Micron-sized ternary precursor and preparation method thereof, positive electrode active material and lithium ion battery

Through the mixing and pyrolysis of high-concentration metal salt and dispersant, the problem of hollow shell particles of ternary precursors in spray pyrolysis is solved, and an excellent micron-scale ternary precursor is prepared, which improves the electrical power of lithium-ion batteries. Chemical properties and production efficiency.

CN119059578APending Publication Date: 2024-12-03BEIJING MINING & METALLURGICAL TECH GRP CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411529436.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing spray pyrolysis method to prepare ternary precursor materials easily form empty shell particles, affecting performance.

Method used

Nickel salt, cobalt salt, manganese salt and dispersant are mixed at high concentrations, and after ball milling and pyrolysis, the pyrolysis temperature and temperature gradient are controlled to form a micron-scale ternary precursor with high spherical morphology and low empty shell rate.

Benefits of technology

A ternary precursor with uniform particle size distribution, high spherical shape and low empty shell rate was prepared to simplify the process flow, reduce production costs, and improve electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059578A_ABST
    Figure CN119059578A_ABST
Patent Text Reader

Abstract

The invention provides a micron-sized ternary precursor and a preparation method thereof, a positive electrode active material and a lithium ion battery, and relates to the field of lithium ion batteries. The preparation method of the micron-sized ternary precursor comprises the following steps: mixing nickel salt, cobalt salt, manganese salt, a dispersing agent and water to obtain a dispersion system; carrying out atomization treatment on the dispersion system to form dispersion liquid drops; performing pyrolysis on the dispersion liquid drops to obtain a ternary precursor; wherein the total metal concentration of the nickel salt, the cobalt salt and the manganese salt in the dispersion system is 300-450 g / L. According to the preparation method, the ternary precursor with high sphericity, low empty shell rate and uniform particle size distribution can be prepared. In addition, the method is simple in technological process and easy to operate. In addition, the ternary precursor is prepared by using a high-concentration metal salt dispersion system, so that the evaporation energy consumption of water can be effectively reduced, and the production cost can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of lithium-ion batteries, and in particular to a micron-sized ternary precursor and a preparation method thereof, a positive electrode active material and a lithium-ion battery. Background Art

[0002] As ternary cathode materials develop towards high nickel and single crystals, the traditional co-precipitation method for preparing ternary precursors has shortcomings such as consuming a large amount of acid and alkali and a long preparation time, resulting in very slow technological progress. Spray pyrolysis has the advantage of short preparation time and is a technology with great development potential and application prospects. However, ternary cathode materials prepared by spray pyrolysis are prone to form empty shell particles, and even breakage and adhesion, which greatly affects the performance of ternary precursors. Summary of the invention

[0003] The purpose of the present application is to provide a micron-sized ternary precursor and a preparation method thereof, a positive electrode active material and a lithium-ion battery, so as to solve the problem of a high proportion of empty shell particles in the existing spray pyrolysis preparation of ternary precursor materials, and to prepare a ternary precursor powder with high sphericity and low empty shell ratio.

[0004] To achieve the above objectives, this application adopts the following technical solutions: A method for preparing a micron-sized ternary precursor comprises: Mixing nickel salt, cobalt salt, manganese salt, dispersant and water to obtain a dispersed system; atomizing the dispersed system to form dispersed droplets; pyrolyzing the dispersed droplets to obtain a micrometer-sized ternary precursor; Wherein, the total metal concentration of the nickel salt, the cobalt salt and the manganese salt in the dispersed system is 300-450 g / L.

[0005] According to an embodiment of the present application, the nickel salt includes at least one of nickel nitrate and nickel acetate; The cobalt salt includes at least one of cobalt nitrate and cobalt acetate; The manganese salt includes at least one of manganese nitrate and manganese acetate; And / or, when preparing the dispersed system, the anion of the nickel salt is the same as the anion of the cobalt salt and the anion of the manganese salt.

