Polyimide super-smooth surface with self-repairing performance and preparation method and application thereof
By preparing polyimide ultraslip surfaces in ultraslip surface materials, using the polycondensation reaction of APT-PDMS with IPDI and TPAL, the problem of insufficient stability and self-repair capabilities of existing ultraslip surface materials is solved, and efficient Self-healing, drag reduction and antibacterial properties are suitable for applications in complex environments.
Patent Information
- Application Number
- CN202411290439.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-14
AI Technical Summary
The existing ultra-slip surface materials are not stable, lubricating oil is easily taken away and the surface is easily damaged, lacking self-repair ability, and cannot show excellent performance in multiple repairs and resistance to crack wounds.
By preparing a polyimide ultraslip surface, polycondensation reaction with IPDI and TPAL is carried out in the presence of silicone oil by using APT-PDMS to form SLIPS with self-healing properties. By changing the molecular weight and reaction conditions of APT-PDMS, the stability of the material is improved. Sex and self-healing ability.
It realizes excellent self-repairing ability, drag reduction and antibacterial properties of ultra-slip surfaces, enhances the stability and multiple repair capabilities of the material, and can quickly restore the lubricating layer after the substrate is damaged, suitable for anti-fouling and Antibacterial applications.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the field of super-slippery surface materials, and in particular relates to a simple preparation method of a super-slippery surface with self-repairing performance and the prepared super-slippery surface material. Background Art
[0002] In 2011, Joanna Aizenberg and her team at Harvard University were inspired by the insect-catching principle of pitcher plants and first proposed the concept of Slippery liquid infused porous super-slippery surface (SLIPS). Because the surface is a liquid-liquid surface composed of a smooth, continuous and uniform lubricating oil layer. Therefore, it has the properties of anti-icing and antifreeze, antibacterial, drag reduction, and self-repair. In recent years, super-slippery surfaces have been one of the research hotspots. Super-slippery surfaces are formed by infusing various types of lubricating fluids into micro-nano structures, among which the construction of the solid phase substrate with a rough structure is very important. However, with the complexity of social life, the stability of super-slippery surfaces is not high, the lubricating oil is easily carried away, and the surface is easily damaged. Therefore, it is of great significance to prepare SLIPS with self-repairing properties.
[0003] CN201811485363.3 A method for preparing a bionic super-slippery surface with self-healing properties at room temperature, using aminopropyl-terminated polydimethylsiloxane (APT-PDMS) and isophorone diisocyanate (IPDI) in the presence of lubricating oil to form a bionic super-slippery surface, which does not involve the preparation and application of polyimide super-slippery surfaces, and the average velocity and drag reduction rate in water (G) and oil (H) are not studied, and the different group reactions used have a great influence on the performance.
[0004] In CN202211423884.2, a rough substrate composed of polyimide microspheres is prepared by combining inverse emulsion polymerization and drop coating, and finally oil is poured to form a lubricating oil layer to form a super-slip surface with a sliding angle of <10°. Soaking silicone oil can only form silicone oil on the surface of the coating, rather than encapsulating silicone oil. When the silicone oil layer on the surface of the coating is damaged, the silicone oil molecules inside the coating will spontaneously migrate to the coating. Therefore, when the substrate is damaged, the performance of the lubricating layer will disappear and it will not have self-repairing ability. Secondly, a self-repairable elastomer is prepared in CN202210600757.9 and CN202310392396.8, and disulfide compounds are present in the monomer. Different monomers, different reaction orders, different reaction conditions and different performances. In addition, the presence of disulfide compounds will also affect the stability of the super-slip surface. CN201710665115.6 A highly transparent, super-lubricating, self-replenishing glass coating and its preparation method and application. The glass coated with PDMS coating is immersed in dimethyl silicone oil, so that the silicone oil molecules penetrate the internal network skeleton of the PDMS coating and the coating surface. When the silicone oil layer on the surface of the coating is damaged, the silicone oil molecules inside the coating will spontaneously migrate to the coating surface, showing excellent self-replenishing performance. It mainly uses external silicone oil to repair the lubricating oil layer. The repair requires the internal silicone oil molecules to spontaneously replenish the surface. The silicone oil consumption is large, and the repair ability will be lost when it is consumed. Therefore, it cannot achieve the effect of multiple repairs, and the cracks and wounds caused by the coating cannot be repaired. Summary of the invention
[0005] The purpose of the present invention is to provide a simple preparation method of a super-slippery surface with self-repairing properties and the super-slippery surface material obtained.
