Method for preparing sodium-ion battery carbon-based negative electrode material from waste wood
Through two-step carbonization method based on waste wood and reducing carbonization treatment, the problem of low efficiency of hard carbon materials for sodium ion battery for the first time was solved. By reducing surface defects and irreversible capacity losses, the electrochemical performance and cyclic performance of the material were improved.
Patent Information
- Application Number
- CN202310644676.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-12-03
AI Technical Summary
The first Coulomb efficiency of hard carbon materials in existing sodium ion batteries is mainly due to surface defects and irreversible sodium ion embedding problems, which affects the electrochemical performance of the material.
Using two-step carbonization method based on waste wood and reducing carbonization treatment method, including ultrasonic washing in deionized water, high-temperature carbonization, acid solution washing and high-temperature pyrolysis under air or inert atmosphere, reducing material defects and irreversible capacity loss, and improving Reversible capacity of the material.
The hard carbon material prepared by this method has fewer surface defects and appropriate layer spacing, which improves the deintercalation capacity of sodium ions, significantly improves the capacity of the material and the first-time Coulomb efficiency, and demonstrates excellent cycling performance.
Smart Images

Figure HSA0000297017610000011 
Figure HSA0000297017610000021 
Figure HSA0000297017610000031
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of sodium ion battery electrode materials, and in particular relates to a method for preparing a carbon-based negative electrode material for a sodium ion battery based on waste wood. Background Art
[0002] Lithium-ion batteries occupy a large share of the energy market and are widely used in daily life due to their excellent high energy density, long cycle life, stable safety and other advantages. However, the content of lithium in the earth's crust is very limited and unevenly distributed, which can no longer meet the growing demand for energy storage. Therefore, there is an urgent need to find alternatives to lithium-ion batteries. Sodium and lithium belong to the same group of elements with similar physical and chemical properties. Sodium ion resources are abundant, cheap, and environmentally friendly, which has attracted widespread attention from researchers and scholars. It has great potential in large-scale energy storage.
[0003] Finding suitable negative electrode materials is of great significance to the development of sodium-ion batteries. Among them, carbon-based materials have the advantages of low cost, good conductivity, and high sodium storage capacity, and have commercial application prospects. Graphite, which is widely used in lithium-ion batteries, is a traditional carbon material with excellent electrochemical properties. However, it is not satisfactory in sodium-ion battery applications because the sodium ion radius is large and the ionization potential is high, resulting in poor sodium storage performance of graphite. Compared with graphite, hard carbon has a larger interlayer spacing and more defects, and has a low potential and high capacity. It is considered to be one of the most promising negative electrode materials for sodium-ion batteries. As one of the precursors of hard carbon materials, biomass materials have rich microstructures, large interlayer spacing, and a high degree of disorder. They can be used as low-cost, green and renewable clean energy, which has attracted widespread attention and is regarded as a reliable large-scale carbon source.
[0004] In the relevant research reports on hard carbon materials, pyrolysis under an inert atmosphere is a common treatment process for biomass carbon. It is usually necessary to use a treatment temperature above 1000°C to obtain hard carbon with a sufficiently ordered structure for electrochemical applications. Two preparation strategies are generally used: one-step carbonization and two-step carbonization. However, in the one-step direct pyrolysis, the carbon atoms may not have enough time to reorganize, resulting in pseudo-graphitization of the structure. The two-step carbonization provides better first coulombic efficiency (ICE) and reversible capacity. Chang et al. used lignin as a precursor, extracted with acetone, and N 2 Carbonization and H 2 The hard carbon material was prepared by reduction, and the first discharge / charge capacity was 882.2 / 550.5mAh / g (Coulomb efficiency (CE) was 62.4%). Zhu et al. used waste apricot shell as raw material to synthesize high-performance hard carbon through pyrolysis and reduction processes. The hard carbon finally prepared had good anode performance, and the improved ICE could reach 79%. 2Reduction treatment can reduce the oxygen content in hard carbon, increase the interlayer spacing, reduce the surface defects of the material and the occurrence of unnecessary side reactions, and further improve the sodium storage performance of the material. However, the irreversible embedding of sodium ions during the first discharge process causes the first coulomb efficiency of hard carbon materials to be low. Therefore, surface defects and specific surface area are the primary factors affecting the electrochemical properties of materials. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a method for preparing a hard carbon negative electrode material for sodium ion batteries based on waste wood. The prepared material has fewer surface defects and a suitable interlayer spacing. This structure is conducive to the deintercalation of sodium ions, effectively improving the capacity and first coulombic efficiency of the material.
