyltin dilaurate.

[0071] The specific amount of each raw material is shown in Table 1.

[0072] Component B is toluene diisocyanate (TDI).

[0073] The preparation of laminating glue includes the following steps: Step a: Mix the vegetable oil polyol and the polyester polyol at 120° C. for 2 hours to obtain a first mixture.

[0074] Step b: Cooling to 70° C., mixing the catalyst, chain extender, rheological additive, calcium fluoride, zinc oxide, glass powder, coupling agent and the first mixture for reaction for 1.5 hours to obtain component A.

[0075] Step c: Mix component A and component B until they are uniform to obtain a laminating glue.

[0076] Example 3 A composite sheet with a gold-stamped surface, which is different from Example 1 in that: The second glue layer is composed of coating glue, including component A and component B, and the mass ratio of component A to component B is 5:1.

[0077] Component A includes the following components: vegetable oil polyol, polyester polyol, chain extender, coupling agent, rheological additive, calcium fluoride, zinc oxide and glass powder.

[0078] The particle size of calcium fluoride is 40 nm, that of zinc oxide is 80 nm, and that of glass powder is 60 nm.

[0079] The plant polyol is castor oil, and the polyester polyol is polyethylene adipate.

[0080] The chain extender is ethylene glycol.

[0081] The coupling agent is a silane coupling agent.

[0082] The rheological additive is organic bentonite.

[0083] The catalyst is dibutyltin dilaurate.

[0084] The specific amount of each raw material is shown in Table 1.

[0085] Component B is toluene diisocyanate (TDI).

[0086] The preparation of laminating glue includes the following steps: Step a: Mix the vegetable oil polyol and the polyester polyol at 100° C. for 2 hours to obtain a first mixture.

[0087] Step b: Cooling to 60° C., mixing the catalyst, chain extender, rheological additive, calcium fluoride, zinc oxide, glass powder, coupling agent and the first mixture for reaction for 1.5 hours to obtain component A.

[0088] Step c: Mix component A and component B until they are uniform to obtain a laminating glue.

[0089] Example 4 A composite sheet with a gold-stamped surface, which is different from Example 1 in that: The second glue layer is composed of coating glue, including component A and component B, and the mass ratio of component A to component B is 4:1.

[0090] Component A includes the following components: vegetable oil polyol, polyester polyol, chain extender, coupling agent, rheological additive, calcium fluoride, zinc oxide and glass powder.

[0091] The particle size of calcium fluoride is 35 nm, that of zinc oxide is 70 nm, and that of glass powder is 55 nm.

[0092] The plant polyol is rapeseed oil, and the polyester polyol is poly(1,4-butylene adipate).

[0093] The chain extender is pentaerythritol.

[0094] The coupling agent is a silane coupling agent.

[0095] The rheological additive is organic bentonite.

[0096] The catalyst is dibutyltin dilaurate.

[0097] The specific amount of each raw material is shown in Table 1.

[0098] Component B is toluene diisocyanate (TDI).

[0099] The preparation of laminating glue includes the following steps: Step a: Mix vegetable oil polyol and polyester polyol at 110° C. for 2 hours to obtain a first mixture.

[0100] Step b: Cooling to 65° C., mixing the catalyst, chain extender, rheological additive, calcium fluoride, zinc oxide, glass powder, coupling agent and the first mixture for reaction for 1.5 hours to obtain component A.

[0101] Step c: Mix component A and component B until they are evenly mixed to obtain a laminating glue.

[0102] Table 1 Category Example 1 Example 2 Example 3 Example 4 Vegetable oil polyols (kg) 20 15 30 20 Polyester polyol (kg) 40 30 45 40 Chain extender (kg) 2 0.5 3 2 Coupling agent(kg) 0.5 0.1 1 0.5 Rheological additive (kg) 0.6 0.01 1 0.6 Calcium fluoride (kg) 18 10 20 13 Zinc oxide (kg) 3 1 5 1 Glass powder(kg) 3.5 1 5 5 Catalyst(kg) 0.1 0.05 0.2 0.1 Example 5 A composite sheet with a gold-stamped surface, which is different from Example 1 in that the particle size of calcium fluoride is 35 mm, the particle size of zinc oxide is 70 mm, and the particle size of glass powder is 55 mm.