[0006] In order to achieve the purpose of the present invention, the technical solution adopted is:
[0007] A simple method for preparing a super-slippery surface with self-repairing properties comprises the following steps:
[0008] (1) Preparation of APT-PDMS: Octamethylcyclotetrasiloxane (D4) and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane were used as monomers and tetramethylammonium hydroxide ((Me)4NOH) was used as a catalyst to obtain amino-terminated polydimethylsiloxane (APT-PDMS) through a ring-opening reaction. The structural formula of APT-PDMS is as follows:
[0009]
[0010] The mass ratio of octamethylcyclotetrasiloxane to 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane is 10-50:2-3, and the obtained APT-PDMS molecular weight ranges from 1000 to 6000; wherein as the molecular weight of APT-PDMS increases, the mechanical properties of the self-healing elastomer increase.
[0011] (2) PDMS m IT-oil n Preparation: Dissolve silicone oil in tetrahydrofuran and stir magnetically at room temperature. Add APT-PDMS and a certain amount of THF to a round-bottom flask and stir thoroughly under a nitrogen atmosphere (10 min). Slowly add a mixed solvent of IPDI and THF to the reaction system and stir at a reaction temperature of 60°C for 12 h. Dissolve TPAL in THF and add it to the flask. Continue stirring at the reaction temperature for at least 24 h before the reaction is complete. Named PDMS m IT-oil n , wherein m is the molecular weight of APT-PDMS, and n is the mass of silicone oil (g), specifically 3 to 5.
[0012] The molar ratio of APT-PDMS:IPDI:TPAL is 1-3:2.4:0.6. The usage ratio of IPDI and silicone oil is 2.4:3-5 mmol / g.
[0013] (3) Preparation of super-slippery surface: PDMS m IT-oil n , 2,2'-bis[4-(4-aminophenoxyphenyl)]propane (BAPP) and 1,2,4,5-cyclohexanetetracarboxylic dianhydride (HPMDA) were subjected to polycondensation. After the reaction, the mixture was poured into a square Teflon mold, and the mold and sample were degassed in a vacuum oven at 50-60°C for 12 hours to obtain a super-slip surface of the polyimide. m -IT x -oil n Indicates; where X represents PDMS m IT-oil n The mass ratio of BAPP to HPMDA is 1:1; and n is the mass of silicone oil.
[0014] Furthermore, PDMS m IT-oil n The mass ratio of BAPP and HPMDA is 5 to 20:1:1; the preferred mass ratio is 5 to 10:1:1.