[0006] In order to solve the above technical problems, the present invention provides a method for preparing a hard carbon negative electrode material for a sodium ion battery based on waste wood, comprising the following steps: Step 1: placing the waste wood in deionized water for ultrasonic washing pretreatment to remove surface dust and impurities, and placing the washed waste wood in a blast drying oven to dry, thereby obtaining a waste wood precursor; Step 2: The obtained waste wood precursor is transferred to a muffle furnace, carbonized in an air atmosphere, and placed in a grinder after natural cooling to grind into powder to obtain a pre-carbonized product; Step 3: Transfer the pre-carbonized product to an atmosphere furnace, perform high-temperature carbonization under the protection of an inert gas, and grind and sieve after natural cooling; Step 4: placing the treated hard carbon material in an acidic solution, then washing with deionized water and ethanol until neutral, placing the obtained product in a blast drying oven to dry, grinding and sieving, and obtaining a waste wood hard carbon material; Step 5: Transfer the waste wood hard carbon material to an atmosphere furnace, carbonize it under a reducing atmosphere, and sieve it after natural cooling to obtain the reduced waste wood hard carbon material.
[0007] Furthermore, the waste wood raw material in step one is sourced from Salix psammophila, the temperature of the blast drying oven is 80° C., and the drying time is 12 hours.
[0008] Furthermore, in step 2, the heating rate of the muffle furnace is 5°C / min, the pyrolysis temperature is 300°C, and the insulation time is 2 hours.
[0009] Furthermore, in step 3, the heating rate of high temperature carbonization is 5°C / min, the pyrolysis temperature is 1400°C, and the holding time is 2 hours. In step 3, the inert gas flow rate is 10-100CC / min. The cooling rate is maintained at 5°C / min.
[0010] Furthermore, in step 4, the acidic solution is selected from one of dilute hydrochloric acid, dilute sulfuric acid or dilute nitric acid, the concentration of the acidic solution is 1-2 mol / L, the soaking time is 6-12 hours, the temperature of the vacuum drying oven is 80° C., and the drying time is 12 hours.
[0011] Furthermore, in step 5, the heating rate of reduction carbonization is 5°C / min, the pyrolysis temperature is 600-1200°C, and the insulation time is 2 hours.
[0012] According to another aspect of the present invention, a carbon-based negative electrode material for a sodium ion battery is provided, characterized in that it is prepared by the method described above.
[0013] According to another aspect of the present invention, a hard carbon material electrode sheet is provided, which is obtained by uniformly grinding the above-mentioned sodium ion battery hard carbon negative electrode material with acetylene black and sodium carboxymethyl cellulose in proportion, adding pure water and magnetically stirring to obtain a uniformly mixed electrode slurry, coating the battery slurry evenly on a copper foil with a coating machine, placing it in a vacuum drying oven for vacuum drying, and then preparing it into a disc electrode with a punching machine to obtain the hard carbon material electrode sheet.
[0014] Furthermore, the mass ratio of the hard carbon material, acetylene black and sodium carboxymethyl cellulose is 8:1:1.
[0015] According to another aspect of the present invention, a sodium ion battery is provided, which comprises the hard carbon material electrode sheet described above.
