Bio-based rigid heat-resistant environment-friendly copolyester

By combining rigid structures and bio-based raw materials in bio-based materials, using catalytic stabilization systems and toners, the contradiction between heat-resistant and environmentally friendly polyester is solved, and high-performance bio-based rigid resistance is achieved The preparation of thermal environmentally friendly copolyester significantly improves the heat resistance and carbon footprint of the material.

CN119060310APending Publication Date: 2024-12-03PETROCHINA CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311529055.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-11-16
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

There is a contradiction between the existing heat-resistant and environmentally friendly polyester in improving heat resistance and environmental protection performance, and it is difficult to take into account the rigidity and excellent appearance of the material, and the additives are easily distributed unevenly and are not environmentally friendly.

Method used

Using some bio-based raw materials with rigid structure and compound additives as catalytic stabilization systems, bio-based rigid heat-resistant and environmentally friendly copolyesters are prepared through esterification and polycondensation reactions, including dibasic acid, bio-based diol, catalyst, and stable and toner, control reaction conditions such as temperature and pressure to improve material properties.

Benefits of technology

A catalytic system with high activity, selectivity and stability is achieved. The Tg temperature of bio-based rigid heat-resistant copolyester reaches at least 90°C, a carbon footprint is reduced by 10%, and the heat resistance of the material is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004552964480000051
    Figure BDA0004552964480000051
Patent Text Reader

Abstract

The invention belongs to the technical field of bio-based materials, and discloses bio-based rigid heat-resistant environment-friendly copolyester. The composition comprises dibasic acid, dihydric alcohol, a modified monomer material, a catalyst, a stabilizer and a toner. A catalytic system of the product has the characteristics of high activity, selectivity and stability; the Tg temperature of the bio-based rigid heat-resistant copolyester at least can reach 90 DEG C; the carbon footprint of the bio-based rigid heat-resistant copolyester can be reduced by at least 10%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of bio-based materials, and specifically relates to a bio-based rigid heat-resistant and environmentally friendly copolyester. Background Art

[0002] The development of heat-resistant and environmentally friendly polyester mainly starts from two aspects, one is to improve the heat resistance of the product, and the other is to make the product environmentally friendly. In terms of heat resistance, rigid structure monomers are usually introduced into the molecular structure for copolymerization, which can improve the rigidity and stability of the polyester molecular chain segment. This rigid monomer can be selected from dibasic acids with benzene ring structures, such as terephthalic acid, isophthalic acid, etc., or dibasic acids with naphthalene ring structures such as naphthalene dicarboxylic acid, etc.; rigid diols can also be selected, such as 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, isosorbide, etc.; or through the modification of additives, heat resistance can be improved, but this solution has limited improvement in product heat resistance, and the additives are prone to uneven distribution, affecting the effect, or the additives are not environmentally friendly.

[0003] The environmental performance of the product is achieved by using bio-based monomer raw materials or making them degradable. However, the degradation performance of the material is in conflict with the introduction of a rigid structure to improve heat resistance, and it is impossible to have both. The best way is to use bio-based raw material modification, such as bio-based dibasic acids furandicarboxylic acid, 1,4-butanedioic acid, etc., bio-based diols isosorbide, 1,3-propylene glycol, etc. However, bio-based raw materials often affect the color of the product, and it is difficult to produce products with good appearance, so the selection of bio-based raw materials is also particularly important. Summary of the invention

[0004] In order to overcome the shortcomings of the prior art, the present invention provides a bio-based rigid heat-resistant and environmentally friendly copolyester, which selects some raw materials with rigid structures and bio-based raw materials as modified monomers, and selects compounded additives as the catalytic stabilization system of the synthesis reaction to obtain a bio-based rigid heat-resistant copolyester material through reaction.

[0005] The above-mentioned object of the present invention is achieved through the following technical scheme: a bio-based rigid heat-resistant and environmentally friendly copolyester, the components of which include dibasic acid, diol, modified monomer material, catalyst, stabilizer, and colorant.

[0006] Furthermore, the dibasic acid is one or more of 2,6-naphthalene dicarboxylic acid, terephthalic acid, and isophthalic acid.

[0007] Furthermore, the diol is 10%-50% by mole of bio-based raw material isosorbide, 0%-90% of ethylene glycol and 0%-90% of 1,4-cyclohexanedimethanol.