[0015] Further, PDMS was weighed m IT-oil nDissolve BAPP in a mixed solvent of THF and CH3OH and react under vacuum for 1 hour. Then add HPMDA three times by starvation feeding method and react for 6 hours in an ice bath. After 2 hours of chemical imidization, pour it into a square Teflon mold, degas the mold and sample in a vacuum oven at 50℃ for 12 hours, and obtain a series of polyimide superslippery surfaces.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] The present invention uses PDMS m IT-oil n , BAPP and HPMDA as raw materials, and by adding silicone oil into the reaction system, a polyimide superslippery surface with self-healing properties was prepared. m IT-oil n , the mass ratio of BAPP to HPMDA, and other conditions were discussed. The material has self-healing properties and SLIPS is more stable. The prepared super-slippery surface has excellent self-healing ability, drag reduction and antibacterial properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is the APT-PDMS reaction formula in step (1) of Example 1;
[0019] Figure 2 PDMS in step (2) of Example 1 m IT x -oil3 reaction formula;
[0020] Figure 3 PDMS prepared in Example 1 m IR curve of IT-oil3 (A) and IR spectrum of polyimide containing polysiloxane with self-healing properties (B);
[0021] Figure 4 Polarized microscope images of the super-slippery surface of polyimide containing polysiloxane with self-healing properties prepared with different molecular weights and the same mass ratio (A.Mn APT-PDMS =1676, APT-PDMS:BAPP:HPMDA=5:1:1; B.Mn APT-PDMS =3060, APT-PDMS:BAPP:HPMDA=5:1:1; C.Mn APT-PDMS =5162, APT-PDMS:BAPP:HPMDA=5:1:1);
[0022] Figure 5 This is the antibacterial test diagram of the super-slippery surface of polyimide containing polysiloxane with self-healing properties.
[0023] Figure 6 The photos of pure glass pieces in motion (A, D), P m IT-oil0(B,E),P m Average velocity and drag reduction of IT-oil3 (C,F) underwater (AC) and oil surface (DF) samples in water (G) and oil (H).
[0024] Figure 7 For super-slippery surface (P m IT-oil3) Water drop sliding diagram before and after scratching and after self-repair.
[0025] Figure 8 P m IT5-oil0, P m IT 10 -oil0,P m IT 15 -oil0 and P m IT 20 -oil0APT-PDMS with different molecular weights, different BAPP and PDMS m Stress-strain curve of IT-oil0 mass ratio.
[0026] Fig. 9 P 1676 IT x -oil3, P 3060 IT x -oil3, P 5162 IT x - Comparison of the healing effects of oil3 at 60°C and room temperature. DETAILED DESCRIPTION
[0027] The present invention is not limited to the following specific embodiments. A person skilled in the art can implement the present invention in various other specific embodiments according to the contents disclosed in the present invention, or any simple changes or modifications made to the design structure and ideas of the present invention fall within the protection scope of the present invention. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict.
[0028] The present invention is further described in detail below in conjunction with embodiments:
[0029] Embodiment 1:
[0030] (1) Preparation of APT-PDMS (Mn=5162)
[0031] 44.5 g of octamethylcyclotetrasiloxane (D4) and 2.5 g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane were weighed separately and added into a three-necked round-bottom flask. Then 0.6 g of catalyst tetramethylammonium hydroxide ((Me)4NOH) was weighed and used as a catalyst for ring opening under a dry N2 atmosphere at a reaction condition of 105°C. After 18 hours of reaction, the temperature was raised to 180°C to degrade the catalyst, and then cooled to 160°C to remove low-boiling small molecular impurities and other by-products to obtain a colorless viscous APT-PDMS liquid (Mn=5162).
[0032] (2) PDMS 5162 Synthesis of IT-oil3
[0033] First, take 3g of silicone oil and dissolve it in 10ml of THF, and stir it magnetically at room temperature for 10 minutes. Then take 5g of APT-PDMS and 10mL of THF and add them to a 250mL round-bottom flask, and stir for 10 minutes under a nitrogen atmosphere. Add 2.44mmol of isophorone diisocyanate (IPDI) to 5mL of THF, slowly drip it into the flask, and stir it for 12h under a nitrogen atmosphere at 60°C. Then dissolve 0.61mmol of terephthalaldehyde (TPAL) in 5mL of THF, add it to the flask, and stir at 60°C for 24h before the reaction is completed to obtain PDMS. 5162 IT-oil3.
