Preparation method of modified attapulgite water-retaining slow-release fertilizer

By modifying the concave and convex rod soil to wrap urea particles, forming an inner and outer envelope structure, and using its crosslinking network structure to improve the water absorption and slow release performance of fertilizers, solving the problems of low utilization rate of existing fertilizers and insufficient slow release performance, realizing the problem of low water resource utilization rate and insufficient slow release performance of existing fertilizers. Efficient fertilizer utilization and low cost fertilizer efficiency extension.

CN119059849AInactive Publication Date: 2024-12-03HEBEI WUXINGYUAN AGRI TECH DEV GRP CO LTD

Patent Information

Application Number
CN202411195941.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing fertilizers are difficult to effectively improve the utilization rate of water resources and fertilizers, and their sustained release performance is insufficient, which cannot be consistent with plant nutrient requirements.

Method used

Modified concave and convex rod soil as raw material, and by forming an inner and outer envelope structure, urea particles are wrapped in the copolymer of the concave and concave and concave and concave and concave and concave and concave and concave and concave and concave, to form a water-absorbent and water-retaining outer envelope and The sustained release inner envelope uses the Michael addition reaction and hydrolysis reaction of aminated concave and convex rod soil with 4-vinylbenzonitrile to form nitrilated and carboxylated concave and concave and concave and concave soil, and combines hydroxymethylurea to form a crosslinking network. Structure to improve water retention and sustained release properties.

Benefits of technology

The efficient water absorption and sustained release performance of modified concave and convex rod soil water-retaining and slow-release fertilizer is achieved, extending the fertilizer efficiency period, and improving the utilization rate and cost-effectiveness of fertilizers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of fertilizers, and discloses a preparation method of a modified attapulgite water-retaining slow-release fertilizer, which comprises the following steps: preparing attapulgite modified urea formaldehyde by using aminated attapulgite, 4-vinylbenzonitrile, hydroxymethyl urea and the like as raw materials, and preparing a modified attapulgite water-retaining slow-release fertilizer by using maleic anhydride, sodium p-styrenesulfonate, aminated attapulgite and the like as raw materials. Urea particles are used as an inner core carrier, the attapulgite modified urea formaldehyde is used as an inner layer, the attapulgite modified maleic anhydride-sodium p-styrenesulfonate copolymer is used as an outer layer, and the attapulgite modified maleic anhydride-sodium p-styrenesulfonate composite material is prepared by using the urea particles as the inner core carrier, the attapulgite modified urea formaldehyde as the inner layer and the attapulgite modified maleic anhydride-sodium p-styrenesulfonate copolymer as the outer layer. The prepared modified attapulgite water-retaining slow-release fertilizer has better water-retaining property and slow-release effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fertilizers, in particular to a method for preparing a modified attapulgite water-retaining slow-release fertilizer. Background Art

[0002] Modern agriculture is characterized by low input, high output, high efficiency and sustainable development. The fertilizer industry and water resource utilization closely related to this are the important material basis for modern agricultural production and development. Therefore, how to improve the utilization rate of water resources and fertilizers is crucial. One of the ways to improve fertilizer utilization is to use slow-release fertilizers. Slow-release fertilizers refer to fertilizers that can slowly release nutrients and whose release pattern is consistent with the nutrient requirements of plants. Attapulgite is a type of natural hydrated magnesium-rich silicate clay mineral with a large number of hydrophilic hydroxyl groups distributed on the surface. It has excellent dispersibility, plasticity and other properties. And because attapulgite itself contains a variety of mineral nutrients and trace elements, using it as a fertilizer can improve soil fertility.

[0003] Based on this, the present invention provides a method for preparing a modified attapulgite water-retaining slow-release fertilizer. With attapulgite as a raw material, attapulgite-modified urea formaldehyde and attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer are prepared, and the urea is wrapped using the attapulgite as an inner membrane and an outer membrane. The fertilizer has good water-retaining performance and slow-release performance, and can be widely used in the field of fertilizers. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] Therefore, the present invention provides a method for preparing a modified attapulgite water-retaining slow-release fertilizer, and the prepared fertilizer has good water absorption and water-retaining properties and slow-release properties.