[0103] Example 6 A composite sheet with a gold-stamped surface, which is different from Example 1 in that: The preparation of laminating glue includes the following steps: Step a: preparing a modified filler, specifically comprising the following steps: Step A: KH560 and solvent were mixed at a mass ratio of 1:15 until uniform to obtain a basic solution.

[0104] The solvent was dichloromethane.

[0105] Step B: Calcium fluoride, zinc oxide, glass powder and the basic solution were mixed and ultrasonically vibrated at 30 kHz for 45 minutes.

[0106] The mass ratio of the total mass of calcium fluoride, zinc oxide and glass powder to the mass ratio of the silane coupling agent is 1:0.01.

[0107] Step C: solid-liquid separation of the material in step B, washing and drying the solid part to constant weight to obtain a modified filler.

[0108] Step b: Mix the vegetable oil polyol and the polyester polyol at 110° C. for 2 hours to obtain a first mixture.

[0109] Step c: cooling to 65° C., mixing the catalyst, chain extender, rheological additive, calcium fluoride, zinc oxide, glass powder, coupling agent and the first mixture for reaction for 1.5 hours to obtain component A.

[0110] Step d: Mix component A and component B until they are uniform to obtain a laminating glue.

[0111] Example 7 A composite sheet with a gold-stamped surface, which is different from Example 1 in that: The preparation of laminating glue includes the following steps: Step a: preparing a modified filler, specifically comprising the following steps: Step A: KH560 and solvent were mixed at a mass ratio of 1:15 until uniform to obtain a basic solution.

[0112] The solvent was dichloromethane.

[0113] Step B: Calcium fluoride, zinc oxide, glass powder and the basic solution were mixed and ultrasonically vibrated at 35 kHz for 20 minutes.

[0114] The mass ratio of the total mass of calcium fluoride, zinc oxide and glass powder to the mass ratio of the silane coupling agent is 1:0.03.

[0115] Step C: solid-liquid separation of the material in step B, washing and drying the solid part to constant weight to obtain a modified filler.

[0116] Step b: Mix the vegetable oil polyol and the polyester polyol at 110° C. for 2 hours to obtain a first mixture.

[0117] Step c: cooling to 65° C., mixing the catalyst, chain extender, rheological additive, calcium fluoride, zinc oxide, glass powder, coupling agent and the first mixture for reaction for 1.5 hours to obtain component A.

[0118] Step d: Mix component A and component B until they are uniform to obtain a laminating glue.

[0119] Comparative Example Comparative Example 1 A composite sheet with a gold-stamped surface, which is different from Example 1 in that in component A, calcium fluoride is replaced by silicon dioxide.

[0120] Comparative Example 2 A composite sheet with a gold-stamped surface, which is different from Example 1 in that in component A, zinc oxide is replaced by titanium oxide.

[0121] Comparative Example 3 A composite sheet with a gold-stamped surface, which is different from Example 1 in that in component A, the glass powder is replaced by aluminum oxide.

[0122] Comparative Example 4 A composite sheet with a gold-stamped surface, which is different from Example 1 in that calcium fluoride is 3.5 kg, zinc oxide is 10 kg, and glass powder is 11 kg.

[0123] Performance testing 1. Light transmittance: Referring to GB / T 2410-2008 "Determination of light transmittance and haze of transparent plastics", the laminating glues of Examples 1-7 and Comparative Examples 1-4 were prepared into corresponding glue layer samples, and light transmittance tests were performed. The light transmittances were recorded in Table 2.

[0124] 2. Adhesion strength: The coating glue of Examples 1-7 and Comparative Examples 1-4 was applied on the surface of PE film (14 μm, 2.5 cm×30 cm) by scraping, and the amount of glue was controlled at 35 g / m 2 .

[0125] The glued PE film was placed in an oven at 45°C and baked for 15 seconds.

[0126] The baked PE film was pressed together with another PE film without glue, the upper mold was controlled at 45°C, the lower mold was at room temperature, the hot pressing time was 10s, and the pressure was 0.2MPa to obtain a sample.

[0127] The samples were subjected to initial adhesion test according to standard GB / T 2790-1995 (the time interval from sample pressing to the start of initial adhesion peel strength test was 15-20s), with a stretching length of 5cm and a speed of 100mm / min.

[0128] The bonding strength is recorded in Table 2.