[0034] (3) Preparation of super-slippery surfaces
[0035] Weigh 1.1435g PDMS at room temperature 5162 IT-oil3 and 0.2287g 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) were dissolved in a mixed solvent of THF and CH3OH (mass ratio 15:85) and reacted under vacuum conditions for 1h. Then, 0.2287g 1,2,4,5-cyclohexanetetracarboxylic dianhydride (HPMDA) was added three times by the starvation feeding method and reacted in an ice bath for 6h. After 2h of chemical imidization, it was poured into a square Teflon mold, and the mold and sample were degassed in a vacuum oven at 50℃ for 12h. The obtained polyimide superslippery surface was treated with P 5162 -IT5-oil3 indicates.
[0036] The static contact angle of the SLIPS prepared in Example 1 was 102°, and the sliding angle was 4°.
[0037] Embodiment 2:
[0038] (1) Preparation of APT-PDMS (Mn=3060)
[0039] 25.4 g of D4 and 2.5 g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane were weighed separately and added into a three-necked round-bottom flask. Then 0.6 g of catalyst (Me)4NOH was weighed and used as a catalyst for ring opening in a dry N2 atmosphere at a reaction condition of 105 °C. After 18 h of reaction, the temperature was raised to 180 °C to degrade the catalyst, and then the temperature was lowered to 160 °C to remove low-boiling small molecular impurities and other by-products to obtain a colorless viscous APT-PDMS liquid (Mn=3060).
[0040] (2) PDMS 3060 The preparation of IT-oil3 was the same as in Example 1.
[0041] (3) The method for preparing the superslippery surface is the same as in Example 1, and P is obtained. 3060 -IT5-oil3.
[0042] The static contact angle of SLIPS prepared in Example 2 was 102° and the sliding angle was 5°.
[0043] Embodiment 3:
[0044] (1) Preparation of APT-PDMS (Mn=1676)
[0045] 11.8 g of D4 and 2.5 g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane were weighed separately and added into a three-necked round-bottom flask. Then 0.6 g of catalyst (Me)4NOH was weighed and used as a catalyst for ring opening in a dry N2 atmosphere at a reaction condition of 105 °C. After 18 h of reaction, the temperature was raised to 180 °C to degrade the catalyst, and then cooled to 160 °C to remove low-boiling small molecular impurities and other by-products to obtain colorless viscous APT-PDMS liquids of different molecular weights.
[0046] (2) PDMS 1676 The preparation method of IT-oil3 is the same as that of Example 1.
[0047] (3) The method for preparing the superslippery surface is the same as in Example 1, and P is obtained. 1676 -IT5-oil3.
[0048] The static contact angle of the SLIPS prepared in Example 3 was 103.5° and the sliding angle was 6°.
[0049] Comparative Example 1
[0050] (1) The preparation method of APT-PDMS is the same as that of Example 1;
[0051] (2) PDMS 5162 Synthesis of IT-oil3
[0052] First, take 3g of silicone oil and dissolve it in 10ml of dimethylacetamide (DMAc) under nitrogen atmosphere, and stir magnetically at room temperature for 10min. Then take 5g of APT-PDMS and 10mL of DMAc and add them to a 250mL round-bottom flask, and stir for 10min under nitrogen atmosphere. Add 2.44mmol of IPDI to 5mL of DMAc, slowly drip it into the flask, and stir for 12h under nitrogen atmosphere at 60℃. Then dissolve 0.61mmol of TPAL in 5mL of DMAc, add it to the flask, stir at 60℃ for 24h, and the reaction is completed to obtain PDMS. 5162 IT-oil3.
[0053] (3) Preparation of super-slippery surfaces
[0054] Weigh 1.1435 PDMS at room temperature 5162 IT-oil3 and 0.2287g BAPP were dissolved in DMAc and reacted under vacuum for 1 hour. Then, 0.2287g HPMDA was added three times by starvation feeding method and reacted in ice bath for 6 hours. After 2 hours of chemical imidization, it was poured into a square Teflon mold, and the mold and sample were degassed in a vacuum oven at 50℃ for 12 hours.
[0055] The main difference between Comparative Example 1 and Example 1 is that the selected solvent is different. In Comparative Example 1, both step (2) and step (3) use DMAc.
