Preparation method of bio-based rigid heat-resistant environment-friendly copolyester

By using bio-based raw materials and catalysts with rigid structures in bio-based polyester materials, combined with esterification and polycondensation reaction technology, high-performance bio-based rigid heat-resistant and environmentally friendly copolyesters are prepared, which solves the problem of heat resistance of existing materials in the heat resistance of existing materials The lack of environmental protection has achieved a balance between high rigidity and low carbon footprint.

CN119060309APending Publication Date: 2024-12-03PETROCHINA CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311529052.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-11-16
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing bio-based polyester materials have shortcomings in terms of heat resistance and environmental protection, and it is difficult to meet the needs of high rigidity and low carbon footprints at the same time.

Method used

Use some bio-based raw materials with rigid structure and compound additives as catalytic stabilization systems to prepare bio-based rigid heat-resistant and environmentally friendly copolyester materials through esterification and polycondensation reactions, and use stainless steel reactors to conduct esterification and polycondensation reactions to control the reaction. Temperature and pressure, add an appropriate amount of catalyst and stabilizer to improve the performance of the material.

Benefits of technology

The glass transition temperature (Tg) of bio-based rigid heat-resistant copolyester and the activity and selectivity of the catalyst are improved, and the carbon footprint of the material is reduced by at least 10%, and the heat resistance of the material is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004552964020000041
    Figure BDA0004552964020000041
  • Figure HDA0004552964030000011
    Figure HDA0004552964030000011
Patent Text Reader

Abstract

The invention belongs to the technical field of bio-based materials, and discloses a preparation method of bio-based rigid heat-resistant environment-friendly copolyester. Comprising esterification reaction, distillation and polycondensation reaction. The catalyst produced by the preparation method has the characteristics of high activity, selectivity and stability; the Tg temperature of the bio-based rigid heat-resistant copolyester at least can reach 90 DEG C; the carbon footprint of the bio-based rigid heat-resistant copolyester can be reduced by at least 10%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of bio-based materials, and specifically relates to a method for preparing a bio-based rigid heat-resistant and environmentally friendly copolyester. Background Art

[0002] The method to improve the heat resistance of polyester is usually to introduce a rigid raw material monomer into the reaction system through polymerization modification to improve the rigidity and stability of the polyester molecular chain segment. This rigid monomer can be a dibasic acid with a benzene ring structure, such as terephthalic acid, isophthalic acid, etc., or a dibasic acid with a naphthalene ring structure such as naphthalene dicarboxylic acid, etc.; you can also choose a diol with a rigid structure, such as 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, isosorbide, etc.

[0003] The method of developing bio-based polyester materials is usually to use bio-based raw materials to replace traditional chemical raw materials, such as bio-based dibasic acids furandicarboxylic acid, 1,4-butanedioic acid, etc., bio-based diols isosorbide, 1,3-propylene glycol, etc. Summary of the invention

[0004] In order to overcome the shortcomings of the prior art, the present invention provides a method for preparing a bio-based rigid heat-resistant and environmentally friendly copolyester, which selects some raw materials with a rigid structure and bio-based raw materials as modified monomers, and selects compounded additives as a catalytic stabilization system for the synthesis reaction, and obtains a bio-based rigid heat-resistant copolyester material through reaction.

[0005] The above object of the present invention is achieved through the following technical scheme: A method for preparing a bio-based rigid heat-resistant and environmentally friendly copolyester, the steps are as follows:

[0006] 1. Esterification reaction: Add dibasic acid, excess diol and catalyst into a stainless steel reactor;

[0007] 2. Distilling off the water generated by the esterification reaction in step 1;

[0008] 3. Vacuum the stainless steel reactor and distill off the remaining diol from the esterification reaction in step 1;

[0009] 4. Polycondensation reaction: Add a stabilizer to the vacuumed stainless steel reactor to carry out a polycondensation reaction to generate a bio-based rigid heat-resistant and environmentally friendly copolyester product.

