Single-base powder material for fireworks and preparation method of single-base powder material

Through the steps of solution preparation, mixed plasticization and drying, single-base powder for fireworks with uniform particle size and good fluidity was prepared, which solved the problems of shortage of single-base powder materials and complex and poor safety in existing preparation methods, and achieved simple Safe and efficient preparation process and excellent performance products.

CN119059856APending Publication Date: 2024-12-03LUZHOU NORTH CHEM IND
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411484518.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Single-based powder materials are short of and existing preparation methods are complex, costly, poor safety and stability, which leads to the fireworks industry facing supply shortage and safety accidents.

Method used

Using the steps of solution preparation, mixing and plasticizing, screening and granulation, drying, polishing and secondary drying, fireworks with uniform particle size and good fluidity are prepared through kneading machines, screening machines, polishing machines and pot-type drying equipment and other equipment. Use single-based powder material to ensure simple, safe and efficient process.

Benefits of technology

The shortage of single-based powder materials has been solved, the preparation process is simple, safe and efficient, and the product performance is comparable to that of existing single-based powders, reducing production costs and safety risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005098382260000041
    Figure BDA0005098382260000041
Patent Text Reader

Abstract

The invention discloses a single-base powder material for fireworks and a preparation method of the single-base powder material, and belongs to the field of fireworks. The single-base powder material for the fireworks comprises the following raw material components in parts by mass in terms of absolute dry weight: 100 parts of nitrocellulose, 1-2 parts of a stabilizing agent, 30-60 parts of water and 50-80 parts of a solvent. The preparation method comprises the following steps: dissolving the stabilizing agent in the solvent, and adding water to prepare a mixed solution; mixing and plasticizing nitrocellulose and the mixed solution, and screening to obtain a granular material; drying the granular material until the moisture content is 1-10%, and then polishing; and drying the polished material until the moisture content is 1-5%, and then screening to obtain the single-base powder material for the fireworks, which is uniform in particle size. The prepared single-base powder material for fireworks is uniform in particle size and good in fluidity, and the problems that an existing single-base powder preparation method is complex in process and high in cost, and a preparation method or a prepared product is poor in safety degree and stability can be effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of fireworks, and in particular relates to a single-base powder material for fireworks and a preparation method thereof. Background Art

[0002] At present, the single-base powder used in the fireworks industry is mainly produced by crushing and drying retired or waste single-base propellants. Single-base powder has the characteristics of high energy, so it can be used as propellant for fireworks. In recent years, the development of the fireworks industry has ushered in spring, and the demand for single-base powder has increased day by day. However, with the gradual reduction of retired drugs in the national reserve and the control of national policies on agents, the supply of single-base powder has tightened, and there is a phenomenon of supply exceeding demand. Therefore, the fireworks industry is in urgent need of a propellant for fireworks that can replace single-base powder.

[0003] CN113307708A discloses a method for preparing a single-base powder and the single-base powder obtained by the method. The method for preparing the single-base powder comprises: (1) a mixing step: dissolving the base material with an organic solvent, adding a stabilizer, and then adding nitrocellulose to obtain a mixture; the base material is at least one of nitrocellulose, a single-base tubular medicine, a single-base powder, a double-base tubular medicine, and a double-base powder; (2) a molding step: pressing the mixture and vacuum filtering to obtain a solid material; (3) a pelletizing step: immersing the solid material in water and pelletizing to obtain a single-base powder. In the preparation process of the method, the materials are first mixed, then vacuum filtered and pressed into shape, and then the solid material is pelletized in water, and the organic solvent in the water is recovered by calcium chloride or distillation. The preparation method is relatively complicated and the production cost is high.

[0004] Some existing single-base powder preparation methods are relatively complicated, or the inherent safety of the preparation methods is not enough, or the safety and stability of the prepared products are poor, so explosion safety accidents often occur in fireworks factories. Therefore, it is urgent to develop a simple and safe single-base powder and its preparation method. Summary of the invention

[0005] The technical problem to be solved by the present invention is that the single-base powder material is in short supply, but the existing single-base powder preparation method has the problems of complex process, high cost, and poor safety and stability of the preparation method or the obtained product.

[0006] The technical solution adopted by the present invention to solve the technical problem is:

[0007] In a first aspect, the present invention provides a method for preparing a single-base powder material for fireworks, comprising the following steps:

[0008] a. Solution preparation: dissolve the stabilizer completely in the solvent, then add water to prepare a mixed solution;

[0009] b. Mixing and plasticizing: The nitrocellulose and the mixed solution obtained in step a are put into a kneader for mixing and plasticizing to obtain a semi-plasticized nitrocellulose material;

[0010] c. Sieving and granulating: Sieving the semi-plasticized nitrocellulose material obtained in step b to obtain a granular material with uniform particle size;

[0011] d. Drying and polishing: The granular material obtained in step c is dried to a moisture content of 1% to 10%, then placed in a polishing machine, and sprayed with an appropriate amount of solvent for polishing;

[0012] e. Drying and screening: Dry the polished material to a moisture content of 1% to 5%, and then screen it to obtain a single-base powder material for fireworks with uniform particle size.