[0056] In Comparative Example 1, DMAc is not miscible with silicone oil, and the material finally prepared does not have the performance of SLIPS.
[0057] Comparative Example 2
[0058] (1) The preparation method of APT-PDMS is the same as that of Example 1
[0059] (2) PDMS m Synthesis of IT-oil0
[0060] Take 5g APT-PDMS and 10mL THF and add them to a 250mL round-bottom flask, and stir for 10min under nitrogen atmosphere. Add 2.44mmol IPDI to 5mL THF, slowly drip into the flask, and stir for 12h under nitrogen atmosphere at 60℃. Then dissolve 0.61mmol TPAL in 5mL THF, add it to the flask, and stir at 60℃ for 24h before the reaction is completed to obtain PDMS. 5162 IT-oil3.
[0061] (3) Preparation of super-slippery surfaces
[0062] Weigh 1.1435g PDMS at room temperature5162 IT-oil3 and 0.2287g BAPP were dissolved in a mixed solvent of THF and CH3OH and reacted under vacuum for 1h. Then, 0.2287g HPMDA was added three times by the starvation feeding method and reacted in an ice bath for 6h. After 2h of chemical imidization, it was poured into a square Teflon mold, and the mold and sample were degassed in a vacuum oven at 50℃ for 12h.
[0063] Compared with Example 1, the main difference between Comparative Example 2 and Example 1 is that: m IT-oil n No silicone oil was added during the preparation. No silicone oil was added in Comparative Example 2, so the final prepared material did not have the performance of SLIPS, WCA: 105°, SA: 18°. Because it does not contain silicone oil, the system does not have self-healing properties.
[0064] Comparative Example 3
[0065] The difference between Comparative Example 3 and Example 1 is that no phthalaldehyde is added. The other operations are the same as those of Example 1. The material prepared in Comparative Example 3 does not have self-healing properties.
[0066] In addition, the following comparative tests were conducted: PDMS m Tests of super-slippery surfaces with self-healing properties prepared with different mass ratios of IT-oil3, BAPP and HPMDA. As shown in Table 1, SLIPS has the best sliding performance when the mass ratio is 5:1:1.
[0067] Table 1: Monomer addition amount formula of polymer and wettability analysis of SLIPS with different ratios
[0068]
[0069] Table 2
[0070]
[0071]
[0072] Figure 1 Reaction formula for the synthesis of APT-PDMS; Figure 2 For the synthesis of PDMS m IT-oil3 reaction formula;
[0073] Figure 3 Curve a in (A) is PDMS m IT-oil n Curve b is APT-PDMS; curve c is the infrared image of IPDI. Curve b is at 3332cm -1 The characteristic absorption peak of -NH2- is 2962cm-1 and 2905cm -1 The two peaks are the stretching vibration absorption peaks of the methyl group attached to the silicon atom of the main chain, 1093 cm -1 and 1020cm -1 The left and right are the stretching vibration peaks of the main chain Si—O, indicating that APT-PDMS was successfully synthesized.
[0074] Figure 3 Curve a in (A) is PDMS m IT-oil n Compared with IPDI (curve c), the infrared curve of 2256cm in curve a -1 The significant characteristic peaks caused by the asymmetric stretching vibration of the -NCO group disappeared, proving that the IPDI reaction was complete. -1 The 1636cm2 and 1636cm3 are the stretching vibration and shear vibration of NH. -1 The vibration absorption peak at is C=O, which further confirms that the imine bond and urea group exist simultaneously in PDMS. m IT-oil3.
[0075] Figure 3 (B) is the infrared spectrum of polyimide containing polysiloxane with self-healing properties. 1390cm -1 There is a characteristic absorption peak of CN at 1780cm -1 and 1717cm -1 The asymmetric and symmetric stretching vibrations of C=O in the imide ring are 804 cm -1 It is the bending vibration of C=O, which proves that the polyimide containing polysiloxane with self-healing properties was successfully synthesized.