[0006] (II) Technical solution

[0007] A preparation method of a modified attapulgite water-retaining slow-release fertilizer, the preparation method comprising: adding urea particles with a particle size of 2-4 mm into a disc granulator, spraying a polyvinyl alcohol binder with a mass fraction of 4% onto the surface of the urea until a layer of binding liquid is formed on the surface of the urea, adding attapulgite-modified urea formaldehyde into the granulator to form an inner film, spraying a polyvinyl alcohol binder with a mass fraction of 4% into the granulator to form a layer of binding liquid on the surface of the inner film, and finally adding attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer into the granulator, and drying to obtain the modified attapulgite water-retaining slow-release fertilizer.

[0008] Preferably, the usage ratio of the urea granules, the attapulgite-modified urea formaldehyde, and the attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer is 100 g:(25-40) g:(50-80) g.

[0009] Preferably, the preparation method of the attapulgite-modified urea formaldehyde is:

[0010] Step (1), under nitrogen conditions, adding aminated attapulgite and 4-vinylbenzonitrile to a methanol solvent, stirring and dispersing, reacting at 20-35° C. for 4-6 days, filtering after the reaction, extracting with methanol, and drying to obtain nitrile attapulgite, the reaction formula of which is:

[0011]

[0012] Step (2), adding a 40-60% by mass sulfuric acid aqueous solution to the nitrilized attapulgite, reacting at 110-130° C. for 4-8 hours, cooling to room temperature after the reaction, filtering, washing with deionized water, and drying to obtain carboxylated attapulgite, wherein the reaction formula is:

[0013]

[0014] Step (3), adding the carboxylated attapulgite to the hydroxymethyl urea solution, stirring and mixing evenly, reacting at 45-60° C. for 15-30 minutes, and after the reaction is completed, drying, crushing, and passing through a 0.1-0.2 mm sieve to obtain attapulgite-modified urea formaldehyde.

[0015] Preferably, in the step (1), the ratio of the amount of amino-attapulgite to 4-vinylbenzonitrile is 100 g:(100-140) g.

[0016] Preferably, in the step (3), the usage ratio of carboxylated attapulgite and hydroxymethyl urea solution is (10-40) g:100 g.

[0017] Preferably, the preparation method of the attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer is:

[0018] S1. Add maleic anhydride to deionized water, stir and disperse, then add sodium p-styrene sulfonate and ammonium persulfate, react at 80-90°C for 2-4h. After the reaction, add 30% sodium hydroxide solution to adjust the pH to 7-8, precipitate with ethanol, filter and dry to obtain maleic anhydride-sodium p-styrene sulfonate copolymer, the reaction formula of which is:

[0019] S2. Under nitrogen conditions, maleic anhydride-sodium p-styrene sulfonate copolymer is added to tetrahydrofuran solvent, stirred and dispersed, and then amino attapulgite is added thereto, and the reaction is carried out at 65-75° C. for 1-3 hours. After the reaction is completed, it is filtered, washed with deionized water, dried, crushed, and passed through a 0.1-0.2 mm sieve to obtain attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer, and the reaction formula is:

[0020]

[0021] Preferably, in S1, the usage ratio of maleic anhydride to sodium p-styrene sulfonate is 100 g:(300-500) g.

[0022] Preferably, in S1, the amount of ammonium persulfate used is 6-12% of the total mass of maleic anhydride and acrylic acid.

[0023] Preferably, in S2, the usage ratio of maleic anhydride-sodium p-styrene sulfonate copolymer and amino attapulgite is 100g:(20-50)g.

[0024] (III) Beneficial technical effects

[0025] The present invention utilizes amination of attapulgite and 4-vinylbenzonitrile to undergo Michael addition reaction to obtain nitrile attapulgite, which is then hydrolyzed to produce carboxylated attapulgite, and the carboxylated attapulgite is used as a carrier to copolymerize with hydroxymethyl urea to form attapulgite-modified urea formaldehyde, which is used as an inner membrane to wrap urea therein, and when the fertilizer is applied to the soil, the easily hydrolyzed urea preferentially releases nitrogen to provide nutrient elements for crops, while the attapulgite-modified urea formaldehyde slowly releases nutrients under the dual effects of hydrolysis and microorganisms, thereby extending the fertilizer effect period and improving the utilization rate of the fertilizer.