[0016] Compared with the prior art, the present invention has the following advantages and technical effects: Salix psammophila is usually used for desert greening, but a large amount of waste wood is generated in actual production. The present invention uses waste Salix psammophila as raw material, has a simple preparation method, low cost, is environmentally friendly, and is suitable for large-scale production. The present invention effectively reduces the defect concentration of the material, reduces the irreversible capacity loss, and improves the reversible capacity of the material through a two-step carbonization method of low-temperature carbonization and high-temperature pyrolysis and a reduction carbonization treatment, showing excellent cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is the XRD pattern of the biomass-derived hard carbon negative electrode material prepared in Examples 1, 2, 3, 4, and 5 of the present invention; Figure 2 is the Raman graph of the biomass-derived hard carbon negative electrode material prepared in Examples 1, 2, 3, 4, and 5 of the present invention; Figure 3 This is a first cycle charge and discharge curve diagram of the biomass-derived hard carbon negative electrode material prepared in Example 2 of the present invention; Figure 4 is a cyclic voltammogram of the biomass-derived hard carbon negative electrode material prepared in Example 2 of the present invention; Figure 5is a rate performance curve diagram of the biomass-derived hard carbon negative electrode material prepared in Example 2 of the present invention; Figure 6 is a SEM image of the biomass-derived hard carbon negative electrode material prepared in Example 2 of the present invention; DETAILED DESCRIPTION
[0018] The method described in the present invention is explained and illustrated in detail by examples below. The examples are only used to explain the present invention and do not exceed the scope of the present invention. However, the protection scope of the present invention is not limited by the examples.
[0019] Example 1 Step 1: The biomass Salix psammophila was ultrasonically washed with deionized water for 6 hours to remove dust and impurities, and the obtained product was dried in a forced air drying oven at 60° C. for 24 hours to remove moisture; Step 2: Transfer the dried Salix psammophila to a muffle furnace, heat it to 300°C at a heating rate of 5°C / min in an air atmosphere and keep it for 2 hours, cool it naturally in the furnace and take it out, crush the pre-carbonized product into powder with a pulverizer for later use; Step 3: Put the pre-carbonized product into a tubular furnace, and under the protection of inert gas argon, heat it from room temperature 20°C to 1400°C at a heating rate of 5°C / min, keep it warm for 2 hours, cool it to room temperature at a cooling rate of 5°C / min with the furnace, take it out and grind it, and sieve it with a 325-mesh sieve; Step 4: The obtained powder is subjected to acid washing treatment. The selected acid washing solution is a 2M dilute hydrochloric acid solution. After soaking for 12 hours, it is repeatedly centrifuged and washed with deionized water and ethanol until it becomes neutral. The obtained product is dried in a forced air drying oven at 80°C for 12 hours to obtain a hard carbon negative electrode material.
[0020] Example 2 Step 1: The biomass Salix psammophila was ultrasonically washed with deionized water for 6 hours to remove dust and impurities, and the obtained product was dried in a forced air drying oven at 60° C. for 24 hours to remove moisture; Step 2: Transfer the dried Salix psammophila to a muffle furnace, heat it to 300°C at a heating rate of 5°C / min in an air atmosphere and keep it for 2 hours, cool it naturally in the furnace and take it out, crush the pre-carbonized product into powder with a pulverizer for later use; Step 3: Put the pre-carbonized product into a tubular furnace, and under the protection of inert gas argon, heat it from room temperature 20°C to 1400°C at a heating rate of 5°C / min, keep it warm for 2 hours, cool it to room temperature at a cooling rate of 5°C / min with the furnace, take it out and grind it, and sieve it with a 325-mesh sieve; Step 4: The obtained powder is subjected to acid washing treatment, and the selected acid washing solution is a 2M dilute hydrochloric acid solution. After soaking for 12 hours, it is repeatedly centrifuged and washed with deionized water and ethanol until it is neutral. The obtained product is dried in a forced air drying oven at 80°C for 12 hours to obtain a powder after drying. Step 5: Place the dried powder into a tube furnace and heat it in H 2 Under the protection of Ar / Ar mixed atmosphere, the temperature was increased from room temperature (20°C) to 600°C at a heating rate of 5°C / min, kept at that temperature for 2 hours, and cooled to room temperature at a cooling rate of 5°C / min along with the furnace to obtain a hard carbon negative electrode material.