[0006] According to an embodiment of the present application, the dispersant includes at least one of citric acid, glucose, and ethylene glycol; And / or, the mass of the dispersant accounts for 1-15% of the total mass of the nickel salt, the cobalt salt and the manganese salt.

[0007] According to an embodiment of the present application, mixing nickel salt, cobalt salt, manganese salt, dispersant and water includes: ball milling the nickel salt, cobalt salt, manganese salt, dispersant and water in a ball mill to prepare a dispersed system, and after the ball milling, more than 90% of the particles in the dispersed system have a size of 3~15 μm.

[0008] According to an embodiment of the present application, the pyrolysis temperature is 100-500°C.

[0009] According to an embodiment of the present application, the pyrolysis is carried out in a pyrolysis device, which includes a feeding section, a discharging section, and a heating section located between the feeding section and the discharging section; the temperature of the feeding section is controlled at 100-300°C, the temperature of the heating section is controlled at 200-500°C, the temperature of the discharging section is controlled at 100-300°C, the temperature of the feeding section is lower than the temperature of the heating section, and the temperature of the heating section is higher than the temperature of the discharging section.

[0010] The present application also provides a micron-sized ternary precursor, which is prepared by the preparation method of the micron-sized ternary precursor described above.

[0011] According to an embodiment of the present application, the empty shell ratio of the micron-sized ternary precursor is <10%; And / or, the D of the micron-sized ternary precursor 50 Particle size is 2~20 μm; And / or, the sphericity of the micron-sized ternary precursor is 0.8~1.

[0012] The present application also provides a positive electrode active material, and the raw materials for preparing the positive electrode active material include the micron-sized ternary precursor mentioned above.

[0013] The present application also provides a lithium-ion battery, which includes the positive electrode active material described above.

[0014] Compared with the prior art, the beneficial effects of this application include: The present application can prepare a micron-sized ternary precursor with high sphericity, low empty shell ratio and uniform particle size distribution. Moreover, the method of the present application has a simple process flow and convenient production operation. In addition, the present application uses a high-concentration metal salt dispersion system to prepare the ternary precursor, which can effectively reduce the energy consumption of water evaporation and reduce production costs.

[0015] The micron-sized ternary precursor, positive electrode active material and lithium-ion battery of the present application all have excellent electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0017] Figure 1 This is the SEM image of the ternary precursor prepared in Example 1; Figure 2 This is the SEM image of the ternary precursor prepared in Example 2; Figure 3 This is the SEM spectrum of the ternary precursor prepared in Comparative Example 1; Figure 4 This is the SEM spectrum of the ternary precursor prepared in Comparative Example 2; Figure 5 This is the SEM spectrum of the ternary precursor prepared in Comparative Example 3; Figure 6 This is a photograph of the suspension in Comparative Example 4. DETAILED DESCRIPTION

[0018] As used herein: "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0019] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0020] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range.

[0021] In these examples, parts and percentages are by mass unless otherwise indicated.

[0022] "Mass parts" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass parts of component A are a parts and the mass parts of component B are b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass parts of all components is not limited to 100 parts.

[0023] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0024] In order to better explain the technical solution provided by this application, before the embodiments, the technical solution is first described as a whole, as follows: The present application provides a method for preparing a micron-sized ternary precursor, comprising: Mixing nickel salt, cobalt salt, manganese salt, dispersant and water to obtain a dispersed system; atomizing the dispersed system to form dispersed droplets; pyrolyzing the dispersed droplets to obtain a micrometer-sized ternary precursor; Wherein, the total metal concentration of the nickel salt, the cobalt salt and the manganese salt in the dispersed system is 300-450 g / L.

[0025] For example, the total metal concentration of the nickel salt, the cobalt salt and the manganese salt in the dispersed system can be 300 g / L, 305 g / L, 310 g / L, 315 g / L, 320 g / L, 325 g / L, 330 g / L, 335 g / L, 340 g / L, 350 g / L, 400 g / L, 450 g / L or any value between 300 and 450 g / L.