[0076] Figure 4 Polarized microscope images of the ultra-slippery surface of polyimide containing polysiloxane with self-healing properties prepared with different molecular weights and the same mass ratio. 1676 IT5-oil3, P 3060 IT5-oil3 and P 5162 IT5-oil3 was used to study the self-healing properties of the samples. Figure 4 The self-healing process was detected using a polarizing microscope. Without external force extrusion, the sample began to heal together after 12 hours at 60°C, and the sample gradually healed after 24 hours. From Figure (A) to Figure (C), it can be seen that at the same temperature and the same time, as the molecular weight of APT-PDMS increases, the self-healing efficiency of the substrate increases. This is because the increase in molecular weight improves fluidity and flexibility, allowing for rapid repair.
[0077] Figure 5This is the antibacterial test diagram of the super-slip surface of polyimide containing polysiloxane with self-healing properties. (Coating plate method. Escherichia coli), it can be seen that compared with pure glass and porous surfaces (porous material P 5162 The number of bacterial adhesion sites on the polyimide super-slip surface is reduced, so the number of surface colonies is reduced, and it has excellent anti-bacterial adhesion.
[0078] Figure 6 The photos of pure glass pieces in motion (A, D), P m IT-oil0-X(B,E),P m IT-oil3-X(C,F); A, B, C are in water; D, E, F are in oil for drag reduction performance testing. Figure 6 It can be seen that when the liquid medium is water, pure glass, P 5162 IT5-oil0, P 5162 The average velocities of IT5-oil3 were 25, 35.3, and 40 cm·s -1 The sailing time was measured and the average sailing speed (v) and drag reduction rate (r) were calculated as follows:
[0079]
[0080] Where v is the average speed calculated from the measured sailing time, t is the sailing time, R is the drag reduction rate, V0 and V are the speeds of the pure sheet and the test sample, respectively. Each drag reduction rate was tested three times to get the average value.
[0081] Therefore, P 5162 IT5-oil0, P 5162 The drag reduction rates of IT5-oil3 are approximately 44.2% and 68%, respectively.
[0082] P 5162 The drag reduction rate of IT5-oil0 is lower than that of P 5162 The drag reduction rate of IT5-oil3 is due to P 5162 There is a solid-liquid interface between IT5-oil0 and water, and a strong adsorption force will be generated between the two interfaces, increasing resistance and reducing speed. 5162 The original solid-liquid interface between IT5-oil3 and water is transformed into a liquid-liquid interface, reducing the resistance and achieving the drag reduction effect. The drag reduction mechanism of the sample is shown in Figures (A) and (B). When P 5162 IT5-oil0, P 5162 When IT5-oil3 sails on the surface of low surface energy and high viscosity peanut oil, the sailing speed is reduced to a certain extent. 5162 IT5-oil0, P 5162The drag reduction rate of IT5-oil3 was reduced to 41.3% and 59%. 5162 There is a solid-liquid interface between IT5-oil0 and peanut oil, and some peanut oil will adhere to the substrate surface. 5162 The drag reduction effect of IT5-oil0 in oil is reduced. 5162 There is a layer of silicone oil on the surface of IT5-oil3, as shown in Figure (B). The immiscible silicone oil and peanut oil form a liquid-liquid interface, which has good non-wetting properties and enhances the P 5162 The drag reduction effect of IT5-oil3 on the oil surface. The working environment of the hull surface materials and underwater parts will contain a large amount of water, oil, microorganisms, organic matter and other pollutants. Taking the above factors into consideration, the present invention P 5162 IT5-oil3 has a broad application prospect in underwater anti-fouling and drag reduction materials.
[0083] Figure 7 For super-slippery surface (P m IT x -oil3) Water droplet sliding diagram before and after scratching and after self-repair. When the super-slippery surface is repeatedly cut by the blade, the water drop stops moving at the scratch. When the substrate self-repairs, new lubricating oil is released from the substrate to form a new lubricating oil layer, and the water drop can still slide smoothly from the repaired surface. Therefore, the surface has excellent self-repairing properties.
