Polyarylene sulfide and preparation method thereof

By controlling the molar ratio and reaction conditions of the sulfonate monomer and dihalogenated aromatic compounds in the polyphenylene sulfide, a polyarylene sulfide with uniform sulfonation unit distribution was prepared, which solved the uneven distribution and performance during the sulfonation process. The loss problem has achieved the high temperature and high strength performance and hydrophilicity of polyphenylene sulfide, and is suitable for high-performance proton exchange membranes.

CN119060339APending Publication Date: 2024-12-03XIN NING HE KE JI (CHENG DU) YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411384688.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing polyphenylene sulfides have uneven distribution of sulfonic acid groups during the sulfation process, which affects their performance. The traditional method uses concentrated sulfuric acid to lead to performance losses and environmental pollution.

Method used

Using sulfur-containing substances, passivated sulfonic acid monomers and dihalogenated aromatic compounds as raw materials, polyarylene sulfides with uniform sulfonation unit distribution are prepared by controlling the molar ratio and reaction conditions, and polyphenylene sulfides are retained. It has high temperature resistance and high strength properties, while enhancing its hydrophilicity and proton exchange functions.

Benefits of technology

The uniform distribution of sulfonated units in polyaryl sulfide is achieved, which improves its polarity and hydrophilicity, while maintaining the high temperature and high strength properties and corrosion resistance of the original polyphenylene sulfide, which is suitable for high-quality proton exchange membranes and other highs. Performance application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005070731670000027
    Figure BDA0005070731670000027
  • Figure BDA0005070731670000031
    Figure BDA0005070731670000031
  • Figure BDA0005070731670000041
    Figure BDA0005070731670000041
Patent Text Reader

Abstract

The invention belongs to the field of high polymer materials, and particularly relates to high-molecular-weight linear polyarylene sulfide with uniformly distributed sulfonation groups and a preparation method of the high-molecular-weight linear polyarylene sulfide. According to the invention, the polyarylene sulfide with a controllable structure and uniformly distributed sulfonation groups is prepared by taking a sulfur-containing substance, a sulfonic monomer and a dihalogenated aromatic compound as raw materials. The polyarylene sulfide has the advantages of excellent proton and ion exchange performance, good mechanical property and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer materials, specifically relating to high molecular weight linear polyarylene sulfides with uniformly distributed sulfonated groups and their preparation methods. Background Technology

[0002] Polyphenylene sulfide (PPS) Polyoxymethylene (POM) is the largest category of special engineering plastics and is hailed as the "world's sixth largest engineering plastic" after polycarbonate (PC), polyester (PET), polyoxymethylene (POM), nylon (PA), and polyphenylene oxide (PPO). It is also one of the eight major aerospace materials.

[0003] (1) It is a linear or slightly branched polymer composed of alternating benzene rings and sulfur atoms, with strong molecular chain regularity. The main chain, which is connected by rigid benzene rings and flexible sulfide bonds, has the characteristics of both rigidity and flexibility, so polyphenylene sulfide can crystallize (its raw powder has a crystallinity of up to 75% and a melting point of up to 285℃);

[0004] (2) Since the benzene ring on the main chain forms a conjugate with the sulfur atom and the sulfur atom is not yet saturated, oxidation can transform the sulfide bond into a sulfoxide group and a sulfone group or cause the benzene ring and adjacent macromolecules to form oxygen bridges or crosslinks, but does not break the main chain. Therefore, it has outstanding thermal and oxygen stability, with a maximum continuous operating temperature of 260℃ and a thermal decomposition temperature of 522℃.

[0005] (3) Due to the conjugation of the sulfur atom by the benzene ring and the high crystallinity, the entire polymer exhibits non-polar or weakly polar characteristics, thus its electrical insulation, dielectric properties and chemical resistance are also very prominent.

[0006] (4) Since polyphenylene sulfide has good compatibility with many polymers and additives, it can be modified by means of blending, reinforcement, alloying, etc. to improve its physical and mechanical properties.

[0007] PPS has a wide range of applications, primarily in the automotive, electronics, machinery, petrochemical, pharmaceutical, light industry, and specialized fields such as military and aerospace. PPS resin has also been used to create high-performance specialty fibers and films, expanding its applications in environmental protection and clean energy sectors.

[0008] Because PPS is a repeating unit formed by the combination of a benzene ring and a sulfur element: Its structure exhibits high rigidity and inertness, demonstrating excellent stability and corrosion resistance. However, this also limits its application in highly polar fields, such as proton exchange membranes and water electrolysis for hydrogen production. These fields require membranes with high hydrophilicity, capable of exchanging ions such as hydrogen and lithium, providing pathways for cation exchange. To meet the needs of these fields, various modifications have been made to polyphenylene sulfide (PPS), mainly including PPS synthetic structural modification and PPS resin grafting chemical modification. Synthetic structural modification includes the preparation of polyphenylene sulfide sulfone. Polyphenylene sulfide ketone Polyphenylene sulfide amide etc.; or forming copolymers, such as polyphenylene sulfide-polyphenylene sulfide sulfone copolymers. Alternatively, a polar side group, such as a hydroxyl group, may be introduced into the benzene ring during the synthesis of polyphenylene sulfide. The side group is a carboxyl group. Another method involves further modifying the synthesized PPS resin through chemical reactions, such as oxidizing the sulfur portion to sulfone to increase polarity, or sulfonating it with concentrated sulfuric acid to graft sulfonic acid structures onto the benzene ring. Among these methods, the use of concentrated sulfuric acid to sulfonate polyphenylene sulfide (PPS) is frequently reported, transforming PPS into a water-soluble and water-swellable product and altering its polarity and hydrophilicity. However, this method requires large amounts of concentrated sulfuric acid, the sulfonation of the benzene ring on the molecular chain is highly random, and the sulfonic acid groups cannot be specifically and uniformly distributed on the benzene ring of the molecular chain. Furthermore, the sulfonation process is accompanied by oxidation, which significantly affects the properties of PPS. Shanghai University prepared a proton exchange membrane copolymer with a sulfonated polyphenylene sulfone (ketone)-phenylene sulfide structure via copolymerization using thiophenol as a monomer.

[0009] Y2 = -SO2-, -CO-, etc. (CN1651485A). Although this type of sulfonated polyarylene sulfide exhibits significantly enhanced polarity and hydrophilicity, and is almost completely soluble in water, it does not possess the traditional polyphenylene sulfide structure. Its performance is significantly different from that of polyphenylene sulfide. Summary of the Invention

[0010] To achieve a structure with uniformly distributed sulfonic acid groups that provides proton exchange functionality, enhances the polarity and hydrophilicity of polyphenylene sulfide (PPS), and maintains its excellent rigidity, strength, and corrosion resistance, this invention preserves the structural unit of PPS. A molecular-type sulfonated polyarylene sulfide with a quantitative sulfonation unit structure is provided.

