Method for rapidly reducing phase transition temperature of vanadium dioxide

By dispersing vanadium dioxide nanopowder with sodium phosphate and potassium nitrate in a controlled chemical reaction, the phase transition temperature of VO2 is rapidly reduced to near room temperature, ensuring stability and suitability for industrial production.

CN119059559APending Publication Date: 2024-12-03INST FOR PROCESS MODELING & OPTIMIZATION JITRI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411484953.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing methods to reduce the phase transition temperature of vanadium dioxide (VO2) are complex, difficult to control, and unsuitable for large-scale production, often affecting the material's intrinsic properties and stability.

Method used

A method involving dispersing vanadium dioxide nanopowder in deionized water with sodium phosphate and potassium nitrate, adjusting pH, and reacting at controlled temperatures to produce oxygen vacancies, reducing the phase transition temperature to near room temperature.

Benefits of technology

The method effectively and controllably reduces the phase transition temperature of VO2 to near room temperature, maintaining its intrinsic properties and being suitable for industrial production without introducing impurities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059559A_ABST
    Figure CN119059559A_ABST
Patent Text Reader

Abstract

The invention discloses a method for rapidly reducing the phase transition temperature of vanadium dioxide, and the method specifically comprises the following steps: 1, dispersing vanadium dioxide nano-powder in deionized water with the mass fraction of 10-30%; 2, sodium phosphate accounting for 0.05-1% of the mass of the solution and potassium nitrate accounting for 1-5% of the mass of the solution are added, the pH of the solution is adjusted to 8, then the solution is transferred into a reaction kettle, a reaction is conducted for 1-3 h at the temperature of 400-600 DEG C, and then the temperature of the reaction kettle is reduced to 1-5 DEG C at the speed of 10 DEG C / min; and 3, taking out the solution, centrifuging, washing, and drying in vacuum to obtain the vanadium dioxide nano-powder with low phase transition temperature. By introducing potassium nitrate, decomposing to generate oxygen and adjusting oxygen vacancy, the phase transition temperature of VO2 is obviously reduced, the temperature can be reduced to be near the room temperature, and the actual application requirement is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of functional materials, in particular to a method for rapidly reducing the phase transition temperature of vanadium dioxide (VO2). Background Art

[0002] Vanadium dioxide (VO2) is a typical metal-insulator phase change material, which undergoes a reversible phase transition from low-temperature monoclinic system (semiconductor phase) to high-temperature tetragonal system (metal phase) at about 68°C. This phase transition is accompanied by significant changes in electrical, optical and structural properties, making VO2 have broad application prospects in the fields of smart windows, infrared detectors, optical switches and memory.

[0003] However, the high phase transition temperature of VO2 limits its development in practical applications. For example, in smart window applications, in order to achieve automatic dimming function at or near room temperature, the phase transition temperature of VO2 needs to be lowered to near room temperature. Therefore, how to effectively lower the phase transition temperature of VO2 has become the focus of researchers.

[0004] At present, the main methods to reduce the phase transition temperature of VO2 include: element doping method, which adjusts the phase transition temperature by introducing other transition metal elements (such as tungsten, molybdenum, chromium, etc.) into the VO2 lattice. Doping elements will affect the electronic structure and lattice parameters of VO2, thereby reducing the phase transition temperature. However, the doping method has the following shortcomings: 1. It is difficult to control doping, and the doping concentration and uniformity are difficult to accurately control, which may lead to unstable material properties; it affects the intrinsic properties, and doping may introduce impurity energy levels, affecting the optical and electrical properties of VO2 and reducing the phase transition characteristics; the process is complicated, and the doping process usually requires high temperature and high pressure conditions, the preparation process is complicated, and the cost is high; 2. Stress regulation method, by applying external stress or preparing thin films to change the lattice structure of VO2 and reduce the phase transition temperature. However, this method requires special equipment and conditions, and it is difficult to achieve large-scale production; 3. Nano size effect, using the size effect of VO2 at the nanoscale, the phase transition temperature can be reduced to a certain extent. However, the preparation and application of nanomaterials have problems such as particle agglomeration and poor stability.

[0005] In summary, the existing technology has many shortcomings in reducing the VO2 phase transition temperature, and a simple, effective and controllable method is urgently needed to achieve a rapid reduction in the VO2 phase transition temperature. Summary of the invention

[0006] The purpose of the present invention is to provide a method for rapidly reducing the phase transition temperature of vanadium dioxide, which has simple steps, is easy to operate and is suitable for industrial production.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] A method for rapidly reducing the phase transition temperature of vanadium dioxide comprises the following steps:

[0009] Step 1, dispersing vanadium dioxide nanopowder in deionized water with a mass fraction of 10 to 30%;

[0010] Step 2, adding 0.05-1% sodium phosphate and 1-5% potassium nitrate by mass of the solution, adjusting the pH of the solution to 8, then transferring the solution to a reactor, reacting at 400-600° C. for 1-3 hours, and then cooling the reactor to 1-5° C. at a rate of 10° C. / min;

[0011] Step three, taking out the solution, washing it after centrifugation and vacuum drying it to obtain vanadium dioxide nanopowder with a low phase transition temperature.