[0010] Furthermore, the stainless steel reactor is externally connected to an esterification water reflux column, a nitrogen inlet, a pressure gauge, and a feed port; a bottom discharge valve is provided at the bottom of the stainless steel reactor; a thermocouple sleeve and a stirring motor are provided inside the stainless steel reactor; a nitrogen valve is provided on the nitrogen inlet external to the stainless steel reactor; a reflux column top temperature thermocouple sleeve is connected to the top of the esterification water reflux column; the esterification water reflux column is provided with two branches from top to bottom; the upper branch is connected to an esterification water valve and an esterification water condenser in sequence; the lower branch is connected to an alcohol discharge valve, an alcohol condenser, a mixed alcohol receiver, a vacuum buffer tank, and a vacuum pump in sequence; the mixed alcohol receiver and the bottom of the vacuum buffer tank are both provided with a mixed alcohol discharge valve; and a vacuum gauge is provided on the top of the vacuum buffer tank.

[0011] Furthermore, the step 1 is specifically as follows: the dibasic acid and excess diol enter from the feed port of the stainless steel reactor, and then the catalyst is added, and then the reactor is heated and the temperature of the entire esterification reaction is controlled at 230-260°C, the stirring motor is turned on and stirred at a low speed of 10-40 Hz frequency, and the reaction time is 60-170 minutes.

[0012] Furthermore, in step 1, the molar ratio of the dibasic acid to the diol is 1:(1-2).

[0013] Furthermore, in step 1, the amount of catalyst added is 1-300 ppm of the amount of dibasic acid added.

[0014] Furthermore, the step 2 is specifically as follows: the water generated by the esterification reaction in step 1 is distilled out through the esterification water reflux column connected to the reactor through the esterification water condenser. This stage is carried out at a pressure of 0.20MPa to 0.30MPa. During this period, the pressure in the reactor and the temperature at the top of the process tower are controlled by the esterification water valve to ensure that the pressure in the reactor is stable within the range of 0.20MPa to 0.30MPa, and the temperature at the top of the process tower is stable between 100-150°C. When the water distillation amount reaches 80% of the theoretical generation amount, the system pressure is slowly reduced to normal pressure, and the alcohol discharge valve is opened and the esterification water valve is closed.

[0015] Furthermore, the step 3 is specifically as follows: start the vacuum pump reaction to perform vacuum treatment to enter the pre-polycondensation reaction stage, during which the excess ethylene glycol and the ethylene glycol generated by the polycondensation reaction are distilled into the mixed alcohol receiver, and the alcohol distillation state of the mixed alcohol receiver is observed during the vacuuming process to prevent the vaporized ethylene glycol from being taken out due to too fast vacuuming, and after the vacuum degree reaches a slightly negative pressure state, the stirring is adjusted to a high speed of 40 to 60 Hz for high-speed devolatilization, and the polycondensation reaction stage is entered, and the temperature is controlled at 260°C-290°C. When the stirring shaft power rises to 0.150 to 0.300 kW, the polycondensation reaction is completed, and the heat-resistant copolyester product is generated.

[0016] Furthermore, the dibasic acid added in step 1 is one, two or three of 2,6-naphthalene dicarboxylic acid, terephthalic acid and isophthalic acid, and the diol added in step 1 is the bio-based raw material isosorbide, the molar fraction of which accounts for 10%-50% of the total alcohol, and the remainder is one of ethylene glycol and 1,4-cyclohexanedimethanol or two of them in any ratio.

[0017] Furthermore, the catalysts germanium dioxide and cobalt acetate added in step 1 are as follows: the amount of germanium dioxide added is 100-600ppm of the total mass of the dibasic acid; the amount of cobalt acetate added is 100-400ppm of the total mass of the dibasic acid; the stabilizer is one or two of phosphoric acid, phosphate esters, and phosphites; and the toner is one or two of color oil or color powder toners.