[0008] Furthermore, the catalyst is germanium dioxide and cobalt acetate.

[0009] In a further preferred embodiment of the present invention, the amount of germanium dioxide added to the catalyst is 100 to 600 ppm by mass of the total dibasic acid, and the amount of cobalt acetate added is 100 to 400 ppm by mass of the total dibasic acid.

[0010] Furthermore, the stabilizer is one or two of phosphoric acid, phosphates, and phosphites.

[0011] Furthermore, the toner is one or both of color oil and color powder.

[0012] Furthermore, in the preparation process of the bio-based rigid heat-resistant and environmentally friendly copolyester, the reaction temperature of the esterification reaction stage is 220-260°C, the reaction pressure is 0.1-0.4MPa, and the reaction time is 60-170 minutes; the condensation reaction temperature in the low vacuum stage is 230-290°C, the reaction pressure is 0-0.1MPa, and the reaction time is 10-60 minutes; the condensation reaction temperature in the high vacuum stage is 250-300°C, the vacuum degree of the reaction system is 50-100Pa, and the reaction time is 60-180 minutes.

[0013] Compared with the prior art, the present invention has the following beneficial effects: the catalytic system of the product has the characteristics of high activity, selectivity and stability; the Tg temperature of the bio-based rigid heat-resistant copolyester can reach at least 90°C; and the carbon footprint of the bio-based rigid heat-resistant copolyester can be reduced by at least 10%. DETAILED DESCRIPTION

[0014] The present invention is described in detail below by specific examples, but the protection scope of the present invention is not limited. Unless otherwise specified, the experimental methods used in the present invention are all conventional methods, and the experimental equipment, materials, reagents, etc. used can be obtained from commercial channels.

[0015] Example 1

[0016] 1500 g of 2,6-naphthalene dicarboxylic acid (2,6-NDA), 482 g of ethylene glycol (EG), 142 g of isosorbide (IS), 140 g of 1,4-cyclohexanedimethanol (CHDM), 0.5 g of germanium dioxide, and 0.25 g of cobalt acetate were added to a 5L stainless steel reactor equipped with a nitrogen inlet, a feed port, a discharge port, a fractionating column, two condensers, and a stirrer. The esterification reaction temperature was 200-250°C, the final esterification reaction temperature was 250°C, the reaction pressure was 0.20-0.25 MPa (gauge pressure), and the reaction time was 180 minutes. After the esterification reaction was completed, 0.25 g of trimethyl phosphate was added to the system for polycondensation reaction. Among them, the condensation reaction temperature in the low vacuum stage is 250-260°C, the reaction pressure is 0-0.1MPa (gauge pressure), the reaction time is 20 minutes, the condensation reaction temperature in the high vacuum stage is 250-285°C, the final temperature of the condensation reaction is 285°C, the vacuum degree of the reaction system is 50-100Pa, and the reaction time is 65 minutes.

[0017] The obtained polymer chips had a glass transition temperature Tg of 120° C., an intrinsic viscosity of 0.605 dL / g, and a molar ratio of isosorbide to diol chain segments of 10%.

[0018] Comparative Example 1 Under the premise that the process conditions remain unchanged relative to Example 1, 1500 grams of terephthalic acid (PTA), 784 grams of ethylene glycol (EG), and 0.875 grams of antimony acetate are added to the reactor. The esterification reaction temperature is 200-250°C, the final esterification reaction temperature is 250°C, the reaction pressure is 0.20-0.25MPa (gauge pressure), and the reaction time is 150 minutes. After the esterification reaction is completed, a polycondensation reaction is carried out. Among them, the polycondensation reaction temperature in the low vacuum stage is 250-260°C, the reaction pressure is 0-0.1MPa (gauge pressure), the reaction time is 20 minutes, the polycondensation reaction temperature in the high vacuum stage is 250-285°C, the final polycondensation reaction temperature is 285°C, the vacuum degree of the reaction system is 50-100Pa, and the reaction time is 110 minutes. The comparative experimental results are shown in Table 1. The results show that the heat resistance of the bio-based rigid heat-resistant copolyester prepared by the present invention is significantly better than that of ordinary polyester.