[0026] According to an embodiment of the present application, the nickel salt includes at least one of nickel nitrate and nickel acetate; The cobalt salt includes at least one of cobalt nitrate and cobalt acetate; The manganese salt includes at least one of manganese nitrate and manganese acetate; and / or, when preparing the dispersed system, the anion of the nickel salt is the same as the anion of the cobalt salt and the anion of the manganese salt; The contents of the nickel salt, the cobalt salt and the manganese salt can be selected according to the molar amounts of nickel, cobalt and manganese in the target product micron-sized ternary precursor. For example, the ratio of the molar amount of nickel in the nickel salt to the molar amount of cobalt in the cobalt salt and the molar amount of manganese in the manganese salt includes but is not limited to 5:2:3, 6:2:2, and 8:1:1.

[0027] According to an embodiment of the present application, the dispersant includes at least one of citric acid, glucose, and ethylene glycol; thereby, solid particles and water molecules can be effectively dispersed, so that the dispersed system can still maintain good fluidity at a higher concentration, which helps to enter the atomization device and be atomized into droplets.

[0028] And / or, the mass of the dispersant accounts for 1-15% of the total mass of the nickel salt, the cobalt salt, and the manganese salt. This helps the particles after atomization and pyrolysis to maintain better sphericity. If the amount of dispersant added is too low, the fluidity of the dispersed system after ball milling will be poor, resulting in poor atomization effect; if the amount of dispersant added is too high, the cost of auxiliary materials and the energy consumption of pyrolysis will increase.

[0029] For example, the mass of the dispersant accounts for 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15% or any value between 1 and 15% of the total mass of the nickel salt, the cobalt salt, and the manganese salt.

[0030] According to an embodiment of the present application, mixing nickel salt, cobalt salt, manganese salt, dispersant and water includes: ball milling nickel salt, cobalt salt, manganese salt, dispersant and water in a ball mill to prepare a dispersed system. The diameter of the solid particles can be controlled by controlling parameters such as the particle size of the small balls, the rotation speed, and the ball milling time, so that more than 90% of the particles in the dispersed system after ball milling have a size of 3 to 15 μm, which is helpful for subsequent spray pyrolysis to obtain micron-sized ternary precursor powder. If the particle size in the dispersed system after ball milling is too large, the particle size of the precursor powder prepared subsequently will be too large.

[0031] Exemplarily, the ball milling process uses balls with a size of 1 to 5 μm, the ball milling speed is controlled at 100 to 500 rpm, and the ball milling process lasts for 2 to 24 hours.

[0032] Furthermore, the atomization process is carried out in an atomizer. The dispersed system can be delivered to the atomizer by a feed pump, and the dispersed system is atomized to form tiny droplets in the atomizer.

[0033] According to an embodiment of the present application, the pyrolysis temperature is 100-500° C. The dispersed droplets undergo evaporation, drying, pyrolysis, crystallization and other processes in the pyrolysis device under the action of the airflow, and the ternary precursor powder is obtained through the powder collection device.

[0034] According to an embodiment of the present application, the pyrolysis is carried out in a pyrolysis device, which includes a feeding section, a discharging section, and a heating section located between the feeding section and the discharging section; the temperature of the feeding section is controlled at 100-300°C, the temperature of the heating section is controlled at 200-500°C, the temperature of the discharging section is controlled at 100-300°C, the temperature of the feeding section is lower than the temperature of the heating section, and the temperature of the heating section is higher than the temperature of the discharging section.

[0035] Specifically, by controlling the temperature of the feeding section to be lower than the temperature of the heating section, it is possible to avoid the occurrence of undesirable problems such as excessive evaporation and pyrolysis caused by the excessively high temperature of the feeding section, which in turn leads to an increase in the powder breakage rate. By controlling the temperature of the heating section to be higher than the temperature of the discharging section, the pyrolysis time of the particles can be extended to allow for full formation, and it is also possible to avoid the problem of water vapor condensation and destruction of the powder structure due to too low a temperature.