[0026] Under the initiation of ammonium persulfate, maleic anhydride and sodium p-styrene sulfonate are copolymerized to obtain a maleic anhydride-sodium p-styrene sulfonate copolymer, and the amino attapulgite is reacted with the anhydride group in the maleic anhydride-sodium p-styrene sulfonate copolymer to obtain an attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer, which is used as an outer membrane to wrap the inner membrane therein, and the hydrolysis property of the siloxy bonds of the attapulgite is utilized to form a hydrophilic silanol group together with the carboxyl group and the sulfonic acid group to form a water-absorbing and water-retaining outer membrane, thereby improving the hydrophilic and water-retaining properties of the fertilizer, and the attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer contains a large number of branched structures, which can cross each other to form a cross-linked network structure, thereby hindering the loss of water molecules and further improving the water-retaining effect of the fertilizer. In addition, since the outer coating has highly polar silanol, carboxyl and sulfonic acid groups, it can form hydrogen bonds with urea, so that the coating material has the function of adsorbing urea. When the urea content in the external environment is low, the urea can be slowly released into the environment, further improving the slow-release effect and fertilizer utilization rate of the fertilizer.

[0027] The invention uses natural, cheap and easily available attapulgite as a raw material, urea particles as a core carrier, attapulgite-modified urea formaldehyde as an inner layer, and attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer as an outer layer to develop a modified attapulgite water-retaining slow-release fertilizer. The prepared modified attapulgite water-retaining slow-release fertilizer has low cost, good slow-release effect and water-retaining effect, and can be widely put into use. DETAILED DESCRIPTION

[0028] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively below, and preferred embodiments of the present invention are provided. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0029] Preparation method of aminated attapulgite: add 5 g of attapulgite to 60 mL of toluene solvent, then add 5 mL of aminopropyltriethoxysilane, react at 60° C. for 4 hours, filter after the reaction, wash with deionized water, and dry to obtain aminated attapulgite.

[0030] Preparation method of hydroxymethyl urea solution: add 5% sodium hydroxide solution by mass to 16.21g formaldehyde aqueous solution by mass fraction, adjust the pH to 8, add 24g urea thereto, stir to dissolve, react at 40°C for 1h to obtain hydroxymethyl urea solution.

[0031] Example 1

[0032] Step (1), under nitrogen conditions, add 5 g of amino attapulgite and 7 g of 4-vinylbenzonitrile to a methanol solvent, stir and disperse, react at 25° C. for 4 days, filter after the reaction, extract with methanol, and dry to obtain nitrile attapulgite.

[0033] Step (2), adding 50% by mass aqueous sulfuric acid solution to 10 g of nitrilized attapulgite, reacting at 120° C. for 6 h, cooling to room temperature after the reaction, filtering, washing with deionized water, and drying to obtain carboxylated attapulgite.

[0034] Step (3), adding 8 g of carboxylated attapulgite to 20 g of hydroxymethyl urea solution, stirring and mixing evenly, reacting at 45° C. for 30 min, and after the reaction, drying, crushing, and passing through a 0.1 mm sieve to obtain attapulgite-modified urea formaldehyde.

[0035] Step (4), adding 5 g of maleic anhydride to deionized water, stirring and dispersing, then adding 20 g of sodium p-styrene sulfonate and 2.2 g of ammonium persulfate thereto, reacting at 85° C. for 3 h. After the reaction is completed, adding 30% sodium hydroxide solution thereto to adjust the pH to 7, ethanol precipitation, filtering, and drying to obtain a maleic anhydride-sodium p-styrene sulfonate copolymer.