[0021] Example 3 Step 1: The biomass Salix psammophila was ultrasonically washed with deionized water for 6 hours to remove dust and impurities, and the obtained product was dried in a forced air drying oven at 60° C. for 24 hours to remove moisture; Step 2: Transfer the dried Salix psammophila to a muffle furnace, heat it to 300°C at a heating rate of 5°C / min in an air atmosphere and keep it for 2 hours, cool it naturally in the furnace and take it out, crush the pre-carbonized product into powder with a pulverizer for later use; Step 3: Put the pre-carbonized product into a tubular furnace, and under the protection of inert gas argon, heat it from room temperature 20°C to 1400°C at a heating rate of 5°C / min, keep it warm for 2 hours, cool it to room temperature at a cooling rate of 5°C / min with the furnace, take it out and grind it, and sieve it with a 325-mesh sieve; Step 4: The obtained powder is subjected to acid washing treatment, and the selected acid washing solution is a 2M dilute hydrochloric acid solution. After soaking for 12 hours, it is repeatedly centrifuged and washed with deionized water and ethanol until it is neutral. The obtained product is dried in a forced air drying oven at 80°C for 12 hours to obtain a powder after drying. Step 5: Place the dried powder into a tube furnace and heat it in H 2 Under the protection of Ar / Ar mixed atmosphere, the temperature was increased from room temperature (20°C) to 800°C at a heating rate of 5°C / min, kept at that temperature for 2 hours, and cooled to room temperature at a cooling rate of 5°C / min along with the furnace to obtain a hard carbon negative electrode material.
[0022] Example 4 Step 1: The biomass Salix psammophila was ultrasonically washed with deionized water for 6 hours to remove dust and impurities, and the obtained product was dried in a forced air drying oven at 60° C. for 24 hours to remove moisture; Step 2: Transfer the dried Salix psammophila to a muffle furnace, heat it to 300°C at a heating rate of 5°C / min in an air atmosphere and keep it for 2 hours, cool it naturally in the furnace and take it out, crush the pre-carbonized product into powder with a pulverizer for later use; Step 3: Put the pre-carbonized product into a tubular furnace, and under the protection of inert gas argon, heat it from room temperature 20°C to 1400°C at a heating rate of 5°C / min, keep it warm for 2 hours, cool it to room temperature at a cooling rate of 5°C / min with the furnace, take it out and grind it, and sieve it with a 325-mesh sieve; Step 4: The obtained powder is subjected to acid washing treatment, and the selected acid washing solution is a 2M dilute hydrochloric acid solution. After soaking for 12 hours, it is repeatedly centrifuged and washed with deionized water and ethanol until it is neutral. The obtained product is dried in a forced air drying oven at 80°C for 12 hours to obtain a powder after drying. Step 5: Place the dried powder into a tube furnace and heat it in H 2 Under the protection of Ar / Ar mixed atmosphere, the temperature was increased from room temperature (20°C) to 1000°C at a heating rate of 5°C / min, kept at that temperature for 2 hours, and cooled to room temperature at a cooling rate of 5°C / min along with the furnace to obtain a hard carbon negative electrode material.
[0023] Example 5 Step 1: The biomass Salix psammophila was ultrasonically washed with deionized water for 6 hours to remove dust and impurities, and the obtained product was dried in a forced air drying oven at 60° C. for 24 hours to remove moisture; Step 2: Transfer the dried Salix psammophila to a muffle furnace, heat it to 300°C at a heating rate of 5°C / min in an air atmosphere and keep it for 2 hours, cool it naturally in the furnace and take it out, crush the pre-carbonized product into powder with a pulverizer for later use; Step 3: Put the pre-carbonized product into a tubular furnace, and under the protection of inert gas argon, heat it from room temperature 20°C to 1400°C at a heating rate of 5°C / min, keep it warm for 2 hours, cool it to room temperature at a cooling rate of 5°C / min with the furnace, take it out and grind it, and sieve it with a 325-mesh sieve; Step 4: The obtained powder is subjected to acid washing treatment, and the selected acid washing solution is a 2M dilute hydrochloric acid solution. After soaking for 12 hours, it is repeatedly centrifuged and washed with deionized water and ethanol until it is neutral. The obtained product is dried in a forced air drying oven at 80°C for 12 hours to obtain a powder after drying. Step 5: Place the dried powder into a tube furnace and heat it in H 2 Under the protection of a mixed atmosphere of Ar / Ar, the temperature was increased from room temperature (20°C) to 1200°C at a heating rate of 5°C / min, kept at that temperature for 2 hours, and cooled to room temperature at a cooling rate of 5°C / min along with the furnace to obtain a hard carbon negative electrode material.