[0036] For example, the temperature of the feed section can be 100°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 300°C or any value between 100-300°C.

[0037] The temperature of the heating section can be 200°C, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 400°C, 450°C, 500°C or any value between 200-500°C.

[0038] The temperature of the discharging section can be 100°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 300°C or any value between 100-300°C.

[0039] The present application also provides a micron-sized ternary precursor, which is prepared by the preparation method of the micron-sized ternary precursor described above.

[0040] According to an embodiment of the present application, the empty shell ratio of the ternary precursor is <10%; "Empty shell ratio" refers to the proportion of the hollow part of the ternary precursor particles in the prepared product. Specifically, the empty shell ratio is calculated in the following way: the ternary precursor particles are cross-sectioned, the sample section is observed using a scanning microscope, and more than 200 particles in the field of view are counted. The empty shell ratio is calculated by converting the diameter of the hollow part and the particle diameter into volume.

[0041] For example, the shell fraction of the ternary precursor may be 1%, 2%, 3%, 4%, 5%, 6%, 6.5%, 7%, 8%, 9% or 9.2%, or any value less than 10%.

[0042] And / or, the D of the micron-sized ternary precursor 50 The particle size is 2~20 μm.

[0043] Further, the micron-sized ternary precursor of the present application is a spherical or quasi-spherical particle. The sphericity of the micron-sized ternary precursor of the present application is 0.8-1. Specifically, the sphericity is measured and calculated based on the data obtained by scanning electron microscopy combined with image analysis software, using the diameter method to measure and calculate, and taking the ratio of the particle's circumference equivalent diameter to the particle's area equivalent diameter as the sphericity, and taking the average value of at least 200 particles, which is the sphericity of the micron-sized ternary precursor.

[0044] For example, the sphericity of the micron-sized ternary precursor can be 0.8, 0.84, 0.85, 0.9, 0.97, 1 or any value between 0.8-1.

[0045] The present application also provides a positive electrode active material, and the raw materials for preparing the positive electrode active material include the micron-sized ternary precursor mentioned above.

[0046] Furthermore, the positive electrode active material is obtained by solid phase sintering of a micron-sized ternary precursor and a lithium source.

[0047] The present application also provides a lithium-ion battery, which includes the positive electrode active material described above.

[0048] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0049] 1. Preparation of micron-sized ternary precursors Example 1 Embodiment 1 provides a micron-sized ternary precursor, and the preparation method thereof comprises the following steps: 89 g of nickel acetate, 15 g of cobalt acetate, 44.5 g of manganese acetate and 15 g of citric acid (the mass of the dispersant accounts for 10% of the total mass of the nickel salt, the cobalt salt and the manganese salt) and 60 g of water are put into a ball mill, 200 g of 2-3 μm small balls are added, and the ball mill is sealed for 8 h. The speed is selected to be 280 rpm. After ball milling, more than 90% of the particles in the dispersed system have a size of 3-15 μm, forming a uniform flowable suspension, and the total metal concentration of nickel, cobalt and manganese in the suspension is 335 g / L.

[0050] A peristaltic pump was used to feed the material into the atomizing spray gun at a feed rate of 120 mL / h. The droplets were evaporated, dried, and pyrolyzed in the pyrolysis furnace. The pyrolysis temperatures were set at 200°C, 300°C, and 200°C from the feed section to the heating section and the discharge end. Micron-sized ternary precursor powder was collected from the discharge section.

[0051] The SEM spectrum of the ternary precursor powder prepared in Example 1 is as follows: Figure 1 As shown by Figure 1 It can be seen that the ternary precursor prepared in Example 1 is spherical particles with good density.

[0052] The empty shell ratio of the ternary precursor prepared in Example 1 is 6.5%. 50 The particle size is 12.8 μm and the sphericity is 0.84.