[0018] Compared with the prior art, the present invention has the following beneficial effects: the catalyst produced by the preparation method has high activity, selectivity and stability; the Tg temperature of the bio-based rigid heat-resistant copolyester can reach at least 90°C; and the carbon footprint of the bio-based rigid heat-resistant copolyester can be reduced by at least 10%. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0020] Figure 1 It is a schematic diagram of the device structure used in the method for preparing bio-based rigid heat-resistant and environmentally friendly copolyester of the present invention.

[0021] In the figure, 1. reactor; 2. feed inlet; 3. pressure gauge; 4. thermocouple sleeve; 5. stirring motor; 6. discharge valve at the bottom of the reactor; 7. nitrogen inlet; 8. esterification water reflux column; 9. alcohol discharge valve; 10. alcohol condenser; 11. mixed alcohol receiver; 12. vacuum buffer tank; 13. mixed alcohol discharge valve; 14. vacuum pump; 15. vacuum gauge; 16. reflux column top temperature thermocouple sleeve; 17. esterification water valve; 18. esterification water condenser. DETAILED DESCRIPTION

[0022] The present invention is described in detail below by specific examples, but the protection scope of the present invention is not limited. Unless otherwise specified, the experimental methods used in the present invention are all conventional methods, and the experimental equipment, materials, reagents, etc. used can be obtained from commercial channels.

[0023] Example 1

[0024] 1500 g of 2,6-naphthalene dicarboxylic acid (2,6-NDA), 482 g of ethylene glycol (EG), 142 g of isosorbide (IS), 140 g of 1,4-cyclohexanedimethanol (CHDM), 0.5 g of germanium dioxide, and 0.25 g of cobalt acetate were added to a 5L stainless steel reactor equipped with a nitrogen inlet, a feed port, a discharge port, a fractionating column, two condensers, and a stirrer. The esterification reaction temperature was 200-250°C, the final esterification reaction temperature was 250°C, the reaction pressure was 0.20-0.25 MPa (gauge pressure), and the reaction time was 180 minutes. After the esterification reaction was completed, 0.25 g of trimethyl phosphate was added to the system for polycondensation reaction. Among them, the condensation reaction temperature in the low vacuum stage is 250-260°C, the reaction pressure is 0-0.1MPa (gauge pressure), the reaction time is 20 minutes, the condensation reaction temperature in the high vacuum stage is 250-285°C, the final temperature of the condensation reaction is 285°C, the vacuum degree of the reaction system is 50-100Pa, and the reaction time is 65 minutes.

[0025] The obtained polymer chips had a glass transition temperature Tg of 120° C., an intrinsic viscosity of 0.605 dL / g, and a molar ratio of isosorbide to diol chain segments of 10%.

[0026] Comparative Example 1 Under the premise that the process conditions remain unchanged relative to Example 1, 1500 grams of terephthalic acid (PTA), 784 grams of ethylene glycol (EG), and 0.875 grams of antimony acetate are added to the reactor. The esterification reaction temperature is 200-250°C, the final esterification reaction temperature is 250°C, the reaction pressure is 0.20-0.25MPa (gauge pressure), and the reaction time is 150 minutes. After the esterification reaction is completed, a polycondensation reaction is carried out. Among them, the polycondensation reaction temperature in the low vacuum stage is 250-260°C, the reaction pressure is 0-0.1MPa (gauge pressure), the reaction time is 20 minutes, the polycondensation reaction temperature in the high vacuum stage is 250-285°C, the final polycondensation reaction temperature is 285°C, the vacuum degree of the reaction system is 50-100Pa, and the reaction time is 110 minutes. The comparative experimental results are shown in Table 1. The results show that the heat resistance of the bio-based rigid heat-resistant copolyester prepared by the present invention is significantly better than that of ordinary polyester.