[0024] Comparative Example 1 Step 1: The biomass Salix psammophila was ultrasonically washed with deionized water for 6 hours to remove dust and impurities, and the obtained product was dried in a forced air drying oven at 60° C. for 24 hours to remove moisture; Step 2: Transfer the dried Salix psammophila to a muffle furnace, heat it to 300°C at a heating rate of 5°C / min in an air atmosphere and keep it for 2 hours, cool it naturally in the furnace and take it out, crush the pre-carbonized product into powder with a pulverizer for later use; Step 3: Put the pre-carbonized product into a tubular furnace, and under the protection of a reducing atmosphere, heat it from room temperature (20°C) to 600°C at a heating rate of 5°C / min, keep it warm for 2 hours, cool it to room temperature at a cooling rate of 5°C / min with the furnace, take it out and grind it, and sieve it with a 325-mesh sieve; Step 4: The obtained powder is subjected to acid washing treatment. The selected acid washing solution is a 2M dilute hydrochloric acid solution. After soaking for 12 hours, it is repeatedly centrifuged and washed with deionized water and ethanol until it becomes neutral. The obtained product is dried in a forced air drying oven at 80°C for 12 hours to obtain a hard carbon negative electrode material.
[0025] Comparative Example 2 Step 1: The biomass Salix psammophila was ultrasonically washed with deionized water for 6 hours to remove dust and impurities, and the obtained product was dried in a forced air drying oven at 60° C. for 24 hours to remove moisture; Step 2: Transfer the dried Salix psammophila to a muffle furnace, heat it to 300°C at a heating rate of 5°C / min in an air atmosphere and keep it for 2 hours, cool it naturally in the furnace and take it out, crush the pre-carbonized product into powder with a pulverizer for later use; Step 3: Put the pre-carbonized product into a tubular furnace, and under the protection of a reducing atmosphere, heat it from room temperature (20°C) to 800°C at a heating rate of 5°C / min, keep it warm for 2 hours, cool it to room temperature at a cooling rate of 5°C / min with the furnace, take it out and grind it, and sieve it with a 325-mesh sieve; Step 4: The obtained powder is subjected to acid washing treatment. The selected acid washing solution is a 2M dilute hydrochloric acid solution. After soaking for 12 hours, it is repeatedly centrifuged and washed with deionized water and ethanol until it becomes neutral. The obtained product is dried in a forced air drying oven at 80°C for 12 hours to obtain a hard carbon negative electrode material.
[0026] Comparative Example 3 Step 1: The biomass Salix psammophila was ultrasonically washed with deionized water for 6 hours to remove dust and impurities, and the obtained product was dried in a forced air drying oven at 60° C. for 24 hours to remove moisture; Step 2: Transfer the dried Salix psammophila to a muffle furnace, heat it to 300°C at a heating rate of 5°C / min in an air atmosphere and keep it for 2 hours, cool it naturally in the furnace and take it out, crush the pre-carbonized product into powder with a pulverizer for later use; Step 3: Put the pre-carbonized product into a tubular furnace, and under the protection of a reducing atmosphere, heat it from room temperature (20°C) to 1000°C at a heating rate of 5°C / min, keep it warm for 2 hours, cool it to room temperature at a cooling rate of 5°C / min with the furnace, take it out and grind it, and sieve it with a 325-mesh sieve; Step 4: The obtained powder is subjected to acid washing treatment. The selected acid washing solution is a 2M dilute hydrochloric acid solution. After soaking for 12 hours, it is repeatedly centrifuged and washed with deionized water and ethanol until it becomes neutral. The obtained product is dried in a forced air drying oven at 80°C for 12 hours to obtain a hard carbon negative electrode material.