[0011] The technical solution of this invention:

[0012] The first technical problem to be solved by the present invention is to provide a type of polyarylene sulfide, which is prepared using sulfur-containing substances, passivated sulfonic acid monomers, and dihaloaromatic compounds as raw materials; wherein, the sulfur-containing substance is sodium sulfide or sodium hydrosulfide, and the sulfonic acid monomer is selected from at least one of 4,4-dihalodiphenyl sulfone-3,3-disulfonic acid, 2,5-dichlorobenzenesulfonic acid, 3,5-dichlorobenzenesulfonic acid, 2,4-dichlorobenzenesulfonic acid, 4-amino-2,5-dichlorobenzenesulfonic acid, 2,5-dichlorophenylhydrazine-4-sulfonic acid, or 2,5-dihalo-4-carboxymethylbenzenesulfonic acid; the passivation refers to converting the protons in the sulfonic acid monomer into metal ions; the ratio of the molar number of sulfur-containing substances to the total molar number of sulfonic acid monomers and dihaloaromatic compounds is 0.95-1.05:1.0, and the molar ratio of sulfonic acid monomers to dihaloaromatic compounds is 50.0-5.0:60.0-95.0.

[0013] Furthermore, in the above-mentioned polyaryl sulfide, the metal ion is selected from Li. + K + Na + Ba 2+ 、Sr 2+ .

[0014] Furthermore, in the above-mentioned polyarylene sulfide, the passivation can be achieved by mixing and reacting the sulfonic acid monomer and the hydroxide of the metal ion in water or an organic solvent.

[0015] Furthermore, in the above-mentioned polyaryl sulfides, the dihaloaromatic compound is selected from 1,4-dihalobenzene, 2,4-dihalobenzene, 3,5-dihalobenzene, 4,4'-dihalobiphenyl, 4,4'-dihalodiphenyl sulfone, 4,4'-dihalobenzophenone, or 4,4'-dihalodiphenyl ether. More preferably, the dihaloaromatic compound is selected from 1,4-dichlorobenzene, 2,4-m-dichlorobenzene, 4,4'-dichlorodiphenyl sulfone, or 4,4'-dichlorobenzophenone.

[0016] Furthermore, the above-mentioned polyarylene sulfide is selected from the structures shown in formulas I, II, III, IV, 1, 2, 3, 4, 5, or 6:

[0017]

[0018]

[0019] In the above formulas, each Z is independently selected from -NH2, -NHHN2, -OH or -COOH, and each M is independently selected from Li. + K + Na + Ba 2+ or Sr 2+ Each m is independently ≥2.

[0020] The second technical problem to be solved by the present invention is to provide a method for preparing the above-mentioned polyarylene sulfide. This method includes the following steps: reacting dehydrated sodium sulfide or sodium hydrosulfide, passivated sulfonic acid monomer, and dihaloaromatic compound in a solvent.

[0021] Furthermore, in the above preparation method, the solvent is a polar aprotic solvent. Even further, the solvent is selected from N-methyl-2-pyrrolidone (NMP), hexamethylphosphoramide (HMPA), N,N-dimethylacetamide, N,N-dimethylamide, N-ethylcaprolactam, N,N-vinylpyrrolidone, caprolactam, tetramethylurea, dimethyl sulfoxide, or sulfolane.

[0022] Furthermore, in the above preparation method, the reaction involves heating the system to 200–250°C and reacting for 2–5 hours, and then heating it to 250–300°C and reacting for another 2–5 hours.

[0023] Furthermore, the preparation method of the above-mentioned polyarylene sulfide includes the following steps: under nitrogen protection, the sulfur-containing substance is stirred and heated. When the temperature reaches 190-200°C, dehydration is stopped, and the temperature is lowered to below 130°C. Then, passivated sulfonic acid monomers and dihalo aromatic compounds are added, and the air in the reactor is replaced with nitrogen. The temperature is then raised to 200-250°C and reacted for 2-5 hours. After that, the temperature is raised to 250-300°C and reacted for 2-5 hours to end the polymerization reaction. Then, the temperature is lowered to below 130°C, deionized water is added, the reactor is stirred, the discharge valve is opened, and the product is filtered and separated.

[0024] Furthermore, the preparation method of the above-mentioned polyarylene sulfide includes the following steps: under nitrogen protection, the sulfur-containing substance is stirred and heated. When the temperature reaches 190-200℃, dehydration is stopped, and the temperature is cooled to below 130℃. Then, passivated sulfonic acid monomers and dihalo aromatic compounds are added, and the air in the reactor is replaced with nitrogen. The temperature is then raised to 200-250℃ and reacted for 2-5 hours. After that, the temperature is raised to 250-300℃ and reacted for 2-5 hours to end the polymerization reaction. Then, the temperature is cooled to 180-200℃, and part of the solvent is recovered by flash evaporation. After that, the temperature is lowered to below 130℃, deionized water is added, the reactor outlet valve is opened with stirring, and the product is filtered and separated. The filtrate enters the solvent recovery tower to separate and recover the solvent, water, and by-product sodium halide for reuse.

[0025] The polyaryl sulfide containing sulfonic acid units prepared by this invention has a controllable number of sulfonated units and forms a random copolymer structure with uniformly distributed sulfonated groups. This invention controls the content and uniform distribution of sulfonated units from the polymer structure, retaining the original high-temperature resistance and high strength properties of polyphenylene sulfide, while also taking into account proton exchange, ion exchange functions, strength, and hydrophilicity. Detailed Implementation

[0026] This invention uses dehydrated sodium sulfide or sodium hydrosulfide, passivated sulfonic acid monomers, and dihaloaromatic compounds as raw materials to prepare a class of polyarylene sulfides. These polyarylene sulfides possess a random copolymer structure with a controllable number of sulfonated units and a uniform distribution of sulfonated groups.

[0027] The present invention relates to polyarylene sulfide, which is prepared using sulfur-containing substances, passivated sulfonic acid monomers, and dihaloaromatic compounds as raw materials; the ratio of the molar number of sulfur-containing substances to the total molar number of (sulfonic acid monomers + dihaloaromatic compounds) is 0.95-1.05:1.0, and the molar ratio or mass ratio of sulfonic acid monomers to dihaloaromatic compounds is 50.0-5.0:60.0-95.0.

[0028] This invention provides a polyarylene sulfide of Formula I, which is a sulfonated proton-type polyarylene sulfide:

[0029]

[0030] Where m≥2.

[0031] This invention provides a polyarylene sulfide of Formula II, which is a sulfonated proton-type polyarylene sulfide:

[0032]

[0033] Where Z is selected from -NH2, -NHHN2, -OH or -COOH, and m≥2.