[0036] Step (5), under nitrogen conditions, add 20g of maleic anhydride-sodium p-styrene sulfonate copolymer to tetrahydrofuran solvent, stir and disperse, then add 8g of amino-attapulgite thereto, react at 75°C for 1h, after the reaction is completed, filter, wash with deionized water, dry, crush, and pass through a 0.2mm sieve to obtain attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer.

[0037] Step (6), adding 20g of urea granules with a particle size of 3mm into a disc granulator, spraying a polyvinyl alcohol binder with a mass fraction of 4% on the surface of the urea until a layer of binding liquid is formed on the surface of the urea, adding 5g of attapulgite modified urea formaldehyde to the granulator to form an inner membrane, and then spraying a polyvinyl alcohol binder with a mass fraction of 4% to form a layer of binding liquid on the surface of the inner membrane, and finally adding 10g of attapulgite modified maleic anhydride-sodium styrene sulfonate copolymer to the granulator, and drying to obtain a modified attapulgite water-retaining slow-release fertilizer.

[0038] Example 2

[0039] Step (1), under nitrogen conditions, add 5 g of amino attapulgite and 6 g of 4-vinylbenzonitrile to a methanol solvent, stir and disperse, react at 20° C. for 6 days, filter after the reaction, extract with methanol, and dry to obtain nitrile attapulgite.

[0040] Step (2), adding 50% by mass aqueous sulfuric acid solution to 10 g of nitrilized attapulgite, reacting at 110° C. for 4 h, cooling to room temperature after the reaction, filtering, washing with deionized water, and drying to obtain carboxylated attapulgite.

[0041] Step (3), adding 4 g of carboxylated attapulgite to 20 g of hydroxymethyl urea solution, stirring and mixing evenly, reacting at 60° C. for 20 min, and after the reaction, drying, crushing, and passing through a 0.2 mm sieve to obtain attapulgite-modified urea formaldehyde.

[0042] Step (4), adding 5 g of maleic anhydride to deionized water, stirring and dispersing, then adding 25 g of sodium p-styrene sulfonate and 2 g of ammonium persulfate thereto, reacting at 85° C. for 3 h. After the reaction is completed, adding 30% sodium hydroxide solution thereto to adjust the pH to 8, ethanol precipitation, filtering, and drying to obtain a maleic anhydride-sodium p-styrene sulfonate copolymer.

[0043] Step (5), under nitrogen conditions, add 20g of maleic anhydride-sodium p-styrene sulfonate copolymer to tetrahydrofuran solvent, stir and disperse, then add 10g of amino attapulgite thereto, react at 65°C for 3h, after the reaction is completed, filter, wash with deionized water, dry, crush, and pass through a 0.1mm sieve to obtain attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer.

[0044] Step (6), adding 20g of urea granules with a particle size of 3mm into a disc granulator, spraying a polyvinyl alcohol binder with a mass fraction of 4% on the surface of the urea until a layer of binding liquid is formed on the surface of the urea, adding 6g of attapulgite modified urea formaldehyde to the granulator to form an inner membrane, and then spraying a polyvinyl alcohol binder with a mass fraction of 4% to form a layer of binding liquid on the surface of the inner membrane, and finally adding 12g of attapulgite modified maleic anhydride-sodium styrene sulfonate copolymer to the granulator, and drying to obtain a modified attapulgite water-retaining slow-release fertilizer.

[0045] Example 3

[0046] Step (1), under nitrogen conditions, add 5 g of amino attapulgite and 5 g of 4-vinylbenzonitrile to a methanol solvent, stir and disperse, react at 35° C. for 4 days, filter after the reaction, extract with methanol, and dry to obtain nitrile attapulgite.

[0047] Step (2), adding a 40% by mass aqueous solution of sulfuric acid to 10 g of the nitrilized attapulgite, reacting at 130° C. for 6 h, cooling to room temperature after the reaction, filtering, washing with deionized water, and drying to obtain carboxylated attapulgite.

[0048] Step (3), adding 2 g of carboxylated attapulgite to 20 g of hydroxymethyl urea solution, stirring and mixing evenly, reacting at 50° C. for 15 min, and after the reaction, drying, crushing, and passing through a 0.1 mm sieve to obtain attapulgite-modified urea formaldehyde.