[0012] Preferably, the vanadium dioxide, sodium phosphate and potassium nitrate are all commercially available powders with a purity greater than 99%.

[0013] Preferably, in step one, the dispersing step is vacuum stirring, the stirring rate is 300 to 600 rpm, and the stirring time is 30 to 60 min.

[0014] Preferably, in step 2, the step of adjusting the pH of the solution is to dropwise add a sodium hydroxide solution with a concentration of 1 to 3 M.

[0015] Preferably, in step 2, the cooling step of the reactor is performed by adopting a circulating water cooling method above 200°C, with a chiller temperature of 10-20°C, and by adopting a refrigerator below 200°C, with a refrigerator temperature of -5--1°C.

[0016] Preferably, in step three, the centrifugal speed is 5000-7200 rpm, the centrifugal time is 15-30 min, deionized water and isopropanol are used for washing 3 times respectively, and the vacuum drying temperature is 40-50°C.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] 1. Rapidly reduce the phase transition temperature: By introducing potassium nitrate, decomposing it to produce oxygen, adjusting oxygen vacancies, and significantly reducing the phase transition temperature of VO2, it can be reduced to near room temperature to meet practical application needs.

[0019] 2. The process is simple and controllable: it uses conventional chemical reaction equipment and conditions, the process flow is simple, the reaction conditions can be precisely controlled, and it is suitable for industrial production.

[0020] 3. Protect the valence state of VO2: The nitrous acid produced by the decomposition of potassium nitrate acts as a reducing agent to prevent the valence state of VO2 from changing and maintain the intrinsic properties of the material.

[0021] 4. Avoid side effects of doping: There is no need to introduce other doping elements, thus avoiding performance instability and material degradation problems that may be caused by doping. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a bar chart comparing the minimum phase transition temperatures of the coatings prepared in Examples 1, 2, 3 and the comparative example. DETAILED DESCRIPTION

[0023] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0024] Example 1

[0025] Take 20 grams of vanadium dioxide nanopowder with a purity greater than 99%, add it to deionized water, adjust the mass fraction to 20%, and stir at a stirring rate of 400 rpm for 45 minutes under vacuum conditions to form a uniform dispersion.

[0026] In the dispersion, add 0.5% sodium phosphate and 2% potassium nitrate by mass of the solution. Add 2M sodium hydroxide solution dropwise to adjust the system pH to 8. Transfer the solution to the reactor and react at 500°C for 2 hours. After the reaction is completed, cool the reactor to 3°C at a cooling rate of 10°C / min. The cooling method is: above 200°C: use the circulating water cooling method, the chiller temperature is 15°C; below 200°C: use the refrigerator to cool, the refrigerator temperature is -3°C.

[0027] The solution was taken out, centrifuged at 6000 rpm for 20 minutes, washed with deionized water and isopropanol three times respectively, and finally dried at 45°C under vacuum conditions to obtain vanadium dioxide nanopowder with a phase transition temperature of 26°C.

[0028] Example 2

[0029] Take 15 grams of vanadium dioxide nanopowder with a purity greater than 99%, add it to deionized water, adjust the mass fraction to 15%, and stir at a stirring rate of 500 rpm for 30 minutes under vacuum conditions to form a uniform dispersion.

[0030] In the dispersion, add 0.1% sodium phosphate and 3% potassium nitrate by mass of the solution. Add 1.5M sodium hydroxide solution dropwise to adjust the system pH to 8. Transfer the solution to the reactor and react at 450°C for 3 hours. After the reaction is completed, cool the reactor to 2°C at a cooling rate of 10°C / min. The cooling method is: above 200°C: use the circulating water cooling method, the chiller temperature is 18°C; below 200°C: use the refrigerator to cool, the refrigerator temperature is -2°C.

[0031] The solution was taken out, centrifuged at 7000 rpm for 25 minutes, washed with deionized water and isopropanol three times respectively, and finally dried at 50° C. under vacuum conditions to obtain vanadium dioxide nanopowder with a phase transition temperature of 28° C.

[0032] Example 3

[0033] Take 25 grams of vanadium dioxide nanopowder with a purity greater than 99%, add it to deionized water, adjust the mass fraction to 25%, and stir at a stirring rate of 350 rpm for 60 minutes under vacuum conditions to form a uniform dispersion.