[0034] This invention provides a polyarylene sulfide of Formula III, which is a sulfonated ionic polyarylene sulfide:

[0035]

[0036] Wherein, M is selected from Li + K + Na + Ba 2+ or Sr 2+ , m≥2.

[0037] This invention provides a polyarylene sulfide of formula IV, which is a sulfonated ionic polyarylene sulfide:

[0038]

[0039]

[0040] Wherein, Z is selected from -NH2, -NHHN2, -OH or -COOH, and M is selected from Li. + K + Na + Ba 2+or Sr 2+ , m≥2. The polyarylethers shown in the above formulas I, II, III, and IV have ternary structures.

[0041] This invention provides a polyarylene sulfide of Formula 1, which is a sulfonated proton-type polyarylene sulfide:

[0042]

[0043] Where m≥2.

[0044] This invention provides a polyarylene sulfide of Formula 2, which is a sulfonated ionic polyarylene sulfide:

[0045]

[0046] Wherein, M is selected from Li + K + Na + Ba 2+ or Sr 2+ , m≥2.

[0047] This invention provides a polyarylene sulfide of Formula 3, which is a sulfonated ionic polyarylene sulfide:

[0048]

[0049] Wherein, M is selected from Li + K + Na + Ba 2+ or Sr 2+ , m≥2.

[0050] This invention provides a polyarylene sulfide of Formula 4, which is a sulfonated proton-type polyarylene sulfide:

[0051]

[0052] Where Z is selected from -NH2, -NHHN2, -OH or -COOH, and m≥2.

[0053] This invention provides a polyarylene sulfide of Formula 5, which is a sulfonated proton-type polyarylene sulfide:

[0054]

[0055] This invention provides a polyarylene sulfide of Formula 6, which is a sulfonated ionic polyarylene sulfide:

[0056]

[0057] Wherein, M is selected from Li + K +Na + Ba 2+ or Sr 2+ .

[0058] The polyarylene sulfides shown in formulas 1, 2, 3, 4, 5, and 6 above have a binary structure.

[0059] In this invention, in order to ensure the number of sulfonated groups with quantitative distribution in the design, and to guarantee the mechanical properties, corrosion resistance, heat resistance, and high polarity, proton or ion exchange performance of the designed polyarylene sulfide, the m value in the above structure is ≥2.

[0060] The preparation method of the polyarylene sulfide of the present invention includes the following steps: reacting dehydrated sodium sulfide or sodium hydrosulfide, passivated sulfonic acid monomer and dihaloaromatic compound in a solvent, and obtaining the polyarylene sulfide after post-treatment.

[0061] In this invention, the sulfonic acid monomers used are selected from 4,4-dihalodiphenylsulfone-3,3-disulfonic acid, 2,5-dichlorobenzenesulfonic acid, 3,5-dichlorobenzenesulfonic acid, 2,4-dichlorobenzenesulfonic acid, 4-amino-2,5-dichlorobenzenesulfonic acid, 2,5-dichlorophenylhydrazine-4-sulfonic acid, and 2,5-dihalo-4-carboxymethylbenzenesulfonic acid.

[0062] Furthermore, the structure of 4,4-dihalodiphenyl sulfone-3,3-disulfonic acid is as follows: X is selected from F, Cl, Br, or I. The structure of 2,5-dichlorobenzenesulfonic acid is... The structure of 3,5-dichlorobenzenesulfonic acid is: The structure of 2,4-dichlorobenzenesulfonic acid is: The structure of 4-amino-2,5-dichlorobenzenesulfonic acid is as follows: The structure of 2,5-dichlorophenylhydrazine-4-sulfonic acid is as follows: The structure of 2,5-dihalo-4-carboxymethylbenzenesulfonic acid is as follows: X is selected from F, Cl, Br, and I.

[0063] In this invention, to avoid affecting the polymerization of dihaloaromatic compounds with sodium sulfide or sodium hydrosulfide, the sulfonic acid monomer needs to be passivated by converting the protons in the sulfonic acid monomer into metal ions, such as Li, that do not affect the polymerization of dihaloaromatic compounds with sodium sulfide or sodium hydrosulfide. + K + Na + Ba 2+ and Sr 2+ wait.

[0064] Passivation methods include, for example: or

[0065] The reaction is carried out using stoichiometric proportions, i.e., 1 mol of sulfonic acid groups Corresponding to 1 mol Li + K + Na + or 1 / 2 mol Ba 2+ 、Sr 2+ The passivation reaction can be carried out in aqueous solution or in polar organic solvents (e.g., NMP, DMF, DMAc, etc.). This passivation reaction is a conventional acid-base reaction in the art.

[0066] In this invention, sodium sulfide is generally selected as the sulfide ion donor. Since sodium sulfide typically exists in the forms of triphia (Na₂S·3H₂O), pentahydrate (Na₂S·5H₂O), and nechohydrate (Na₂S·9H₂O), water removal is necessary during the polymerization reaction. For example, under an inert gas such as nitrogen to prevent oxidation of the sodium sulfide, the temperature is increased while stirring, and dehydration is stopped when the temperature reaches 190-200°C.

[0067] In this invention, the dihaloaromatic compound is selected from 1,4-dihalobenzene, 2,4-dihalobenzene, 3,5-dihalobenzene, 4,4'-dihalobiphenyl, 4,4'-dihalodiphenyl sulfone, 4,4'-dihalobenzophenone, or 4,4'-dihalodiphenyl ether. More preferably, the dihaloaromatic compound is selected from 1,4-dichlorobenzene, 2,4-m-dichlorobenzene, 4,4'-dichlorodiphenyl sulfone, or 4,4'-dichlorobenzophenone.

[0068] In this invention, the polymerization reaction of polyarylene sulfides uses a polar aprotic solvent as the reaction medium, such as N-methyl-2-pyrrolidone (NMP), hexamethylphosphoramide (HMPA), N,N-dimethylacetamide, N,N-dimethylamide, N-ethylcaprolactam, N,N-vinylpyrrolidone, caprolactam, tetramethylurea, dimethyl sulfoxide, or sulfolane. The amount of polar aprotic solvent used is 50–500 mL per mole of polymer monomer (i.e., the total molar amount of sulfonic acid monomer + dihaloaromatic compound or the total molar amount of sodium sulfide).

[0069] The polymerization reaction of polyarylene sulfides in this invention is illustrated below:

[0070]

[0071] In this invention, the polymerization reaction of polyarylene sulfide is divided into the following three stages: (1) sodium sulfide dehydration stage, (2) adding passivated sulfonic acid monomers and dihalo aromatic compounds to polymerize and form oligomers with randomly and uniformly distributed benzenesulfonic acid groups, and (3) forming linear high molecular weight polyarylene sulfide with randomly and uniformly distributed benzenesulfonic acid groups.