[0027] Table 1 Example 1 and Comparative Example 1

[0028]

[0029] Example 2

[0030] 1500 g of terephthalic acid (PTA), 196 g of ethylene glycol (EG), 462 g of isosorbide (IS), 911 g of 1,4-cyclohexanedimethanol (CHDM), 0.5 g of germanium dioxide, 0.2 g of cobalt acetate, 0.02 g of blueing agent, and 0.01 g of redding agent were added to a 5L stainless steel reactor equipped with a nitrogen inlet, a feed port, a discharge port, a fractionating column, two condensers, and a stirrer. The esterification reaction temperature was 200-250°C, the final esterification reaction temperature was 250°C, the reaction pressure was 0.20-0.25 MPa (gauge pressure), and the reaction time was 150 minutes. After the esterification reaction was completed, 0.25 g of trimethyl phosphate was added to the system for polycondensation reaction. Among them, the condensation reaction temperature in the low vacuum stage is 250-260°C, the reaction pressure is 0-0.1MPa (gauge pressure), the reaction time is 20 minutes, the condensation reaction temperature in the high vacuum stage is 250-270°C, the final temperature of the condensation reaction is 270°C, the vacuum degree of the reaction system is 50-100Pa, and the reaction time is 130 minutes.

[0031] The obtained polymer chips had a glass transition temperature Tg of 90° C., an intrinsic viscosity of 0.66 dL / g, and a molar ratio of isosorbide to diol chain segments of 25%.

[0032] Example 3

[0033] 1310 g of terephthalic acid (PTA), 190 g of 2,6-naphthalene dicarboxylic acid (2,6-NDA), 685 g of ethylene glycol (EG), 179 g of isosorbide (IS), 0.5 g of germanium dioxide, and 0.25 g of cobalt acetate were added to a 5L stainless steel reactor equipped with a nitrogen inlet, a feed port, a discharge port, a fractionating column, two condensers, and a stirrer. The esterification reaction temperature was 200-250°C, the final esterification reaction temperature was 250°C, the reaction pressure was 0.20-0.25 MPa (gauge pressure), and the reaction time was 160 minutes. After the esterification reaction was completed, 0.25 g of trimethyl phosphate was added to the system for polycondensation reaction. Among them, the condensation reaction temperature in the low vacuum stage is 250-260°C, the reaction pressure is 0-0.1MPa (gauge pressure), the reaction time is 20 minutes, the condensation reaction temperature in the high vacuum stage is 250-280°C, the final temperature of the condensation reaction is 280°C, the vacuum degree of the reaction system is 50-100Pa, and the reaction time is 115 minutes.

[0034] The obtained polymer chips had a glass transition temperature Tg of 90° C., an intrinsic viscosity of 0.63 dL / g, and a molar ratio of isosorbide to diol chain segments of 10%.

[0035] Example 4

[0036] 1200 g of terephthalic acid (PTA), 300 g of isophthalic acid (IPA), 196 g of ethylene glycol (EG), 462 g of isosorbide (IS), 911 g of 1,4-cyclohexanedimethanol (CHDM), 0.6 g of germanium dioxide, 0.2 g of cobalt acetate, 0.02 g of blueing agent, and 0.01 g of redding agent were added to a 5L stainless steel reactor equipped with a nitrogen inlet, a feed port, a discharge port, a fractionating column, two condensers, and a stirrer. The esterification reaction temperature was 200-250°C, the final esterification reaction temperature was 250°C, the reaction pressure was 0.20-0.25 MPa (gauge pressure), and the reaction time was 155 minutes. After the esterification reaction was completed, 0.25 g of trimethyl phosphate was added to the system for polycondensation reaction. Among them, the condensation reaction temperature in the low vacuum stage is 250-260°C, the reaction pressure is 0-0.1MPa (gauge pressure), the reaction time is 20 minutes, the condensation reaction temperature in the high vacuum stage is 250-270°C, the final temperature of the condensation reaction is 270°C, the vacuum degree of the reaction system is 50-100Pa, and the reaction time is 150 minutes.