[0129] 3. Stability of coating glue: The coating glue of Examples 1-7 and Comparative Examples 1-4 was coated on the surface of PE film (14 μm, 2.5 cm×30 cm) by scraping, and the amount of glue was controlled at 35 g / m 2 .

[0130] The glued PE film was placed in an oven at 45°C and baked for 15 seconds.

[0131] The baked PE film was pressed together with another PE film without glue, the upper mold was controlled at 45°C, the lower mold was at room temperature, the hot pressing time was 10s, and the pressure was 0.2MPa to obtain a sample.

[0132] The samples were immersed in 20% toothpaste water for 24 hours, taken out, and boiled in 60°C water for 4 hours to obtain the treated samples.

[0133] The treated samples were tested according to the standard GB / T 2790-1995, with a stretching length of 5 cm and a speed of 100 mm / min.

[0134] The bond strength after treatment is recorded in Table 2.

[0135] 4. Fluidity: Observe the surface of the PE film after baking in Test 2 to see whether the coating glue forms a uniform and smooth glue layer. Record the observation results in Table 2.

[0136] Table 2 Comparative Examples 1-3 are based on Example 1, and any of calcium fluoride, zinc oxide, and glass powder is replaced with other raw materials; Comparative Example 4 is based on Example 1, and the amount of calcium fluoride, zinc oxide, and glass powder in the system is changed. According to the test data in Table 2, Example 1 has better fluidity and forms a uniform, smooth, and bubble-free glue layer, while Comparative Examples 1-4 are not as good as Example 1. Under this difference, the performance gap between Comparative Examples 1-4 and Example 1 is further widened. The light transmittance of Comparative Examples 1-4 is significantly lower than that of Example 1, and the bonding strength is not as good as that of Example 1. It shows that the special combination of calcium fluoride, zinc oxide, and glass powder in the system can not only ensure mechanical properties, but also not affect transparency. In Test 3, after being soaked in toothpaste water, boiled in water, etc., Example 1 still shows better bonding strength than Comparative Examples 1-4, indicating that Example 1 is more stable, can resist external influences, and has a good effect for a long time.

[0137] Example 5 is based on Example 1, but the particle sizes of calcium fluoride, zinc oxide and glass powder are changed. The transparency of Example 5 is reduced to a certain extent, but the performance in terms of bonding strength and fluidity is not significantly affected. This shows that further limiting the particle sizes of calcium fluoride, zinc oxide and glass powder is more conducive to improving the performance of the glue layer.

[0138] In Examples 6 and 7, based on Example 1, calcium fluoride, zinc oxide and glass powder are processed to prepare modified fillers and mixed into the system, which effectively further improves the agglomeration of calcium fluoride, zinc oxide and glass powder in the system, thereby improving transparency, bonding performance and stability.

[0139] 5. Composite sheet stability: (1) Toothpaste water: prepare toothpaste water with a concentration of 20%. Roll the composite sheets with gold stamping on the surface of Examples 1-7 and Comparative Examples 1-4 into a simulated hose, wrinkle the entire hose, soak it in toothpaste water for 24 hours, take it out and wash it with clean water, fold it front and back, and rub it in a friction tester for 100 times to observe whether the gold stamping falls off.

[0140] The protective film layer, as the outermost layer, protects the composite sheet as a whole, and cooperates with the high-performance second glue layer. In the composite sheet stability test, the composite sheets with gold stamping on the surface of Examples 1-7 do not lose ink or gold stamping. In the test of the composite sheets of Comparative Examples 1-4, due to the corrosive ability of toothpaste water, the toothpaste water penetrates into the protective film layer and the second glue layer. The composite sheets of Comparative Examples 1-4 use a poor-performance laminating glue, which causes the gold stamping layer to be corroded by the toothpaste water, showing different degrees of gold stamping falling.

[0141] (2) Boiling: The composite sheets with gold stamping on the surface of Examples 1-7 and Comparative Examples 1-4 were rolled into a hose, the whole hose was crumpled, and boiled in 60°C water for 30 hours. After taking out, the water was wiped off and the gold stamping was observed to see if it fell off.

[0142] The composite sheets with gold stamping on the surface of Examples 1-7 did not lose ink or gold stamping. The laminating glue of Comparative Examples 1-4 was not stable enough, so that the protective film layer and the gold stamping layer could not be firmly bonded, and the gold stamping layer partially fell off in the water boiling test.