[0072] In this invention, the polymerization reaction of polyarylene sulfides involves dehydrating sodium sulfide using an inert gas such as nitrogen to prevent oxidation. Under nitrogen protection, the temperature is raised while stirring. Dehydration is stopped when the temperature reaches 190–200°C, and then the temperature is lowered to below 130°C. Then, the passivated sulfonic acid monomer and dihaloaromatic compound are added to the reactor. The air inside the reactor is replaced with nitrogen, and the temperature is raised to 200–250°C for 2–5 hours. The reaction is then raised to 250–300°C for another 2–5 hours to complete the polymerization reaction. The reactor is then cooled to 180–200°C, and some solvent is recovered by flash evaporation. Afterward, the temperature is lowered to below 130°C, deionized water is added, the reactor outlet valve is opened with stirring, and the product is filtered and separated. The filtrate enters a solvent recovery tower for the separation, recovery, and reuse of the solvent, water, and byproduct sodium halide.

[0073] After transferring polyphenylene sulfide containing sulfonate structure to deionized water, stirring, and washing 6-9 times: (1) Sulfonate ionic polyaryl sulfide is dried at 80-120℃ for 8-20 hours to obtain linear high molecular weight polyaryl sulfide with randomly and uniformly distributed benzenesulfonic acid groups; (2) Protonation reaction of proton-type sulfonated polyaryl sulfide: When it is necessary to restore it to proton-type sulfonated polyaryl sulfide, the product does not enter the drying process. The washed product is directly transferred to an acid-resistant ceramic kettle, and a certain amount of dilute sulfuric acid or dilute hydrochloric acid is added to carry out the protonation reaction. The reaction diagram is as follows:

[0074] The amount of dilute sulfuric acid or dilute hydrochloric acid added exceeds 5%-10% of the passivation sulfonic acid groups.

[0075] The further processing method for the linear high molecular weight polyarylene sulfide with randomly and uniformly distributed benzenesulfonic acid groups of the present invention is as follows:

[0076] The polyarylene sulfide obtained from the above polymerization and post-treatment was granulated using a twin-screw extruder at an extrusion temperature of 300-350℃. The temperatures of the first to fourth screw sections were 300-310℃, 310-320℃, 315-325℃, and 300-310℃, respectively. The resulting granules were then injection molded into mechanical specimens at 310-350℃ using an injection molding machine for testing.

[0077] The linear high molecular weight polyarylether sulfide granules with randomly and uniformly distributed benzenesulfonic acid groups were drawn into films using a casting machine. The temperature of the first to fourth sections of the screw was 300-350℃, and the rotation speed of the take-up roller was 10-300 mm / min. Through the casting process, a cast film with a thickness of 10-250 μm was formed, and its hydrophilicity angle was tested.

[0078] Performance testing of this invention:

[0079] Molecular weight and viscosity: expressed using melt flow index, measured in grams per 10 minutes at 315°C and 5 kg pressure; g / 10min.

[0080] Sulfonation degree test: The acid-base titration method is used. DS (sulfonation degree, relative value, compared with PPS) = CV / [CV+(m1-CVM1) / M2], where C is the molar concentration of sodium hydroxide, m1 is the mass of polyarylene sulfide containing sulfonated groups, M1 is the mass of pure PPS unit, and M2 is the total mass of polymer units containing a certain amount of sulfonic acid groups.

[0081] Membrane thickness: Labthink CHY-C2A thickness gauge.

[0082] Polyaryl sulfides: Polarity - Water contact angle:

[0083] Samples were fabricated into 2×2 cm thin films for water contact angle testing. Test conditions included room temperature, a seated drop method with a drop volume of 2 μL, and six parallel measurements for each film sample. Statistical analysis was performed using OriginPro 2022b. All data are expressed as mean ± standard deviation. Normality was tested using the Kolmogorov-Smirnov method, homogeneity of variance was tested using the Levene method, and mean comparisons were performed using the Scheffe test in One Way ANOVA.

[0084] Melting point: The DSC test was performed using a Mettler Toledo DSC 3+ differential scanning calorimeter in a nitrogen atmosphere. The sample was first heated from 40°C to 320°C at a heating rate of 10°C / min, held at 320°C for 5 min to eliminate thermal history, and then cooled to 40°C at a cooling rate of 10°C / min. Finally, it was heated to 320°C at a heating rate of 10°C / min.

[0085] Mechanical performance testing: routine mechanical testing.

[0086] Example 1 (Ternary Structure of Polyarylether Sulfide Backbone)

[0087] (1) 2.24 kg of 4,4-dihalodiphenyl sulfone-3,3-disulfonic acid ( Dissolve X=Cl in 10L of deionized water, add 400g of sodium hydroxide, and stir for 20 minutes. Add 1.14kg of 2,5-dichlorobenzenesulfonic acid to 200g of sodium hydroxide and stir for 20 minutes.

[0088] (2) Preparation of polyaryl sulfides containing sulfonic acid groups: 50L of N-methylpyrrolidone (NMP), 17.33kg of sodium sulfide (45%), the above-mentioned sodium 4,4-dihalodiphenyl sulfone-3,3-disulfonic acid solution, and the above-mentioned sodium 2,5-dichlorobenzenesulfonate solution were added to a 100L reactor; then, under nitrogen protection, the mixture was stirred and heated to 200℃, and the fractionated water was cooled and recovered through a cooling tower; 13.23kg of p-dichlorobenzene was added, and the temperature was gradually increased to 225℃, reacting at this temperature for 3 hours, then gradually increased to 260℃ and reacting for 3 hours, then cooled to 130℃ and deionized water was slowly added, filtered, and washed once. The first and second filtrates were combined, and the combined filtrate was sent to a distillation column to separate water and NMP, and the byproduct sodium chloride was collected. Then, the mixture was washed 6 times with deionized water at 60℃.

[0089] (3) Add the above undried resin to 20L of dilute sulfuric acid solution (containing 0.75kg of sulfuric acid) and stir for 2 hours. Then filter, wash 6 times with deionized water at room temperature, and dry under vacuum at 100℃ for 12 hours to obtain protonated sulfonated polyarylene sulfide.

[0090] (4) The sulfonic acid-containing polyarylene sulfide resin obtained in (3) was extruded and granulated using a twin-screw extruder at 300-350℃. The first stage temperature was 310℃, the second stage temperature was 320℃, the third stage temperature was 325℃, and the fourth stage temperature was 310℃. The extrusion speed was 25 kg / h. Mechanical specimens were injection molded at 310-350℃ using an injection molding machine for testing.