[0049] Step (4), adding 5 g of maleic anhydride to deionized water, stirring and dispersing, then adding 15 g of sodium p-styrene sulfonate and 2.4 g of ammonium persulfate thereto, reacting at 80° C. for 4 h. After the reaction is completed, adding 30% sodium hydroxide solution thereto to adjust the pH to 8, ethanol precipitation, filtering, and drying to obtain a maleic anhydride-sodium p-styrene sulfonate copolymer.

[0050] Step (5), under nitrogen conditions, add 20g of maleic anhydride-sodium p-styrene sulfonate copolymer to tetrahydrofuran solvent, stir and disperse, then add 4g of amino-attapulgite thereto, react at 70°C for 2h, after the reaction is completed, filter, wash with deionized water, dry, crush, and pass through a 0.1mm sieve to obtain attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer.

[0051] Step (6), adding 20g of urea granules with a particle size of 4mm into a disc granulator, spraying a polyvinyl alcohol binder with a mass fraction of 4% on the surface of the urea until a layer of binding liquid is formed on the surface of the urea, adding 7g of attapulgite modified urea formaldehyde to the granulator to form an inner membrane, and then spraying a polyvinyl alcohol binder with a mass fraction of 4% to form a layer of binding liquid on the surface of the inner membrane, and finally adding 14g of attapulgite modified maleic anhydride-sodium styrene sulfonate copolymer to the granulator, and drying to obtain a modified attapulgite water-retaining slow-release fertilizer.

[0052] Example 4

[0053] Step (1), under nitrogen conditions, 5 g of amino attapulgite and 6 g of 4-vinylbenzonitrile are added to a methanol solvent, stirred and dispersed, and reacted at 25° C. for 5 days. After the reaction is completed, the mixture is filtered, extracted with methanol, and dried to obtain nitrile attapulgite.

[0054] Step (2), adding a 60% by mass aqueous solution of sulfuric acid to 10 g of the nitrilized attapulgite, reacting at 120° C. for 8 h, cooling to room temperature after the reaction, filtering, washing with deionized water, and drying to obtain carboxylated attapulgite.

[0055] Step (3), adding 6 g of carboxylated attapulgite to 20 g of hydroxymethyl urea solution, stirring and mixing evenly, reacting at 50° C. for 20 min, and after the reaction is completed, drying, crushing, and passing through a 0.1 mm sieve to obtain attapulgite-modified urea formaldehyde.

[0056] Step (4), adding 5 g of maleic anhydride to deionized water, stirring and dispersing, then adding 20 g of sodium p-styrene sulfonate and 1.2 g of ammonium persulfate, reacting at 90° C. for 2 h, after the reaction is completed, adding 30% sodium hydroxide solution to adjust the pH to 7, ethanol precipitation, filtering, and drying to obtain a maleic anhydride-sodium p-styrene sulfonate copolymer.

[0057] Step (5), under nitrogen conditions, add 20g of maleic anhydride-sodium p-styrene sulfonate copolymer to tetrahydrofuran solvent, stir and disperse, then add 8g of amino-attapulgite thereto, react at 70°C for 2h, after the reaction is completed, filter, wash with deionized water, dry, crush, and pass through a 0.1mm sieve to obtain attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer.

[0058] Step (6), adding 20g of urea granules with a particle size of 2mm into a disc granulator, spraying a polyvinyl alcohol binder with a mass fraction of 4% on the surface of the urea until a layer of binding liquid is formed on the surface of the urea, adding 8g of attapulgite modified urea formaldehyde to the granulator to form an inner membrane, and then spraying a polyvinyl alcohol binder with a mass fraction of 4% to form a layer of binding liquid on the surface of the inner membrane, and finally adding 16g of attapulgite modified maleic anhydride-sodium styrene sulfonate copolymer to the granulator, and drying to obtain a modified attapulgite water-retaining slow-release fertilizer.