[0084] Figure 8 P m IT5-oil0, P m IT 10 -oil0,P m IT 15 -oil0 and P m IT 20 -oil0APT-PDMS with different molecular weights, different BAPP and PDMS m Figures (EH) show the stress-strain curves of IT-oil0 mass ratio. m IT5-oil3, P m IT 10 -oil3, P m IT 15 -oil3 and P m IT 20 Comparison of stress-strain curves of APT-PDMS with different molecular weights and different mass ratios of BAPP to PDMSmIT-oil0. 1676 IT5-oil0,bP 3060 IT5-oil0,cP 5162IT5-oil0.(B)aP 1676 IT 10 -oil0,bP 3060 IT 10 -oil0,cP 5162 IT 10 -oil0.(C)aP 1676 IT 15 -oil0,bP 3060 IT 15 -oil0,c.
[0085] P 5162 IT 15 -oil0.(D)aP 1676 IT 20 -oil0,bP 3060 IT 20 -oil0,cP 5162 IT 20 -oil0.(E)aP 1676 IT5-oil3,bP 3060 IT5-oil3,cP 5162 IT5-oil3.(F)aP 1676 IT 10 -oil3,bP 3060 IT 10 -oil3,cP 5162 IT 10 -oil3.(G)aP 1676 IT 15 -oil3,bP 3060 IT 15 -oil3,cP 5162 IT 15 -oil3.(H)aP 1676 IT 20 -oil3,bP 3060 IT 20 -oil3,cP 5162 IT 20 -oil3.]
[0086] After curing at room temperature and 60 °C for 24 h, the molecular weight of APT-PDMS and PDMS m The increase of IT-oil3, P m IT x The healing rate of -oil3 gradually increased. This is because the flexibility of the elastomer molecular chain accelerates the rapid healing of the fracture surface. The self-healing efficiency is calculated by the tensile strain, and the formula is as follows:
[0087]
[0088] HE original and HE healed are the average tensile strains of the original and healed specimens, respectively. Each self-healing efficiency was tested three times to obtain the average value.
[0089] The mechanical properties of the self-healing elastomers depend largely on the molecular weight of APT-PDMS and the m The content of IT-oil3. Figure 8 (H) It can be seen that P 1676 IT 20 -oil3 has good mechanical properties, with a tensile strength of about 0.1009MPa, an elongation at break of about 922.81%, and P 3060 IT 20 -oil3 tensile strength is about 0.0566MPa, elongation at break is about 1005.03%, P 5162 IT 20 -oil3 has a tensile strength of only 0.0484MPa, and the highest elongation at break is about 1049.16%. This is because the intermolecular hydrogen bonds formed by the urea group act as physical crosslinking points. In addition, the high content of TPAL improves the flexibility of the self-healing elastomer, but reduces the physical crosslinking.
[0090] Fig. 9 The self-healing properties of the samples after 24 h of healing at room temperature and 60 °C were compared. 1676 IT x -oil3 self-healing efficiency, (B) P after recovery at room temperature (RT) and 60℃ for 24h 3060 IT x -oil3 self-healing efficiency and (C) P after recovery at room temperature (RT) and 60℃ for 24h 5162 IT x -oil3 self-healing efficiency. When the sample is healed at 60℃ 1676 IT x -oil3, P 3060 IT x -oil3, P 5162 IT x -oil3 healing rate compared with room temperature 1676 IT x -oil3, P 3060 IT x -oil3, P 5162 IT x -oil3's healing rate increased by about 15%, which shows that increasing the temperature can improve the mobility of molecular segments.