[0091] (5) Film casting of the sulfonic acid-containing polyarylene sulfide resin obtained in (3): The sulfonic acid-containing polyarylene sulfide resin obtained in (3) was cast into a film using a casting machine. The temperatures of the first to fourth sections of the screw were 310℃, 325℃, 325℃, and 315℃, respectively, and the rotation speed of the take-up roller was 100 mm / min. By controlling the roller rotation speed and tension during the casting process, two casting films with thicknesses of 10 μm and 250 μm were formed, and their hydrophilicity angle and other properties were tested.

[0092] Performance parameter testing:

[0093] (i) Melt index (g / 10min): 230

[0094] (ii) DS (%): 35%

[0095] (iii) Membrane hydrophilicity angle (°): 36

[0096] (iv) Melting point (DSC test, heating rate 2℃ / min): 286

[0097] (v) Tensile strength (MPa): 69; Flexural strength (MPa): 95; Modulus (GPa): 3.6

[0098] Example 2 (same as Example 1, except the protonation process is omitted)

[0099] (1) Step 1 is the same as step 1 in Example 1.

[0100] (2) Preparation of polyarylene sulfides containing sulfonic acid groups: 50L of NMP and 17.33kg of sodium sulfide (45%) were added to a 100L reactor. The above-mentioned sodium 4,4-dihalodiphenyl sulfone-3,3-disulfonic acid solution and sodium 2,5-dichlorobenzenesulfonic acid solution were also added. The mixture was then heated to 200℃ under nitrogen protection with stirring. The fractionated water was cooled and recovered using a cooling tower. 13.23kg of p-dichlorobenzene was added. The temperature was gradually increased to 225℃ and reacted at this temperature for 3 hours. Then, the temperature was gradually increased to 260℃ and reacted for another 3 hours. The mixture was cooled to 130℃, and deionized water was slowly added. After filtration and washing once, the first and second filtrates were combined. The combined filtrate was sent to a distillation column to separate water and NMP, and the byproduct sodium chloride was collected. The mixture was then washed 6 times with deionized water at 60℃ and dried under vacuum at 100℃ for 12 hours to obtain ionized sulfonated polyarylene sulfides.

[0101] (3) Remove this process (protonation reaction).

[0102] (4) The sulfonic acid-containing polyarylene sulfide resin obtained in (2) was extruded and granulated using a twin-screw extruder at 300-350℃. The first stage temperature was 310℃, the second stage temperature was 320℃, the third stage temperature was 325℃, and the fourth stage temperature was 310℃. The extrusion speed was 25 kg / h. Mechanical specimens were injection molded using an injection molding machine at 310-350℃ for testing.

[0103] (5) The sulfonic acid-containing polyarylene sulfide resin granules obtained in (4) were stretched into films: the temperatures of the first to fourth sections of the screw were 310℃, 325℃, 325℃ and 315℃, and the rotation speed of the take-up roller was 100mm / min. By controlling the roller rotation speed and tension during the casting process, two types of cast films with thicknesses of 10 and 250μm were formed, and their hydrophilicity angle and other properties were tested.

[0104] (6) Determination of sulfonation degree: The sulfonation degree was determined according to Example 1, i.e., protonation followed by titration: The above-mentioned undried resin was added to 20L of dilute sulfuric acid solution (containing 0.75kg of sulfuric acid) and stirred for 2 hours. Then it was filtered, washed 6 times with deionized water at room temperature, and dried under vacuum at 100℃ for 12 hours to obtain protonated sulfonated polyarylene sulfide.

[0105] Performance parameter testing:

[0106] (i) Melt index (g / 10min): 190

[0107] (ii) DS (%): 35%

[0108] (iii) Membrane hydrophilicity angle (°): 32

[0109] (iv) Melting point (DSC test, heating rate 2℃ / min): 288

[0110] (v) Tensile strength (MPa): 70; Flexural strength (MPa): 95; Modulus (GPa): 3.7

[0111] Example 3 (same as Example 1, but with barium ions passivated for benzenesulfonic acid)

[0112] (1) 2.24 kg of 4,4-dihalodiphenyl sulfone-3,3-disulfonic acid ( X=Cl) is dissolved in 10L of deionized water, 856g of barium hydroxide is added, and the mixture is stirred for 20 minutes for later use (emulsion); 1.14kg of 2,5-dichlorobenzenesulfonic acid is added to 429g of barium hydroxide, and the mixture is stirred for 20 minutes for later use (emulsion).

[0113] (2)-(5) Same as Example 1.

[0114] Performance parameter testing:

[0115] (i) Melt index (g / 10min): 180

[0116] (ii) DS (%): 35%

[0117] (iii) Hydrophilic angle (°): 38

[0118] (iv) Melting point (DSC test, heating rate 2℃ / min): 287

[0119] (v) Tensile strength (MPa): 72; Flexural strength (MPa): 100; Modulus (GPa): 3.8 Example 4 (same as Example 1, polyarylene sulfide main chain ternary structure, different content of benzenesulfonic acid unit)

[0120] (1) 3.36 kg of 4,4-dihalodiphenyl sulfone-3,3-disulfonic acid ( Dissolve X=Cl in 10L of deionized water, add 600g of sodium hydroxide, and stir for 20 minutes. Add 200g of sodium hydroxide to 1.14kg of 2,5-dichlorobenzenesulfonic acid and stir for 20 minutes.

[0121] (2) Preparation of polyarylene sulfides containing sulfonic acid groups: 50 L of NMP and 17.33 kg of sodium sulfide (45%) were added to a 100 L reactor. The above-mentioned sodium 4,4-dihalodiphenyl sulfone-3,3-disulfonic acid solution and sodium 2,5-dichlorobenzenesulfonic acid solution were also added. The mixture was then heated to 200 °C under nitrogen protection with stirring. The fractionated water was cooled and recovered using a cooling tower. 12.88 kg of p-dichlorobenzene was added. The temperature was gradually increased to 225 °C and reacted at this temperature for 3 hours. Then, the temperature was gradually increased to 260 °C and reacted for another 3 hours. The mixture was cooled to 130 °C, and deionized water was slowly added. After filtration and washing once, the first and second filtrates were combined. The combined filtrate was sent to a distillation column to separate water and NMP, and the byproduct sodium chloride was collected. The mixture was then washed 6 times with deionized water at 60 °C.

[0122] (3) Add the above undried resin to 25L of dilute sulfuric acid solution (containing 0.75kg of sulfuric acid) and stir for 2 hours. Then filter, wash 6 times with deionized water at room temperature, and dry under vacuum at 100℃ for 12 hours to obtain protonated sulfonated polyarylene sulfide.

[0123] (4)-(5) Same as Example 1.