[0037] The obtained polymer chips had a glass transition temperature Tg of 90° C., an intrinsic viscosity of 0.62 dL / g, and a molar ratio of isosorbide to diol chain segments of 25%.

[0038] Example 5

[0039] 1165 g of terephthalic acid (PTA), 146 g of isophthalic acid (IPA), 189 g of 2,6-naphthalene dicarboxylic acid (2,6-NDA), 609 g of ethylene glycol (EG), 179 g of isosorbide (IS), 177 g of 1,4-cyclohexanedimethanol (CHDM), 0.5 g of germanium dioxide, and 0.25 g of cobalt acetate were added to a 5L stainless steel reactor equipped with a nitrogen inlet, a feed port, a discharge port, a fractionating column, two condensers, and a stirrer. The esterification reaction temperature was 200-250°C, the final esterification reaction temperature was 250°C, the reaction pressure was 0.20-0.25 MPa (gauge pressure), and the reaction time was 150 minutes. After the esterification reaction was completed, 0.25 g of trimethyl phosphate was added to the system for polycondensation. Among them, the condensation reaction temperature in the low vacuum stage is 250-260°C, the reaction pressure is 0-0.1MPa (gauge pressure), the reaction time is 20 minutes, the condensation reaction temperature in the high vacuum stage is 250-285°C, the final temperature of the condensation reaction is 285°C, the vacuum degree of the reaction system is 50-100Pa, and the reaction time is 130 minutes.

[0040] The obtained polymer chips had a glass transition temperature Tg of 95° C., an intrinsic viscosity of 0.65 dL / g, and a molar ratio of isosorbide to diol chain segments of 10%.

[0041] The above-described embodiments are only preferred embodiments of the present invention, but not all feasible embodiments of the present invention. For those skilled in the art, any obvious changes made thereto without departing from the principles and spirit of the present invention should be considered to be included in the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a bio-based rigid heat-resistant and environmentally friendly copolyester, characterized in that: Here are the steps: S1. Esterification reaction: Add dibasic acid, excess diol and catalyst into a stainless steel reactor; S2. distilling the water generated by the esterification reaction in step S1; S3. The stainless steel reactor is evacuated and the remaining diol from the esterification reaction in step S1 is distilled off; S4. Condensation polymerization reaction: adding a stabilizer to the vacuumized stainless steel reactor to carry out a condensation polymerization reaction to generate a bio-based rigid heat-resistant and environmentally friendly copolyester product.

2. The method for preparing bio-based rigid heat-resistant and environmentally friendly copolyester according to claim 1, characterized in that: The stainless steel reactor (1) is externally connected to an esterification water reflux column (8), a nitrogen inlet (7), a pressure gauge (3), and a feed port (2); a bottom discharge valve (6) is provided at the bottom of the stainless steel reactor (1); a thermocouple sleeve (4) and a stirring motor (5) are provided inside the stainless steel reactor (1); a nitrogen valve is provided on the nitrogen inlet (7) external to the stainless steel reactor (1); a reflux column top temperature thermocouple sleeve (16) is connected to the top of the esterification water reflux column (8); The flow column (8) is provided with two branches from top to bottom, the upper branch is connected to the esterification water valve (17) and the esterification water condenser (18) in sequence, and the lower branch is connected to the alcohol discharge valve (9), the alcohol condenser (10), the mixed alcohol receiver (11), the vacuum buffer tank (12), and the vacuum pump (14) in sequence, the mixed alcohol receiver (11) and the vacuum buffer tank (12) are both provided with a mixed alcohol discharge valve (13) at the bottom, and a vacuum gauge (15) is provided at the top of the vacuum buffer tank (12).