[0091] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a polyimide super-slippery surface with self-healing properties, Features: The steps include: (1) Preparation of APT-PDMS: Using octamethylcyclotetrasiloxane and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane as monomers and tetramethylammonium hydroxide as catalyst, an amino-terminated polydimethylsiloxane liquid was prepared by ring-opening reaction under heating conditions, which was referred to as APT-PDMS. (2) PDMS m IT-oil n Synthesis: PDMS was prepared using silicone oil, APT-PDMS, isophorone diisocyanate and terephthalaldehyde as raw materials. m IT-oil n ; Wherein m is the molecular weight of APT-PDMS, the range of m is 1000 to 6000, and n is the mass of silicone oil; (3) Preparation of polyimide superslippery surface: PDMS m IT-oil n The polycondensation reaction was carried out with 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) and 1,2,4,5-cyclohexanetetracarboxylic dianhydride (HPMDA). After the reaction, the sample was poured onto a substrate and degassed in a vacuum oven to obtain a polyimide superslippery surface with self-healing properties, which was calculated as P m IT x -oil n ; x is PDMS m IT-oil n The mass ratio of x to BAPP is 5-20.
2. The method for preparing a polyimide super-slippery surface with self-repairing properties according to claim 1, Features: The mass ratio of octamethylcyclotetrasiloxane to 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane is 10-50:2-3.
3. The method for preparing a polyimide super-slippery surface with self-repairing properties according to claim 1, Features: Step (2) PDMS m IT-oil n The specific steps include: dissolving silicone oil in tetrahydrofuran, adding a tetrahydrofuran solution of APT-PDMS therein, stirring under a nitrogen atmosphere, adding a tetrahydrofuran solution of isophorone diisocyanate, stirring under a nitrogen atmosphere, adding a tetrahydrofuran solution of terephthalaldehyde under heating conditions, stirring under heating conditions to react, and obtaining PDMS. m IT-oil n ; The molar ratio of APT-PDMS:IPDI:TPAL is =1~3:2.4:0.6; the usage ratio of IPDI and silicone oil is 2.4:3~5mmol / g.
4. The method for preparing a polyimide super-slippery surface with self-repairing properties according to claim 3, Features: The reaction temperature is 60°C and the reaction time is at least 12 hours.
5. The simple preparation method for preparing a super-slippery surface material with self-repairing properties according to claim 1, Features: The specific steps of step (3) include: weighing PDMS at room temperature m IT-oil 3 Dissolve BAPP in THF and CH 3 OH mixed solvent, react under vacuum conditions, then add HPMDA in batches, react in an ice bath, pour on the substrate after chemical imidization, and degas in a vacuum oven to obtain a polyimide super-smooth surface.
6. The simple preparation method for preparing a super-slippery surface material with self-repairing properties according to claim 1, Features: THF and CH 3 The mass ratio of OH is 15:
85.
7. The simple preparation method for preparing a super-slippery surface material with self-repairing properties according to claim 1, Features: PDMS m IT-oil 3 The mass ratio with BAPP and HPMDA is 5-20:1:
1.
8. The simple preparation method for preparing a super-slippery surface material with self-repairing properties according to claim 7, Features: PDMS m IT-oil 3 The mass ratio with BAPP and HPMDA is 5-10:1:
1.
9. An ultra-slip surface material with self-repairing properties prepared according to the method according to any one of claims 1 to 8.
10. Application of the ultra-lubricating surface material with self-repairing properties prepared by the method according to any one of claims 1 to 8 in ultra-lubricity, self-repairing, drag reduction and antibacterial properties.
Citation Information
Patent Citations
Method for preparing bionic super-smooth surface with self-repairing performance at room temperature
CN109627946A
Preparation method of silicon dioxide hybrid polyimide super-smooth surface material with good stability
CN115536901A
Simple preparation method of super-smooth surface composed of polyimide composite microspheres
CN115678098A
Crosslinked polydimethylsiloxane elastomer material and preparation method thereof
CN115873256A
Self-repairing organic silicon-based triboelectric material and preparation method thereof
CN118580498A