[0124] Performance parameter testing:

[0125] (i) Melt index (g / 10min): 270

[0126] (ii) DS (%): 45%

[0127] (iii) Hydrophilic angle (°): 26

[0128] (iv) Melting point (DSC test, heating rate 2℃ / min): 285

[0129] (v) Tensile strength (MPa): 65; Flexural strength (MPa): 88; Modulus (GPa): 3.5

[0130] Example 5 (same as Example 1, except that the benzenesulfonic acid unit is replaced with a single unit, forming a binary structure)

[0131] (1) 2.24 kg of 4,4-dihalodiphenyl sulfone-3,3-disulfonic acid ( Dissolve X=Cl in 10L of deionized water, add 400g of sodium hydroxide, and stir for 20 minutes.

[0132] (2) Preparation of polyarylene sulfides containing sulfonic acid groups: 50L of NMP and 17.33kg of sodium sulfide (45%) were added to a 100L reactor, along with the above-mentioned sodium 4,4-dihalodiphenyl sulfone-3,3-disulfonic acid solution. The mixture was then heated to 200℃ under nitrogen protection with stirring. The fractionated water was cooled and recovered using a cooling tower. 13.96kg of p-dichlorobenzene was added. The temperature was gradually increased to 225℃ and reacted at this temperature for 3 hours. Then, the temperature was gradually increased to 260℃ and reacted for another 3 hours. The mixture was cooled to 130℃, and deionized water was slowly added. After filtration and washing once, the first and second filtrates were combined. The combined filtrate was sent to a distillation column to separate water and NMP, and the byproduct sodium chloride was collected. The mixture was then washed 6 times with deionized water at 60℃.

[0133] (3) Add the above undried resin to 15L of dilute sulfuric acid solution (containing 0.75kg of sulfuric acid) and stir for 2 hours. Then filter, wash 6 times with deionized water at room temperature, and dry under vacuum at 100℃ for 12 hours to obtain protonated sulfonated polyarylene sulfide.

[0134] (4)-(5) Same as Example 1.

[0135] Performance parameter testing:

[0136] (i) Melt index (g / 10min): 160

[0137] (ii)DS(%): 25

[0138] (iii) Hydrophilic angle (°): 45

[0139] (iv) Melting point (DSC test, heating rate 2℃ / min): 288

[0140] (v) Tensile strength (MPa): 72; Flexural strength (MPa): 100; Modulus (GPa): 3.8

[0141] Example 6 (same as Example 5, but with double the content of 4,4-dihalodiphenyl sulfone-3,3-disulfonic acid)

[0142] (1) 4.48 kg of 4,4-dihalodiphenyl sulfone-3,3-disulfonic acid ( Dissolve X=Cl in 10L of deionized water, add 800g of sodium hydroxide, and stir for 20 minutes.

[0143] (2) Preparation of polyarylene sulfides containing sulfonic acid groups: 50L of NMP and 17.33kg of sodium sulfide (45%) were added to a 100L reactor, along with the above-mentioned sodium 4,4-dihalodiphenyl sulfone-3,3-disulfonic acid solution. The mixture was then heated to 200℃ under nitrogen protection with stirring. The fractionated water was cooled and recovered using a cooling tower. 13.23kg of p-dichlorobenzene was added. The temperature was gradually increased to 225℃ and reacted at this temperature for 3 hours. Then, the temperature was gradually increased to 260℃ and reacted for another 3 hours. The mixture was cooled to 130℃, and deionized water was slowly added. After filtration and washing once, the first and second filtrates were combined. The combined filtrate was sent to a distillation column to separate water and NMP, and the byproduct sodium chloride was collected. The mixture was then washed 6 times with deionized water at 60℃.

[0144] (3)-(5) Same as Example 1.

[0145] Performance parameter testing:

[0146] (i) Melt index of the product (g / 10min): 210

[0147] (ii) DS (%): 40%

[0148] (iii) Hydrophilic angle (°): 30

[0149] (iv) Melting point (DSC test, heating rate 2℃ / min): 287

[0150] (v) Tensile strength (MPa): 69; Flexural strength (MPa): 88; Modulus (GPa): 3.6

[0151] Example 7 (same as Example 6, but with strontium hydroxide passivated benzenesulfonic acid)

[0152] (1) 4.48 kg of 4,4-dihalodiphenyl sulfone-3,3-disulfonic acid ( Dissolve X=Cl in 10L of deionized water, add 1.22kg of strontium hydroxide, and stir for 20 minutes (emulsion).

[0153] (2)-(5) Same as Example 6.

[0154] Performance parameter testing:

[0155] (i) Melt index (g / 10min): 185

[0156] (ii) DS (%): 38%

[0157] (iii) Hydrophilic angle (°): 32

[0158] (iv) Melting point (DSC test, heating rate 2℃ / min): 288

[0159] (v) Tensile strength (MPa): 69; Flexural strength (MPa): 87; Modulus (GPa): 3.7 Example 8 (same as Example 1, except that 4,4-dihalodiphenylsulfone-3,3-disulfonic acid is removed, and only 2,5-dichlorobenzenesulfonic acid is used, with a binary main chain structure)

[0160] (1) Add 1.14 kg of 2,5-dichlorobenzenesulfonic acid and 200 g of sodium hydroxide to 10 L of water and stir for 20 minutes.

[0161] (2) Preparation of polyarylene sulfides containing sulfonic acid groups: 50L NMP and 17.33kg sodium sulfide (45%) were added to a 100L reactor, along with the above-mentioned sodium 2,5-dichlorobenzenesulfonate solution. The mixture was then heated to 200℃ under nitrogen protection with stirring. The fractionated water was cooled and recovered via a cooling tower. 13.96kg of p-dichlorobenzene was added. The temperature was gradually increased to 225℃ and reacted at this temperature for 3 hours. Then, the temperature was gradually increased to 260℃ and reacted for another 3 hours. The mixture was cooled to 130℃, and deionized water was slowly added. After filtration and washing once, the first and second filtrates were combined. The combined filtrate was sent to a distillation column to separate water and NMP, and the byproduct sodium chloride was collected. The mixture was then washed 6 times with deionized water at 60℃.

[0162] (3) Add the above undried resin to 10L of dilute sulfuric acid solution (containing about 0.38kg of sulfuric acid) and stir for 2 hours. Then filter, wash 6 times with deionized water at room temperature, and dry under vacuum at 100℃ for 12 hours to obtain protonated sulfonated polyarylene sulfide.

[0163] (4)-(5) Same as Example 1.

[0164] Performance parameter testing:

[0165] (i) Melt index (g / 10min): 155

[0166] (ii) DS (%): 17%

[0167] (iii) Hydrophilic angle (°): 49

[0168] (iv) Melting point (DSC test, heating rate 2℃ / min): 289

[0169] (v) Tensile strength (MPa): 72; Flexural strength (MPa): 101; Modulus (GPa): 3.9

[0170] Example 9 (same as Example 8, except 2,5-dichlorobenzenesulfonic acid is doubled)

[0171] (1) Add 2.28 kg of 2,5-dichlorobenzenesulfonic acid and 400 g of sodium hydroxide to 10 L of water and stir for 20 minutes.