[0019] Table 1 Example 1 and Comparative Example 1

[0020]

[0021] Example 2

[0022] 1500 g of terephthalic acid (PTA), 196 g of ethylene glycol (EG), 462 g of isosorbide (IS), 911 g of 1,4-cyclohexanedimethanol (CHDM), 0.5 g of germanium dioxide, 0.2 g of cobalt acetate, 0.02 g of blueing agent, and 0.01 g of redding agent were added to a 5L stainless steel reactor equipped with a nitrogen inlet, a feed port, a discharge port, a fractionating column, two condensers, and a stirrer. The esterification reaction temperature was 200-250°C, the final esterification reaction temperature was 250°C, the reaction pressure was 0.20-0.25 MPa (gauge pressure), and the reaction time was 150 minutes. After the esterification reaction was completed, 0.25 g of trimethyl phosphate was added to the system for polycondensation reaction. Among them, the condensation reaction temperature in the low vacuum stage is 250-260°C, the reaction pressure is 0-0.1MPa (gauge pressure), the reaction time is 20 minutes, the condensation reaction temperature in the high vacuum stage is 250-270°C, the final temperature of the condensation reaction is 270°C, the vacuum degree of the reaction system is 50-100Pa, and the reaction time is 130 minutes.

[0023] The obtained polymer chips had a glass transition temperature Tg of 90° C., an intrinsic viscosity of 0.66 dL / g, and a molar ratio of isosorbide to diol chain segments of 25%.

[0024] Example 3

[0025] 1310 g of terephthalic acid (PTA), 190 g of 2,6-naphthalene dicarboxylic acid (2,6-NDA), 685 g of ethylene glycol (EG), 179 g of isosorbide (IS), 0.5 g of germanium dioxide, and 0.25 g of cobalt acetate were added to a 5L stainless steel reactor equipped with a nitrogen inlet, a feed port, a discharge port, a fractionating column, two condensers, and a stirrer. The esterification reaction temperature was 200-250°C, the final esterification reaction temperature was 250°C, the reaction pressure was 0.20-0.25 MPa (gauge pressure), and the reaction time was 160 minutes. After the esterification reaction was completed, 0.25 g of trimethyl phosphate was added to the system for polycondensation reaction. Among them, the condensation reaction temperature in the low vacuum stage is 250-260°C, the reaction pressure is 0-0.1MPa (gauge pressure), the reaction time is 20 minutes, the condensation reaction temperature in the high vacuum stage is 250-280°C, the final temperature of the condensation reaction is 280°C, the vacuum degree of the reaction system is 50-100Pa, and the reaction time is 115 minutes.

[0026] The obtained polymer chips had a glass transition temperature Tg of 90° C., an intrinsic viscosity of 0.63 dL / g, and a molar ratio of isosorbide to diol chain segments of 10%.

[0027] Example 4

[0028] 1200 g of terephthalic acid (PTA), 300 g of isophthalic acid (IPA), 196 g of ethylene glycol (EG), 462 g of isosorbide (IS), 911 g of 1,4-cyclohexanedimethanol (CHDM), 0.6 g of germanium dioxide, 0.2 g of cobalt acetate, 0.02 g of blueing agent, and 0.01 g of redding agent were added to a 5L stainless steel reactor equipped with a nitrogen inlet, a feed port, a discharge port, a fractionating column, two condensers, and a stirrer. The esterification reaction temperature was 200-250°C, the final esterification reaction temperature was 250°C, the reaction pressure was 0.20-0.25 MPa (gauge pressure), and the reaction time was 155 minutes. After the esterification reaction was completed, 0.25 g of trimethyl phosphate was added to the system for polycondensation reaction. Among them, the condensation reaction temperature in the low vacuum stage is 250-260°C, the reaction pressure is 0-0.1MPa (gauge pressure), the reaction time is 20 minutes, the condensation reaction temperature in the high vacuum stage is 250-270°C, the final temperature of the condensation reaction is 270°C, the vacuum degree of the reaction system is 50-100Pa, and the reaction time is 150 minutes.

[0029] The obtained polymer chips had a glass transition temperature Tg of 90° C., an intrinsic viscosity of 0.62 dL / g, and a molar ratio of isosorbide to diol chain segments of 25%.