[0034] In the dispersion, add 1% sodium phosphate and 5% potassium nitrate by mass of the solution. Add 3M sodium hydroxide solution dropwise to adjust the system pH to 8. Transfer the solution to the reactor and react at 600℃ for 1 hour. After the reaction, cool the reactor to 5℃ at a cooling rate of 10℃ / min. The cooling method is: above 200℃: use the circulating water cooling method, the chiller temperature is 10℃; below 200℃: use the refrigerator to cool, the refrigerator temperature is -1℃.

[0035] The solution was taken out, centrifuged at 5000 rpm for 15 minutes, washed with deionized water and isopropanol three times respectively, and finally dried at 40°C under vacuum conditions to obtain vanadium dioxide nanopowder with a phase transition temperature of 27°C.

[0036] Comparative Example

[0037] Take 25 grams of vanadium dioxide nanopowder with a purity greater than 99%, add it to deionized water, adjust the mass fraction to 25%, and stir at a stirring rate of 350 rpm for 60 minutes under vacuum conditions to form a uniform dispersion.

[0038] Add 1% sodium phosphate by mass to the dispersion. Add 3M sodium hydroxide solution dropwise to adjust the pH of the system to 8. Transfer the solution to the reactor and react at 600°C for 1 hour. After the reaction, cool the reactor to 5°C at a cooling rate of 10°C / min. The cooling method is: above 200°C: use the circulating water cooling method, the chiller temperature is 10°C; below 200°C: use the refrigerator to cool, the refrigerator temperature is -1°C.

[0039] The solution was taken out, centrifuged at 5000 rpm for 15 minutes, washed with deionized water and isopropanol three times respectively, and finally dried at 40°C under vacuum conditions to obtain vanadium dioxide nanopowder with a phase transition temperature of 67°C.

[0040] Figure 1 It is a phase transition temperature line graph of vanadium dioxide nanopowders prepared in Examples 1, 2, 3 and Comparative Example.

[0041] like Figure 1 As shown, the phase transition temperatures of Examples 1, 2, and 3 are all close to room temperature, while the phase transition temperature of the comparative example is 67°C, and the final phase transition temperature is close to the original VO2 phase transition temperature. In summary, the present invention adjusts the oxygen vacancies in VO2 by adding potassium nitrate and utilizing its decomposition at high temperature to produce oxygen. At the same time, the generated nitrous acid acts as a reducing agent to protect the valence state of VO2, thereby achieving a rapid reduction in the VO2 phase transition temperature. The method is simple and easy to implement, has significant effects, and has good application prospects.

[0042] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for rapidly reducing the phase transition temperature of vanadium dioxide, characterized in that: The phase transition temperature is lowered by controlling and adjusting oxygen vacancies, which specifically includes the following steps: Step 1, dispersing vanadium dioxide nanopowder in deionized water with a mass fraction of 10 to 30%; Step 2, adding 0.05-1% sodium phosphate and 1-5% potassium nitrate by mass of the solution, adjusting the pH of the solution to 8, then transferring the solution to a reactor, reacting at 400-600° C. for 1-3 hours, and then cooling the reactor to 1-5° C. at a rate of 10° C. / min; Step three, taking out the solution, washing it after centrifugation and vacuum drying it to obtain vanadium dioxide nanopowder with a low phase transition temperature.

2. A method for rapidly reducing the phase transition temperature of vanadium dioxide according to claim 1, characterized in that: The vanadium dioxide, sodium phosphate and potassium nitrate are all commercially available powders with a purity greater than 99%.

3. A method for rapidly reducing the phase transition temperature of vanadium dioxide according to claim 1, characterized in that: In step 1, the dispersing step is vacuum stirring, the stirring rate is 300-600 rpm, and the stirring time is 30-60 min.

4. A method for rapidly reducing the phase transition temperature of vanadium dioxide according to claim 1, characterized in that: In step 2, the step of adjusting the pH of the solution is to dropwise add a sodium hydroxide solution with a concentration of 1 to 3 M.

5. A method for rapidly reducing the phase transition temperature of vanadium dioxide according to claim 1, characterized in that: In step 2, the reaction kettle is cooled by circulating water above 200°C, with a chiller temperature of 10-20°C, and by a refrigerator below 200°C, with a refrigerator temperature of -5--1°C.

6. A method for rapidly reducing the phase transition temperature of vanadium dioxide according to claim 1, characterized in that: In step 3, the centrifugal speed is 5000-7200 rpm, the centrifugal time is 15-30 min, deionized water and isopropanol are used for washing 3 times respectively, and the vacuum drying temperature is 40-50°C.

Citation Information

Cited By

  • Method for preparing M-phase vanadium dioxide at low temperature and reducing phase change temperature of M-phase vanadium dioxide

    CN120271042A