[0059] Comparative Example 1

[0060] The difference between this comparative example and Example 1 is that step (6) does not contain attapulgite-modified urea formaldehyde.

[0061] Comparative Example 2

[0062] The difference between this comparative example and Example 1 is that step (6) does not contain attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer.

[0063] Water retention performance test of water-retaining slow-release fertilizer:

[0064] Add 200g of dry soil passed through a 0.2mm sieve and 5g of fertilizer into a beaker, add deionized water until there is no water on the soil surface, and when the beaker is tilted, water seeps out between the inner wall of the beaker and the soil. Place it in an oven, dry it, weigh the mass, and calculate the water retention rate. Water retention rate (%) = (total mass of soil and fertilizer - mass of dry soil and fertilizer) / (total mass of fertilizer and soil when fully absorbed and saturated - mass of dry soil and fertilizer) × 100%.

[0065] Table 1:

[0066] 24h water retention rate (%) 72h water retention rate (%) Example 1 71.4 23.4 Example 2 74.0 28.1 Example 3 78.2 31.3 Example 4 80.1 32.4 Comparative Example 1 67.8 19.3 Comparative Example 2 59.4 14.8

[0067] As can be seen from the table, the 24h and 72h water retention rates of Examples 1-4 and Comparative Example 1 are better than those of Comparative Example 2. This is because Examples 1-4 and Comparative Example 1 contain attapulgite-modified maleic anhydride-sodium styrene sulfonate copolymers, which have silanol, carboxyl and sulfonic acid groups, all of which are hydrophilic groups and can form hydrogen bonds with water molecules, and have good water absorption and water retention properties, while Comparative Example 2 does not contain such a structure, and Comparative Example 2 lacks an outer membrane structure, so its water retention effect is not as good as that of Examples 1-4 and Comparative Example 1, and the water retention rate of Comparative Example 1 is lower than that of Examples 1-4, because Examples 1-4 have a three-layer structure, while Comparative Example 1 has a double-layer structure, and the water retention effect of the three-layer is better than that of the double-layer structure, so the water retention effect of Examples 1-4 is the best.

[0068] Test of slow-release performance of water-retaining slow-release fertilizer:

[0069] Add 5g of water-retaining slow-release fertilizer to a 0.15mm nylon bag, place it in a plastic bottle containing 100mL of deionized water, seal it, and place it in a constant temperature and humidity incubator at 30°C. After 24 hours, take out the plastic bottle, measure 10mL of the solution, and use the Kjeldahl method to test the cumulative nitrogen release rate of the fertilizer.

[0070] Table 2:

[0071] Cumulative nitrogen release rate (%) Example 1 59.2 Example 2 53.5 Example 3 45.1 Example 4 42.9 Comparative Example 1 79.1 Comparative Example 2 63.0

[0072] It can be seen from the table that the slow-release performance of Examples 1-4 and Comparative Example 2 is better than that of Comparative Example 1. This is because Examples 1-4 and Comparative Example 2 contain attapulgite modified urea formaldehyde, which can slowly release nitrogen elements. Examples 1-4 are better than Comparative Example 2 because the polar groups contained in Examples 1-2 can form hydrogen bonds with urea, thereby slowly releasing nitrogen elements and improving the slow-release effect of the fertilizer. Therefore, the modified attapulgite water-retaining slow-release fertilizer prepared by the present invention has a good slow-release effect.

[0073] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a modified attapulgite water-retaining slow-release fertilizer, characterized in that: The preparation method comprises the following steps: adding urea particles with a particle size of 2-4 mm into a disc granulator, spraying a polyvinyl alcohol binder with a mass fraction of 4% onto the surface of the urea until a layer of binding liquid is formed on the surface of the urea, adding attapulgite-modified urea formaldehyde into the granulator to form an inner film, spraying a polyvinyl alcohol binder with a mass fraction of 4% into the granulator to form a layer of binding liquid on the surface of the inner film, and finally adding attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer into the granulator, drying, and obtaining a modified attapulgite water-retaining slow-release fertilizer.