[0143] Figure 2 This is a picture of the condition of the conventional composite sheet after the toothpaste water test in Test 5 (1). The gold stamping can be seen to have fallen off with the naked eye.

[0144] The traditional composite sheet is a layer of varnish wrapped on the surface of the hot stamping layer, that is, the varnish is coated on the surface of the hot stamping layer by a rubber roller and cured by a UV lamp to form a varnish protective layer.

[0145] Figure 3 This is a diagram of the composite sheet of Example 1 after the toothpaste water test in Test 5 (1). It can be seen that the hot stamping and printing areas of the composite sheet of Example 1 are in good condition.

[0146] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A composite sheet with a gold-stamped surface, characterized in that: It includes a base sheet, a printing layer, a first glue layer, a hot stamping layer, a second glue layer, and a protective film layer which are arranged in sequence; The second glue layer is composed of a coating glue, which includes component A and component B in terms of mass fraction, and the mass ratio of component A to component B is (3-5):1; Component A comprises the following components in parts by mass: 15-30 parts of vegetable oil polyol, 30-45 parts of polyester polyol, 0.5-3 parts of chain extender, 0.1-1 parts of coupling agent, 0-1 parts of rheological additive, 10-20 parts of calcium fluoride, 1-5 parts of zinc oxide, 1-5 parts of glass powder, and 0.05-0.2 parts of catalyst; Component B is isocyanate.

2. The composite sheet with hot stamping on the surface according to claim 1, characterized in that: Calculated by mass of the component A, calcium fluoride is 13-18 parts, zinc oxide is 1-3 parts, and glass powder is 3.5-5 parts.

3. The composite sheet with hot stamping on the surface according to claim 1, characterized in that: The particle size of the calcium fluoride is 30-40nm, the particle size of the zinc oxide is 60-80nm, and the particle size of the glass powder is 50-60nm.

4. The composite sheet with hot stamping on the surface according to claim 1, characterized in that: The vegetable oil polyol includes one or more of soybean oil, palm oil, castor oil, and rapeseed oil; the polyester polyol includes one or more of polyhexanediol adipate, poly1,4-butylene adipate, and polyethylene adipate.

5. The composite sheet with hot stamping on the surface according to claim 4, characterized in that: The vegetable oil polyol is rapeseed oil, and the polyester polyol is poly(1,4-butylene adipate).

6. The composite sheet with hot stamping on the surface according to any one of claims 1 to 5, characterized in that: The preparation of the coating glue comprises the following steps: Step a: mixing vegetable oil polyol and polyester polyol at 100-120° C. to obtain a first mixture; Step b: cooling to 60-70° C., mixing the catalyst, chain extender, rheological additive, calcium fluoride, zinc oxide, glass powder, coupling agent and the first mixture until uniform, to obtain component A; Step c: Mix component A and component B until they are uniform to obtain a laminating glue.

7. The composite sheet with hot stamping on the surface according to claim 6, characterized in that: The calcium fluoride, zinc oxide and glass powder are mixed with a silane coupling agent in a solvent by ultrasonic oscillation, filtered, washed and dried to obtain a modified filler.

8. The composite sheet with hot stamping on the surface according to claim 7, characterized in that: The preparation of the modified filler comprises the following steps: Step A: mixing the silane coupling agent and the solvent until uniform to obtain a basic solution; Step B: Mix calcium fluoride, zinc oxide, glass powder and the base solution, and ultrasonically oscillate for 20-45 minutes at 30-35kHz; the mass ratio of the total mass of calcium fluoride, zinc oxide and glass powder to the mass ratio of the silane coupling agent is 1:(0.01-0.03); Step C: solid-liquid separation of the material in step B, washing and drying the solid part to obtain a modified filler.

9. A method for preparing a composite sheet with a surface hot stamping according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1: Printing on the surface of the base sheet to form a printing layer; Step 2: Apply cold stamping glue on the surface of the printed layer to form a first glue layer; Step 3: Cover the surface of the first glue layer with a hot stamping film and transfer it to the surface of the first glue layer to form a hot stamping layer; Step 4: Apply laminating glue on the surface of the hot stamping layer to form a second glue layer; Step 5: Press the protective film layer and the surface of the second glue layer to obtain a composite sheet.