[0027] Comparative Example 4 Step 1: The biomass Salix psammophila was ultrasonically washed with deionized water for 6 hours to remove dust and impurities, and the obtained product was dried in a forced air drying oven at 60° C. for 24 hours to remove moisture; Step 2: Transfer the dried Salix psammophila to a muffle furnace, heat it to 300°C at a heating rate of 5°C / min in an air atmosphere and keep it for 2 hours, cool it naturally in the furnace and take it out, crush the pre-carbonized product into powder with a pulverizer for later use; Step 3: Put the pre-carbonized product into a tubular furnace, and under the protection of a reducing atmosphere, heat it from room temperature (20°C) to 1200°C at a heating rate of 5°C / min, keep it warm for 2 hours, cool it to room temperature at a cooling rate of 5°C / min with the furnace, take it out and grind it, and sieve it with a 325-mesh sieve; Step 4: The obtained powder is subjected to acid washing treatment. The selected acid washing solution is a 2M dilute hydrochloric acid solution. After soaking for 12 hours, it is repeatedly centrifuged and washed with deionized water and ethanol until it becomes neutral. The obtained product is dried in a forced air drying oven at 80°C for 12 hours to obtain a hard carbon negative electrode material.
[0028] The biomass-derived hard carbon material obtained in each embodiment and comparative example was evenly ground with acetylene black and sodium carboxymethyl cellulose (CMC) in a mass ratio of 8:1:1, and then an appropriate amount of deionized water was added to form a slurry, which was evenly coated on a copper foil with a coater, placed in a vacuum drying oven at 80°C for 12 hours, and then prepared into a disc electrode with a diameter of 12 mm using a punching machine.
[0029] The electrode sheet obtained above was used as the negative electrode, a glass fiber (Whitman, GF / D) disc with a diameter of 19 mm was used as the diaphragm, a sodium metal sheet with a diameter of 12 mm and a thickness of 0.2 mm was used as the counter electrode and the reference electrode, and the electrolyte was 1 mol / L sodium perchlorate / ethylene carbonate / dimethyl carbonate solution. The sodium ion battery was assembled according to the structure of the CR2016 standard button cell in a glove box filled with high-purity argon, and the battery was charged and discharged with a current density of 30 mA / g on a battery test platform.
[0030] Table 1 Main parameters and electrochemical properties of Examples 1-5 and Comparative Examples 1-2 Waste wood Pyrolysis temperature Pyrolysis atmosphere Initial specific capacity First coulombic efficiency Example 1 Salix psammophila 1400 Ar 276mAh / g 76.62% Example 2 Salix psammophila 600 <![CDATA[Ar+H 2 / With]]> 325mAh / g 80.84% Example 3 Salix psammophila 800 <![CDATA[Ar+H 2 / With]]> 300.8mAh / g 77.56% Example 4 Salix psammophila 1000 <![CDATA[Ar+H 2 / With]]> 284.6mAh / g 74.61% Example 5 Salix psammophila 1200 <![CDATA[Ar+H 2 / With]]> 264.1mAh / g 76.56% Comparative Example 1 Salix psammophila 600 <![CDATA[H 2 / With]]> 246.6mAh / g 30.48% Comparative Example 2 Salix psammophila 800 <![CDATA[H 2 / With]]> 282.1mAh / g 41.43% Comparative Example 3 Salix psammophila 1000 <![CDATA[H 2 / With]]> 212.5mAh / g 43.52% Comparative Example 4 Salix psammophila 1200 <![CDATA[H 2 / With]]> 186.7mAh / g 38.53%
[0031] Figure 1 The XRD diagrams shown show that the characteristic peaks of the materials of Examples 1, 2, 3, 4, and 5 at different pyrolysis temperatures are all around 23° and 43°, with no other obvious impurity peaks, corresponding to the (002) and (100) diffraction crystal planes, respectively, indicating that the materials are all amorphous carbon materials;
[0032] Figure 2 The Raman graphs shown show that the materials of Examples 1, 2, 3, 4, and 5 at different pyrolysis temperatures have a peak at 1350 cm -1 and 1580cm -1 There are two obvious characteristic peaks nearby, corresponding to the D peak and the G peak, indicating that the materials are amorphous carbon materials;
[0033] Figure 3 The charge-discharge curves shown in the figure show that the material of Example 2 shows an initial coulombic efficiency of 80.84% and an initial specific capacity of 325 mAh / g in the 0-2 V voltage region at a current density of 20 mA / g, and has a clear charge-discharge platform;
[0034] Figure 4 It can be seen from the cyclic voltammetry curve shown that Example 2 has a reduction peak at 0.25V in the first cycle, which is mainly due to the formation of the solid electrolyte interface film and some side reactions. The second and third cycles are basically overlapped, indicating that the sodium storage process is highly reversible;
[0035] Figure 5 The rate performance graph shown shows that the material of Example 2 exhibits good rate performance;
[0036] Figure 6 The SEM image shown shows the special pipeline structure of the material itself and the reduction of surface defects after reduction treatment.