2. The method for preparing the modified attapulgite water-retaining slow-release fertilizer according to claim 1, characterized in that: The usage ratio of the urea granules, the attapulgite-modified urea formaldehyde, and the attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer is 100g:(25-40)g:(50-80)g.

3. The method for preparing the modified attapulgite water-retaining slow-release fertilizer according to claim 1, characterized in that: The preparation method of the attapulgite-modified urea formaldehyde is: Step (1), under nitrogen conditions, adding aminated attapulgite and 4-vinylbenzonitrile to a methanol solvent, stirring and dispersing, reacting at 20-35° C. for 4-6 days, filtering after the reaction, extracting with methanol, and drying to obtain nitrified attapulgite; Step (2), adding a 40-60% by mass sulfuric acid aqueous solution to the nitrilized attapulgite, reacting at 110-130° C. for 4-8 hours, cooling to room temperature after the reaction, filtering, washing with deionized water, and drying to obtain carboxylated attapulgite; Step (3), adding the carboxylated attapulgite to the hydroxymethyl urea solution, stirring and mixing evenly, reacting at 45-60° C. for 15-30 minutes, and after the reaction is completed, drying, crushing, and passing through a 0.1-0.2 mm sieve to obtain attapulgite-modified urea formaldehyde.

4. The method for preparing the modified attapulgite water-retaining slow-release fertilizer according to claim 3, characterized in that: In the step (1), the usage ratio of the amino-attapulgite and 4-vinylbenzonitrile is 100 g:(100-140) g.

5. The method for preparing the modified attapulgite water-retaining slow-release fertilizer according to claim 3, characterized in that: In the step (3), the usage ratio of carboxylated attapulgite and hydroxymethyl urea solution is (10-40) g:100 g.

6. The method for preparing the modified attapulgite water-retaining slow-release fertilizer according to claim 1, characterized in that: The preparation method of the attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer is: S1, adding maleic anhydride to deionized water, stirring and dispersing, then adding sodium p-styrene sulfonate and ammonium persulfate thereto, reacting at 80-90° C. for 2-4 hours, after the reaction is completed, adding 30% sodium hydroxide solution thereto to adjust the pH to 7-8, ethanol precipitation, filtering, and drying to obtain maleic anhydride-sodium p-styrene sulfonate copolymer; S2. Under nitrogen conditions, add maleic anhydride-sodium p-styrene sulfonate copolymer to tetrahydrofuran solvent, stir and disperse, then add amino attapulgite thereto, react at 65-75°C for 1-3 hours. After the reaction is completed, filter, wash with deionized water, dry, crush, and pass through a 0.1-0.2 mm sieve to obtain attapulgite-modified maleic anhydride-sodium p-styrene sulfonate copolymer.

7. The method for preparing the modified attapulgite water-retaining slow-release fertilizer according to claim 6, characterized in that: In the S1, the usage ratio of maleic anhydride and sodium p-styrene sulfonate is 100 g:(300-500) g.

8. The method for preparing the modified attapulgite water-retaining slow-release fertilizer according to claim 6, characterized in that: In the above S1, the amount of ammonium persulfate used is 6-12% of the total mass of maleic anhydride and acrylic acid.

9. The method for preparing the modified attapulgite water-retaining slow-release fertilizer according to claim 6, characterized in that: In the S2, the usage ratio of maleic anhydride-sodium p-styrene sulfonate copolymer and amino attapulgite is 100g:(20-50)g.

Citation Information

Patent Citations

  • Preparation for coating material for nitrogenous fertilizer and coating method thereof

    CN101270013A

  • Double-layer coated slow-release nitrogen fertilizer for improving saline-alkali soil and preparation method thereof

    CN106699449A

  • Method for preparing biological crust sand-fixing material

    CN108841393A

  • Modified attapulgite-based slow release fertilizer special for saline-alkali soil, preparation method and application thereof

    CN109232082A

  • Controlled-release fertilizer for wheat-intercropped peanuts and preparation method thereof

    CN111662124A

Cited By

  • Nanometer assistant for stabilizing pesticide as well as preparation method and application of nanometer assistant

    CN122556468A