[0013] In the above steps a and b, the mass parts of the raw material components are as follows: 100 parts of nitrocellulose, 1 to 2 parts of stabilizer, 30 to 60 parts of water, and 50 to 80 parts of solvent, calculated on an absolute dry basis.

[0014] Furthermore, the nitrogen content of the above-mentioned nitrocellulose is 10% to 13.5%, and specifically, it is at least one of cotton pulp nitrocellulose, bamboo pulp nitrocellulose, and wood pulp nitrocellulose.

[0015] Furthermore, the above-mentioned stabilizer is at least one of diphenylamine, stabilizer I and stabilizer II.

[0016] Furthermore, the above-mentioned solvent is at least one of ethers, alcohols, esters and ketones.

[0017] In the above step b, the mixing time is 30 min to 60 min.

[0018] In the above step c, screening is performed by a screening machine or a hand screen, and the mesh number of the screen is 10 to 50 meshes.

[0019] In the above step d, a basin-type drying device is used for drying, and the drying temperature is 30-60°C.

[0020] In the above step e, a basin-type drying device is used for drying at a drying temperature of 30 to 50° C.; and sieving is performed through a sieve of 10 to 50 meshes.

[0021] In a second aspect, the present invention provides a single-base powder material for fireworks, which is prepared by the above-mentioned preparation method.

[0022] The beneficial effects of the present invention are as follows: first, the present invention provides a method for preparing a single-base powder material for fireworks to solve the problem of shortage of single-base powder materials. The single-base powder material for fireworks prepared by the method has the characteristics of uniform particle size, good fluidity and comparable performance to existing single-base powders. At the same time, the preparation method provided by the present invention has a simple preparation process, is easy to operate mechanically, and can achieve human-machine isolation throughout the preparation process, which has the advantages of low labor intensity for operators, high operation efficiency, and high safety of the preparation process. DETAILED DESCRIPTION

[0023] The technical solution of the present invention can be specifically implemented in the following manner.

[0024] The single-base powder material for fireworks, the weight proportions of each component of its raw material preparation are calculated on an absolute dry basis as follows: 100 parts of nitrocellulose, 1 to 2 parts of stabilizer, 30 to 60 parts of water, and 50 to 80 parts of solvent; wherein the weight proportion of nitrocellulose is the weight of the dry amount of nitrocellulose in the nitrocellulose, and the water content in the nitrocellulose is included in the weight proportion of water.

[0025] The method for preparing the above-mentioned single-base powder material for fireworks comprises the following steps:

[0026] (1) Solution preparation: Weigh the stabilizer, solvent and water according to the mass ratio, completely dissolve the stabilizer in the solvent, and then add water to prepare a mixed solution. If the nitrocellulose contains a certain amount of water, the corresponding mass of water in the nitrocellulose should be deducted in this step;

[0027] (2) Mixing and plasticizing: Put the aqueous nitrocellulose and the prepared mixed solution into a kneader and mix for 30 to 60 minutes to ensure that the components are evenly mixed to obtain a semi-plasticized nitrocellulose material;

[0028] (3) Screening and granulation: The nitrocellulose material prepared in step (2) is screened by a screening machine or a hand screen (the mesh size is 10 to 50 meshes), and the material under the screen is a qualified product, thereby obtaining a granular material with uniform particle size;

[0029] (4) Drying: The prepared granular material is dried at a temperature of 30 to 60° C. using a basin drying device, and the moisture content after drying is 1% to 10%, thereby obtaining a granular material with good fluidity and uniform particle size;

[0030] (5) Polishing: The dried granular material is placed in a polishing machine and sprayed with solvent for polishing;

[0031] (6) Secondary drying: The polished material is dried using a basin drying device at a temperature of 30 to 50°C (the moisture content is relatively low at this time, and the temperature should not be too high to ensure safety). The moisture content after drying is 1% to 5%;

[0032] (7) Secondary screening: Use a 10-50 mesh sieve to sieve the granular material obtained in step (6). The sieved material is the single-base powder material for fireworks.

[0033] The technical solution and effects of the present invention are further illustrated below through practical examples.

[0034] Example

[0035] The present invention provides four groups of Examples 1 to 4 of single-base powder materials for fireworks prepared by the method of the present invention. The raw material formulas used in the examples (in terms of absolute dry weight, kg) are: 100 nitrocellulose (dry weight of nitrocellulose), 1 stabilizer, 60 solvent, and 1% HCl. 2 O 40.