3. The method for preparing bio-based rigid heat-resistant and environmentally friendly copolyester according to claim 1, characterized in that: The step S1 is specifically as follows: dibasic acid and excess diol are introduced into the feed port of a stainless steel reactor, and then a catalyst is added, and then the reactor is heated and the temperature of the entire esterification reaction is controlled at 230-260° C., and the stirring motor is turned on to stir at a low speed of 10-40 Hz, and the reaction time is 60-170 minutes.

4. The method for preparing bio-based rigid heat-resistant and environmentally friendly copolyester according to claim 1, characterized in that: In step S1, the molar ratio of the dibasic acid to the diol is 1:(1-2).

5. The method for preparing bio-based rigid heat-resistant and environmentally friendly copolyester according to claim 1, characterized in that: The amount of catalyst added in step S1 is 1-300 ppm of the amount of dibasic acid added.

6. The method for preparing bio-based rigid heat-resistant and environmentally friendly copolyester according to claim 1, characterized in that: The step S2 specifically comprises: the water generated by the esterification reaction in step S1 is distilled out through the esterification water reflux column (8) connected to the reaction kettle (1) via the esterification water condenser (18). This stage is carried out at a pressure of 0.20MPa to 0.30MPa. During this period, the pressure in the kettle and the temperature at the top of the process tower are controlled by the esterification water valve (17) to ensure that the pressure in the kettle is stable within the range of 0.20MPa to 0.30MPa and the temperature at the top of the process tower is stable between 100-150°C. When the water distillation amount reaches 80% of the theoretical amount, the system pressure is slowly reduced to normal pressure, and then the alcohol discharge valve (9) is opened and the esterification water valve (17) is closed.

7. The method for preparing bio-based rigid heat-resistant and environmentally friendly copolyester according to claim 1, characterized in that: The step S3 specifically comprises: starting the vacuum pump (14) to conduct vacuum treatment to enter the pre-polycondensation reaction stage, during which the excess ethylene glycol and the ethylene glycol generated by the polycondensation reaction are distilled into the mixed alcohol receiver (11), and during the vacuuming process, the alcohol distillation state of the mixed alcohol receiver (11) is observed to prevent the vaporized ethylene glycol from being taken out due to excessive vacuuming, and after the vacuum degree reaches a slightly negative pressure state, the stirring is adjusted to a high speed of 40 to 60 Hz for high-speed devolatilization to enter the polycondensation reaction stage, and the temperature is controlled at 260° C. to 290° C. When the power of the stirring shaft rises to 0.150 to 0.300 kW, the polycondensation reaction is terminated, and the heat-resistant copolyester product is generated.

8. The method for preparing bio-based rigid heat-resistant and environmentally friendly copolyester according to claim 1, characterized in that: The dibasic acid added in step S1 is one, two or three of 2,6-naphthalene dicarboxylic acid, terephthalic acid and isophthalic acid; the diol added in step S1 is the bio-based raw material isosorbide, the molar fraction of which accounts for 10%-50% of the total alcohol, and the remainder is one of ethylene glycol and 1,4-cyclohexanedimethanol or two of them in any ratio.

9. The method for preparing bio-based rigid heat-resistant and environmentally friendly copolyester according to claim 1, characterized in that: The catalysts germanium dioxide and cobalt acetate added in step S1 are as follows: the amount of germanium dioxide added is 100-600ppm of the total dibasic acid mass; the amount of cobalt acetate added is 100-400ppm of the total dibasic acid mass; the stabilizer is one or two of phosphoric acid, phosphate esters, and phosphites; and the toner is one or two of color oil or toner powder.

Citation Information

Patent Citations

  • Thermoplastic molded product comprising decorative material

    CN102712210A

  • Isosorbide-modified high-heat-resistance biodegradable polyester and preparation method thereof

    CN111087588A

  • Bio-based copolyester, preparation method and application thereof

    CN113896874A

  • Polyester polyol vacuum production system

    CN201343512Y

  • Aging-resistant polyester film and preparation method therefor

    WO2022142404A1