[0030] Example 5

[0031] 1165 g of terephthalic acid (PTA), 146 g of isophthalic acid (IPA), 189 g of 2,6-naphthalene dicarboxylic acid (2,6-NDA), 609 g of ethylene glycol (EG), 179 g of isosorbide (IS), 177 g of 1,4-cyclohexanedimethanol (CHDM), 0.5 g of germanium dioxide, and 0.25 g of cobalt acetate were added to a 5L stainless steel reactor equipped with a nitrogen inlet, a feed port, a discharge port, a fractionating column, two condensers, and a stirrer. The esterification reaction temperature was 200-250°C, the final esterification reaction temperature was 250°C, the reaction pressure was 0.20-0.25 MPa (gauge pressure), and the reaction time was 150 minutes. After the esterification reaction was completed, 0.25 g of trimethyl phosphate was added to the system for polycondensation. Among them, the condensation reaction temperature in the low vacuum stage is 250-260°C, the reaction pressure is 0-0.1MPa (gauge pressure), the reaction time is 20 minutes, the condensation reaction temperature in the high vacuum stage is 250-285°C, the final temperature of the condensation reaction is 285°C, the vacuum degree of the reaction system is 50-100Pa, and the reaction time is 130 minutes.

[0032] The obtained polymer chips had a glass transition temperature Tg of 95° C., an intrinsic viscosity of 0.65 dL / g, and a molar ratio of isosorbide to diol chain segments of 10%.

[0033] The above-described embodiments are only preferred embodiments of the present invention, but not all feasible embodiments of the present invention. For those skilled in the art, any obvious changes made thereto without departing from the principles and spirit of the present invention should be considered to be included in the scope of protection of the claims of the present invention.

Claims

1. A bio-based rigid heat-resistant and environmentally friendly copolyester, It is characterized in that The ingredients include dibasic acid, diol, modified monomer material, catalyst, stabilizer and toner.

2. The bio-based rigid heat-resistant and environmentally friendly copolyester according to claim 1, It is characterized in that The dibasic acid is one or more of 2,6-naphthalene dicarboxylic acid, terephthalic acid and isophthalic acid.

3. The bio-based rigid heat-resistant and environmentally friendly copolyester according to claim 1, It is characterized in that The diols are 10%-50% by mole of isosorbide, a bio-based raw material, 0%-90% of ethylene glycol and 0%-90% of 1,4-cyclohexanedimethanol.

4. The bio-based rigid heat-resistant and environmentally friendly copolyester according to claim 1, It is characterized in that The catalyst is germanium dioxide and cobalt acetate.

5. The bio-based rigid heat-resistant and environmentally friendly copolyester according to claim 4, It is characterized in that The amount of germanium dioxide added to the catalyst is 100-600 ppm of the total mass of the dibasic acid, and the amount of cobalt acetate added is 100-400 ppm of the total mass of the dibasic acid.

6. The bio-based rigid heat-resistant and environmentally friendly copolyester according to claim 1, It is characterized in that The stabilizer is one or two of phosphoric acid, phosphates and phosphites.

7. The bio-based rigid heat-resistant and environmentally friendly copolyester according to claim 1, It is characterized in that The toner is one or both of color oil and color powder.

8. The bio-based rigid heat-resistant and environmentally friendly copolyester according to claim 1, It is characterized in that In the preparation process of the bio-based rigid heat-resistant and environmentally friendly copolyester, the reaction temperature of the esterification reaction stage is 220-260°C, the reaction pressure is 0.1-0.4MPa, and the reaction time is 60-170 minutes; the condensation reaction temperature of the low vacuum stage is 230-290°C, the reaction pressure is 0-0.1MPa, and the reaction time is 10-60 minutes; the condensation reaction temperature of the high vacuum stage is 250-300°C, the vacuum degree of the reaction system is 50-100Pa, and the reaction time is 60-180 minutes.

Citation Information

Patent Citations

  • Heat resistant polyethylene terephthalate and a process for the preparation of the same

    CN105392816A

  • Isosorbide-modified high-heat-resistance biodegradable polyester and preparation method thereof

    CN111087588A

  • Preparation method of rigid copolyester

    CN114591496A

  • Polyester resin copolymerized with isosorbide and 1,4- cyclohexane dimethanol and preparing method thereof

    KR1020170037588A