[0172] (2) Preparation of polyarylene sulfides containing sulfonic acid groups: 50L NMP and 17.33kg sodium sulfide (45%) were added to a 100L reactor, along with the above-mentioned sodium 2,5-dichlorobenzenesulfonate solution. The mixture was then heated to 200℃ under nitrogen protection with stirring. The fractionated water was cooled and recovered using a cooling tower. 13.23kg of p-dichlorobenzene was added. The temperature was gradually increased to 225℃ and reacted at this temperature for 3 hours. Then, the temperature was gradually increased to 260℃ and reacted for another 3 hours. The mixture was cooled to 130℃, and deionized water was slowly added. After filtration and washing once, the first and second filtrates were combined. The combined filtrate was sent to a distillation column to separate water and NMP, and the byproduct sodium chloride was collected. The mixture was then washed 6 times with deionized water at 60℃.

[0173] (3) Add the above undried resin to 20L of dilute sulfuric acid solution (containing 0.75kg of sulfuric acid) and stir for 2 hours. Then filter, wash 6 times with deionized water at room temperature, and dry under vacuum at 100℃ for 12 hours to obtain protonated sulfonated polyarylene sulfide.

[0174] (4)-(5) Same as Example 8.

[0175] Performance parameter testing:

[0176] (i) Melt index (g / 10min): 192

[0177] (ii) DS (%): 35%

[0178] (iii) Hydrophilic angle (°): 38

[0179] (iv) Melting point (DSC test, heating rate 2℃ / min): 286

[0180] (v) Tensile strength (MPa): 69; Flexural strength (MPa): 96; Modulus (GPa): 3.7 Example 10 (Same as Example 9, but barium hydroxide is used to passivate benzenesulfonic acid and remove the protonation process to form an ionic sulfonated polyarylene sulfide)

[0181] (1) Add 2.28 kg of 2,5-dichlorobenzenesulfonic acid and 1.71 kg of barium hydroxide to 10 L of water and stir for 20 minutes for later use (emulsion).

[0182] (2) Preparation of polyarylene sulfides containing sulfonic acid groups: 50L of NMP and 17.33kg of sodium sulfide (45%) were added to a 100L reactor, along with the above-mentioned barium 2,5-dichlorobenzenesulfonate emulsion. The mixture was then heated to 200℃ under nitrogen protection with stirring, and the fractionated water was cooled and recovered via a cooling tower. 13.23kg of p-dichlorobenzene was added. The temperature was gradually increased to 225℃ and reacted at this temperature for 3 hours, then gradually increased to 260℃ and reacted for another 3 hours. The mixture was cooled to 130℃, and deionized water was slowly added. After filtration and washing once, the first and second filtrates were combined. The combined filtrate was sent to a distillation column to separate water and NMP, and the byproduct sodium chloride was collected. The mixture was then washed 6 times with deionized water at 60℃. Finally, it was vacuum dried at 100℃ for 12 hours to obtain ionized sulfonated polyarylene sulfides.

[0183] (4)-(5) Same as Example 9.

[0184] Performance parameter testing:

[0185] (i) Melt index (g / 10min): 163

[0186] (ii) DS (%): 35% (protonated during measurement)

[0187] (iii) Hydrophilic angle (°): 39

[0188] (iv) Melting point (DSC test, heating rate 2℃ / min): 287

[0189] (v) Tensile strength (MPa): 71; Flexural strength (MPa): 99; Modulus (GPa): 3.9

[0190] Comparative Example 1 (General Purpose Polyphenylene Sulfide) )

[0191] 50 L of NMP was added to a 100 L reactor. Under nitrogen protection, 17.3 kg of sodium sulfide (45%) and 0.2 kg of NaOH were added. The mixture was heated to 200 °C under nitrogen protection, and 6.0 L of water was fractionated. 14.7 kg of p-dichlorobenzene was added. The temperature was gradually increased to 250 °C, and the reaction was carried out at this temperature for 3 hours, completing the first stage of the reaction. The temperature was then increased to 260 °C and reacted for another 3 hours. After cooling to 150 °C, deionized water was slowly added. The mixture was filtered, washed once, and the first and second filtrates were combined. The combined filtrate was sent to a distillation column to separate water and NMP, and the byproduct sodium chloride was collected. The resin was washed 6 times with deionized water at 60 °C. Then, it was vacuum dried at 120 °C for 24 hours, yielding 10.1 kg of white granular polyphenylene sulfide product.

[0192] Test results: High resin melt index, difficult to cast film.

[0193] (i) Melt index (g / 10min): 580

[0194] (ii) Hydrophilic angle (°): 110

[0195] (iii) Tensile strength (MPa): 68; Flexural strength (MPa): 98; Modulus (GPa): 3.9

[0196] (iv) Melting point (DSC test, heating rate 2℃ / min): 285

[0197] (v) Sulfonation degree, undetectable, cannot perform proton exchange and ion exchange.

[0198] Comparative Example 2 (The polyphenylene sulfide prepared in Comparative Example 1 was treated with 20% sulfuric acid).

[0199] Weigh 1 kg of the polyphenylene sulfide prepared in Comparative Example 1 and add it to 20 L of 20% sulfuric acid aqueous solution. Stir and heat to 60°C, maintaining the temperature for 6 hours. Then filter, wash 6 times with deionized water, and vacuum dry at 100°C for 10 hours. Granulate, sample, and test performance.

[0200] Performance test results: High resin melt index, difficult to cast film.

[0201] (i) Melt index (g / 10min): 630

[0202] (ii) Hydrophilic angle (°): 108

[0203] (iii) Tensile strength (MPa): 67; Flexural strength (MPa): 95; Modulus (GPa): 3.9

[0204] (iv) Melting point (DSC test, heating rate 2℃ / min): 285

[0205] (v) Sulfonation degree, cannot be measured, and proton exchange and ion exchange cannot be performed.

[0206] Comparative Example 3 (same as Comparative Example 2, the polyphenylene sulfide prepared in Comparative Example 1 was treated with 40% sulfuric acid)

[0207] Weigh 1 kg of the polyphenylene sulfide prepared in Comparative Example 1 and add it to 20 L of 40% sulfuric acid aqueous solution. Stir and heat to 60°C, maintaining the temperature for 6 hours. Then filter, wash 6 times with deionized water, and vacuum dry at 100°C for 10 hours. Granulate, sample, and test performance.

[0208] Test results: High resin melt index, difficult to cast film.