[0037] The above-mentioned Examples 1-5 and Comparative Examples 1-4 are only preferred embodiments of the present invention, which describe the basic principles and features of the present invention. The present invention is not limited to the above-mentioned specific implementation methods. All improvements and optimizations made within the methods disclosed in the present invention are within the protection of the present invention.
Claims
1. A method for preparing a hard carbon negative electrode material for a sodium ion battery based on waste wood, comprising the following steps: Step 1: placing the waste wood in deionized water for ultrasonic washing pretreatment to remove surface dust and impurities, and placing the washed waste wood in a blast drying oven to dry, thereby obtaining a waste wood precursor; Step 2: The obtained waste wood precursor is transferred to a muffle furnace, carbonized in an air atmosphere, and placed in a grinder after natural cooling to grind into powder to obtain a pre-carbonized product; Step 3: Transfer the pre-carbonized product to an atmosphere furnace, perform high-temperature carbonization under the protection of an inert gas, and grind and sieve after natural cooling; Step 4: placing the treated hard carbon material in an acidic solution, then washing with deionized water and ethanol until neutral, placing the obtained product in a blast drying oven to dry, grinding and sieving, and obtaining a waste wood hard carbon material; Step 5: Transfer the waste wood hard carbon material to an atmosphere furnace, carbonize it under a reducing atmosphere, and sieve it after natural cooling to obtain the reduced waste wood hard carbon material.
2. The method according to claim 1, characterized in that: The waste wood raw material described in step 1 comes from Salix psammophila, the temperature of the blast drying oven is 80° C., and the drying time is 12 hours.
3. The method according to claim 2, characterized in that: The heating rate of the muffle furnace in step 2 is 5°C / min, the pyrolysis temperature is 300°C, and the holding time is 2 hours.
4. The method according to claim 3, characterized in that: In step 3, the inert gas for high-temperature carbonization is selected from nitrogen, argon, helium, and a mixture of hydrogen and argon (5% H2 + 95% Ar), the heating rate is 5°C / min, the pyrolysis temperature is 1400°C, the holding time is 2 hours, and the inert gas flow rate is 10-100CC / min. The cooling rate is maintained at 5°C / min.
5. The method according to claim 4, characterized in that: In step 4, the acidic solution is selected from one of dilute hydrochloric acid, dilute sulfuric acid or dilute nitric acid, the concentration of the acidic solution is 1-2 mol / L, the soaking time is 6-12 hours, the vacuum drying oven temperature is 80°C, and the drying time is 12 hours.
6. The method according to claim 5, characterized in that: In step 5, the heating rate of reduction carbonization is 5°C / min, the pyrolysis temperature is 600-1200°C, and the insulation time is 2 hours.
7. A sodium ion battery carbon negative electrode material, characterized in that: Prepared by any one of the methods of claims 1 to 6.
8. A hard carbon material electrode sheet, characterized in that: The sodium ion battery carbon negative electrode material according to claim 7 is evenly ground with acetylene black and sodium carboxymethyl cellulose in proportion, deionized water is added and magnetically stirred to obtain a uniformly mixed electrode slurry, the battery slurry is evenly coated on a copper foil with a coating machine, placed in a vacuum drying oven for vacuum drying for 12 hours, and then prepared into a disc electrode with a punching machine to obtain a hard carbon material electrode sheet.
9. The hard carbon material electrode sheet according to claim 8, characterized in that: The mass ratio of the hard carbon material, acetylene black and sodium carboxymethyl cellulose is 8:1:
1.
10. A sodium ion battery, characterized in that: Comprising the hard carbon material electrode sheet as described in claim 8 or 9.
Citation Information
Cited By
Preparation method of xylem-derived array type through pore channel structure hard carbon negative electrode material
CN119390041A
Short-range graphite and closed pore synergistic hard carbon negative electrode material and preparation method thereof
CN119528115A
Preparation method of hard carbon negative electrode material, hard carbon negative electrode material and battery
CN119735198A