[0053] Example 2 Embodiment 2 provides a micron-sized ternary precursor, and the preparation method thereof comprises the following steps: Nickel nitrate, cobalt nitrate and manganese nitrate were weighed according to a metal atomic molar ratio of 8:1:1, and 5% of glucose and 30% of pure water accounting for the total mass of nickel nitrate, cobalt nitrate and manganese nitrate were added. The mixture was stirred for 4 h until completely dissolved. The stirring rate was selected to be 320 rpm to form a uniform solution with a total metal concentration of nickel, cobalt and manganese of 305 g / L.

[0054] A peristaltic pump was used to feed the material into the atomizing spray gun at a feed rate of 100 mL / h. The droplets were evaporated, dried, and pyrolyzed in the pyrolysis furnace. The pyrolysis temperatures were set at 180°C, 280°C, and 240°C from the feed section to the heating section and the discharge section. Micron-sized ternary precursor powder was collected from the discharge section.

[0055] The SEM spectrum of the ternary precursor powder prepared in Example 2 is as follows: Figure 2 As shown by Figure 2 It can be seen that the ternary precursor product prepared in Example 2 is spherical particles with good particle size distribution uniformity.

[0056] The empty shell ratio of the ternary precursor prepared in Example 2 is 9.2%. 50 The particle size is 7.6 μm and the sphericity is 0.97.

[0057] Comparative Example 1 The only difference from Example 2 is that no glucose is added in Comparative Example 1.

[0058] The SEM spectrum of the ternary precursor prepared in Comparative Example 1 is as follows: Figure 3 As shown by Figure 3 It can be seen that the product particles of Comparative Example 1 are obviously broken and adhered, and the powder quality of the ternary precursor of Comparative Example 1 is significantly lower than that of Example 2.

[0059] The empty shell ratio of the ternary precursor prepared in Comparative Example 1 is 12.9%, and the D 50 The particle size is 57 μm and the sphericity is 0.57.

[0060] Comparative Example 2 The only difference from Example 1 is that in Comparative Example 2, 300 g of water is added to prepare a uniform solution, and the total metal concentration of nickel, cobalt and manganese in the solution of Comparative Example 2 is 100 g / L.

[0061] The SEM spectrum of the ternary precursor prepared in Comparative Example 2 is as follows: Figure 4 As shown by Figure 4 It can be seen that the ternary precursor particles prepared in Comparative Example 2 have an obvious hollow structure, and the solidity of the ternary precursor prepared in Comparative Example 2 is significantly lower than that in Example 1.

[0062] The empty shell ratio of the ternary precursor prepared in Comparative Example 2 is 34.5%, and the D 50 The particle size is 7.2 μm and the sphericity is 0.96.

[0063] Comparative Example 3 The only difference from Example 1 is that in Comparative Example 3, the pyrolysis temperatures from the feeding section to the heating section and the discharging section are set to 400° C., 600° C., and 400° C. respectively.

[0064] The SEM spectrum of the ternary precursor prepared in Comparative Example 3 is as follows: Figure 5 As shown, it can be seen that the sphericity of the ternary precursor prepared in Comparative Example 3 is significantly reduced compared to Example 1.

[0065] The empty shell ratio of the ternary precursor prepared in Comparative Example 3 is 7.4%, and the D 50 The particle size is 9.3 μm and the sphericity is 0.73.

[0066] Comparative Example 4 The only difference from Example 1 is that in Comparative Example 4, 30 g of water is added to prepare a suspension, and the total concentration of nickel, cobalt and manganese metals in the suspension of Comparative Example 4 is 460 g / L.

[0067] like Figure 6 As shown, the viscosity of the suspension in Comparative Example 4 is extremely high, and the fluidity is poor, so it cannot enter the atomization process.

[0068] 2. Performance Test The positive electrode active materials were prepared by using the ternary precursors of Examples 1-2 and Comparative Examples 1-3. The specific preparation process was as follows: the nickel-cobalt-manganese ternary precursors prepared in Examples 1-2 and Comparative Examples 1-3 were fully mixed with lithium carbonate, and then calcined at 850° C. for 15 h. After crushing and screening, D 50 Ternary positive electrode active material powder with a particle size of 2-20 μm.