[0209] (i) Melt index (g / 10min): 710

[0210] (ii) Hydrophilic angle (°): 106

[0211] (iii) Tensile strength (MPa): 65; Flexural strength (MPa): 89; Modulus (GPa): 3.7

[0212] (iv) Melting point (DSC test, heating rate 2℃ / min): 285

[0213] (v) Sulfonation degree, cannot be measured, and proton exchange and ion exchange cannot be performed.

[0214] Comparative Example 4 (same as Comparative Example 2, the polyphenylene sulfide prepared in Comparative Example 1 was treated with 60% sulfuric acid)

[0215] Weigh 1 kg of the polyphenylene sulfide prepared in Comparative Example 1 and add it to 20 L of 60% sulfuric acid aqueous solution. Stir and heat to 60°C, maintaining the temperature for 6 hours. Then filter, wash 6 times with deionized water, and vacuum dry at 100°C for 10 hours. Granulate, sample, and test performance.

[0216] Test results: High resin melt index, difficult to cast film.

[0217] (i) Melt index (g / 10min): 805

[0218] (ii) Hydrophilic angle (°): 103

[0219] (iii) Tensile strength (MPa): 63; Flexural strength (MPa): 85; Modulus (GPa): 3.6

[0220] (iv) Melting point (DSC test, heating rate 2℃ / min): 283

[0221] (v) Sulfonation degree, cannot be measured, and proton exchange and ion exchange cannot be performed.

[0222] Comparative Example 5 (same as Comparative Example 2, the polyphenylene sulfide prepared in Comparative Example 1 was treated with fuming sulfuric acid containing 20% ​​sulfur trioxide).

[0223] Weigh 100g of each of the two polyphenylene sulfide groups prepared in Comparative Example 1, and add them separately to 1L of fuming sulfuric acid containing 20% ​​sulfur trioxide. Incubate in a 100°C water bath; the initial color is blue. After 20 minutes, remove one sample. Incubate the other sample in a water bath for 1 hour; the color turns orange. After cooling, pour 10L of cold water along the wall and stir. The polyphenylene sulfide ...

[0224] The following tests were performed only on samples sulfonated for 20 minutes.

[0225] (i) Melt index (g / 10min): 1120

[0226] (ii) Hydrophilic angle (°): 21

[0227] (iii) Melting point (DSC test, heating rate 2℃ / min): 269

[0228] (iv) Tensile strength (MPa): 43; Flexural strength (MPa): 55; Modulus (GPa): 2.7

[0229] The comparative examples show a significant difference in performance compared to the sulfonated polyarylene sulfides synthesized in this invention.

[0230] This invention controls the content and uniform distribution of sulfonation units in the polymer structure, preserving the original high temperature resistance and high strength properties of polyphenylene sulfide, while also taking into account proton exchange, ion exchange functions, strength and hydrophilicity.

Claims

1. Polyarylene sulfide, Features: It is prepared by using sulfur-containing substances, passivated sulfonic acid monomers and dihalogenated aromatic compounds as raw materials; wherein the sulfur-containing substance is sodium sulfide or sodium hydrosulfide, and the sulfonic acid monomer is selected from at least one of 4,4-dihalodiphenyl sulfone-3,3-disulfonic acid, 2,5-dichlorobenzenesulfonic acid, 3,5-dichlorobenzenesulfonic acid, 2,4-dichlorobenzenesulfonic acid, 4-amino-2,5-dichlorobenzenesulfonic acid, 2,5-dichlorophenylhydrazine-4-sulfonic acid or 2,5-dihalo-4-formylbenzenesulfonic acid; the passivation refers to converting the protons in the sulfonic acid monomer into metal ions; the ratio of the molar number of the sulfur-containing substance to the total molar number of the sulfonic acid monomer and the dihalogenated aromatic compound is 0.95-1.05﹕1.0, and the molar ratio of the sulfonic acid monomer to the dihalogenated aromatic compound is 50.0-5.0﹕60.0-95.

0.

2. The polyarylene sulfide according to claim 1, Features: The metal ion is selected from Li + , K + 、Na + , Ba 2+ , Sr 2+ ; Further, the passivation is to mix the sulfonic acid monomer and the hydroxide of the metal ion in water or an organic solvent for reaction.

3. The polyarylene sulfide according to claim 1 or 2, Features: The dihalogenated aromatic compound is selected from 1,4-dihalobenzene, 2,4-dihalobenzene, 3,5-dihalobenzene, 4,4'-dihalobiphenyl, 4,4'-dihalodiphenyl sulfone, 4,4'-dihalobenzophenone or 4,4'-dihalodiphenyl ether; preferably, the dihalogenated aromatic compound is selected from 1,4-dichlorobenzene, 2,4-m-dichlorobenzene, 4,4'-dichlorodiphenyl sulfone or 4,4'-dichlorobenzophenone.

4. The polyarylene sulfide according to any one of claims 1 to 3, Features: Selected from the following structures represented by formula I, II, III, IV, 1, 2, 3, 4, 5 or 6: Wherein, in the above formulas, each Z is independently selected from -NH 2 、-NHHN 2 , -OH or -COOH, each M is independently selected from Li + , K + 、Na + , Ba 2+ or Sr 2+ , each m is independently ≥ 2.

5. The method for preparing the polyarylene sulfide according to any one of claims 1 to 4, Features: The following steps are involved: The dehydrated sodium sulfide or sodium hydrosulfide, the passivated sulfonic acid monomer and the dihalogenated aromatic compound are reacted in a solvent.

6. The preparation method according to claim 5, Features: The solvent is a polar aprotic solvent; further, the solvent is selected from N-methyl-2-pyrrolidone, hexamethylphosphoramide, N,N-dimethylacetamide, N,N-dimethylamide, N-ethylcaprolactam, N,N-vinylpyrrolidone, caprolactam, tetramethylurea, dimethyl sulfoxide or cyclopentane sulfone.

7. The preparation method according to claim 5 or 6, Features: The reaction is to heat the system to 200-250° C. and react for 2-5 hours, and then heat the system to 250-300° C. and react for 2-5 hours.

8. The preparation method according to any one of claims 5 to 7, Features: The following steps are involved: The sulfur-containing substance is heated while being stirred under nitrogen protection. When the temperature rises to 190-200° C., dehydration is stopped and the temperature is lowered to below 130° C. Then, the passivated sulfonic acid monomer and dihalogenated aromatic compound are added, the air in the kettle is replaced with nitrogen, and then the temperature is raised to 200-250° C. for reaction for 2-5 hours, and then the temperature is raised to 250-300° C. for reaction for 2-5 hours to terminate the polymerization reaction; then the temperature is lowered to below 130° C., deionized water is added, stirring is performed, the discharge valve of the reactor is opened, and the product is filtered and separated.