[0036] The specific preparation process steps for the preparation of the single-base powder material for fireworks in Examples 1 to 4 are as follows:

[0037] (1) Prepare the materials according to the above formula, weigh 133 kg of aqueous nitrocellulose (100 kg of dry nitrocellulose, 33 kg of water), 1 kg of stabilizer, 60 kg of solvent, and 7 kg of water; wherein: the stabilizer used in Example 1 is diphenylamine and the solvent is ethyl acetate, the stabilizer used in Example 2 is stabilizer I and the solvent is ethyl acetate, the stabilizer used in Example 3 is stabilizer II and the solvent is ethyl acetate, and the stabilizer used in Example 4 is diphenylamine and the solvent is acetone;

[0038] (2) Dissolve 1 kg of the stabilizer completely in 60 kg of the solvent, and then add 7 kg of water to prepare a mixed solution;

[0039] (2) placing the aqueous nitrocellulose and the prepared mixed solution into a kneader and mixing for 60 minutes to ensure uniform mixing of the components, thereby obtaining a semi-plasticized nitrocellulose material;

[0040] (3) The nitrocellulose material prepared in step (2) is sieved by a sieving machine or a hand sieve, the mesh number of the sieve is 20 meshes, and the material is sieved to obtain a granular material with uniform particle size;

[0041] (4) drying the granular material prepared in step (3) at a drying temperature of 55° C. using a basin drying device to dry the moisture content to 1% to 10%, thereby obtaining a granular material with good fluidity and uniform particle size;

[0042] (5) placing the granular material dried in step (4) into a polishing machine and spraying a solvent for polishing;

[0043] (6) Drying the polished material in step (5) by using a basin drying device to dry the prepared granular material at a drying temperature of 50° C., and controlling the moisture content of the material to be dried to be between 1% and 5%;

[0044] (7) Secondary screening: Use a 20-mesh sieve to sieve the solid material with uniform particle size obtained in step (6). The material below the sieve is the single-base powder material for fireworks.

[0045] The burning speed of the single-base powder products for fireworks prepared in Examples 1-4 was tested. The single-base powder for fireworks prepared in Examples 1-4 was made into ground spray flowers, and then the burning spray time and spray height were tested. The test results are shown in Table 1.

[0046]

[0047] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a single-base powder material for fireworks, characterized in that: The steps include: a. Solution preparation: dissolve the stabilizer completely in the solvent, then add water to prepare a mixed solution; b. Mixing and plasticizing: The nitrocellulose and the mixed solution obtained in step a are put into a kneader for mixing and plasticizing to obtain a semi-plasticized nitrocellulose material; c. Sieving and granulating: Sieving the semi-plasticized nitrocellulose material obtained in step b to obtain a granular material with uniform particle size; d. Drying and polishing: The granular material obtained in step c is dried to a moisture content of 1% to 10%, then placed in a polishing machine, and sprayed with an appropriate amount of solvent for polishing; e. Drying and screening: Dry the polished material to a moisture content of 1% to 5%, and then screen it to obtain a single-base powder material for fireworks with uniform particle size.

2. The method for preparing a single-base powder material for fireworks according to claim 1, characterized in that: In steps a and b, the mass parts of each raw material component are calculated as follows on an absolute dry basis: 100 parts of nitrocellulose, 1 to 2 parts of a stabilizer, 30 to 60 parts of water, and 50 to 80 parts of a solvent.

3. The method for preparing a single-base powder material for fireworks according to claim 2, characterized in that: The nitrogen content of the nitrocellulose is 10% to 13.5%, and the nitrocellulose is specifically at least one of cotton pulp nitrocellulose, bamboo pulp nitrocellulose and wood pulp nitrocellulose.

4. The method for preparing a single-base powder material for fireworks according to claim 2, characterized in that: The stabilizer is at least one of diphenylamine, stabilizer I and stabilizer II.

5. The method for preparing a single-base powder material for fireworks according to claim 2, characterized in that: The solvent is at least one of ethers, alcohols, esters and ketones.

6. The method for preparing a single-base powder material for fireworks according to claim 1, characterized in that: In step b, the mixing time is 30 min to 60 min.

7. The method for preparing a single-base powder material for fireworks according to claim 1, characterized in that: In step c, screening is performed by a screening machine or a hand screen, and the mesh number of the screen is 10 to 50 meshes.

8. The method for preparing a single-base powder material for fireworks according to claim 1, characterized in that: In step d, a basin-type drying device is used for drying, and the drying temperature is 30 to 60°C.

9. The method for preparing a single-base powder material for fireworks according to claim 1, characterized in that: In step e, drying is performed using a basin drying device at a drying temperature of 30 to 50° C., and sieving is performed using a 10-mesh to 50-mesh sieve.

10. Single base powder material for fireworks, characterized by: The method is prepared according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Wood pulp nitrocellulose single-base propellant and preparation method thereof

    CN104003825A

  • Production method of nitrocellulose for indoor fireworks

    CN109251116A

  • Continuous preparation process of nitrocotton for fireworks

    CN110540484A