[0069] The button-type half-cell was prepared using the positive electrode active material. The prepared button-type half-cell was tested under the conditions of 3.0-4.3 V, 25°C, and 0.1C charge and discharge. The test results are shown in Table 1.

[0070] Table 1 Electrochemical performance test results of positive electrode active materials of embodiments and comparative examples

[0071] It can be seen from Table 1 that the electrochemical performance of the button-type half-cell prepared in the embodiment is significantly better than that of the button-type half-cell prepared in the comparative example. Specifically, the button-type half-cell prepared in the embodiment has a first discharge specific capacity greater than 170 mAh / g, and a first charge and discharge efficiency greater than 85%; while the button-type half-cell prepared in the comparative example, under the same conditions, has a first discharge specific capacity less than 170 mAh / g, and a first charge and discharge efficiency less than 80%.

[0072] It can be seen from the test results that the ternary precursor prepared in this application can meet the requirements of positive electrode materials.

[0073] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

[0074] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. A method for preparing a micron-sized ternary precursor, characterized in that: include: Mixing nickel salt, cobalt salt, manganese salt, dispersant and water to obtain a dispersed system; atomizing the dispersed system to form dispersed droplets; pyrolyzing the dispersed droplets to obtain a micrometer-sized ternary precursor; Wherein, the total metal concentration of the nickel salt, the cobalt salt and the manganese salt in the dispersed system is 300-450 g / L.

2. The method for preparing a micron-sized ternary precursor according to claim 1, characterized in that: The nickel salt includes at least one of nickel nitrate and nickel acetate; The cobalt salt includes at least one of cobalt nitrate and cobalt acetate; The manganese salt includes at least one of manganese nitrate and manganese acetate; And / or, when preparing the dispersed system, the anion of the nickel salt is the same as the anion of the cobalt salt and the anion of the manganese salt.

3. The method for preparing a micron-sized ternary precursor according to claim 1, characterized in that: The dispersant includes at least one of citric acid, glucose, and ethylene glycol; And / or, the mass of the dispersant accounts for 1-15% of the total mass of the nickel salt, the cobalt salt and the manganese salt.

4. The method for preparing a micron-sized ternary precursor according to claim 1, characterized in that: Mixing nickel salt, cobalt salt, manganese salt, dispersant and water includes: ball milling the nickel salt, cobalt salt, manganese salt, dispersant and water in a ball mill to prepare a dispersed system, and after the ball milling, more than 90% of the particles in the dispersed system have a size of 3-15 μm.

5. The method for preparing a micron-sized ternary precursor according to claim 1, characterized in that: The pyrolysis temperature is 100-500°C.

6. The method for preparing a micron-sized ternary precursor according to claim 5, characterized in that: The pyrolysis is carried out in a pyrolysis device, which includes a feeding section, a discharging section, and a heating section located between the feeding section and the discharging section; the temperature of the feeding section is controlled at 100-300°C, the temperature of the heating section is controlled at 200-500°C, the temperature of the discharging section is controlled at 100-300°C, the temperature of the feeding section is lower than the temperature of the heating section, and the temperature of the heating section is higher than the temperature of the discharging section.

7. A micron-sized ternary precursor, characterized in that: The micron-sized ternary precursor is prepared by the method for preparing a micron-sized ternary precursor according to any one of claims 1-6.

8. The micron-sized ternary precursor according to claim 7, characterized in that: The empty shell ratio of the micron-sized ternary precursor is less than 10%; And / or, the D of the micron-sized ternary precursor 50 Particle size is 2~20 μm; And / or, the sphericity of the micron-sized ternary precursor is 0.8~1.

9. A positive electrode active material, characterized in that: The raw material for preparing the positive electrode active material includes the micron-sized ternary precursor according to claim 7 or 8.

10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode active material according to claim 9.