Room-temperature self-repairing polydimethylsiloxane elastomer material and preparation method thereof
By introducing polymaleic anhydride copolymer and aromatic diaminodisulfide into polydimethylsiloxane, a non-toxic and harmless room temperature self-healing polydimethylsiloxane elastomer is solved in the prior art The problem of self-healing at room temperature and the problem of toxic crosslinking agents has achieved efficient self-healing and environmentally friendly performance.
Patent Information
- Application Number
- CN202310645693.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-06-01
AI Technical Summary
The existing polydimethylsiloxane (PDMS) elastomer materials are difficult to achieve self-healing at room temperature, and commonly used crosslinking agents are toxic, affecting environmental protection performance.
Using materials composed of polydimethylsiloxane, polymaleic anhydride copolymer and aromatic diaminodisulfide, a self-healing polydimethylsiloxane elastomer is formed through room temperature reaction, and non-toxic and harmless Crosslinking agent to achieve room temperature self-healing performance.
The material can achieve a self-repair rate of more than 70% at room temperature, up to 97.5%, and maintains good elasticity and processing performance, avoiding the environmental pressure of toxic crosslinking agents.
Smart Images

Figure CN119060340A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of material technology, and specifically relates to a room temperature self-healing polydimethylsiloxane elastomer material and a preparation method thereof. Background Art
[0002] Polydimethylsiloxane (PDMS) has good thermal stability, biocompatibility and UV resistance, but its mechanical strength is very poor and it cannot be used alone. It is often used to form an elastomer through processes such as chain extension and cross-linking. In polydimethylsiloxane elastomer materials, by introducing reversible covalent bonds or dynamic non-covalent bond interactions to form a reversible cross-linking structure, a responsive self-healing elastomer material can be obtained. Elastomer materials with self-healing properties can be repaired under certain conditions when cracks, scratches, and breaks occur, so as to achieve the effect of reuse. They can also be recycled and reprocessed after use and reused, thus forming a cycle to achieve the purpose of reducing waste materials, protecting the environment and reducing carbon emissions.
[0003] The key point of self-healing materials lies in the conditions for self-healing. Generally speaking, self-healing requires that the molecular chain structure of the material obtains sufficient activity and energy to achieve a rapid balance of "fracture-crosslinking". Repair at high temperature may be difficult to achieve, so room temperature repair has very important application value. Disulfide compounds containing aromatic structures can make the material repairable at room temperature. Therefore, by adding aromatic disulfides containing amino groups to polydimethylsiloxane elastomers, polydimethylsiloxane elastomers with room temperature self-healing properties can be formed.
[0004] Common cross-linking agents such as diisocyanates or polyisocyanates are toxic to a certain extent, and raw materials such as phosgene are often required during the synthesis process, which will bring additional environmental pressure to PDMS elastomers. Summary of the invention
[0005] In view of the above problems existing in the prior art, the purpose of the present invention is to provide a room temperature self-healing polydimethylsiloxane (PDMS) elastomer material and a preparation method thereof, which can achieve self-healing at room temperature and has good elastic properties and processing properties, and the material is prepared using a non-toxic, harmless, convenient and easily available cross-linking agent.
[0006] The first aspect of the present invention provides a room temperature self-healing polydimethylsiloxane elastomer material, which is composed of a segment R1 containing a polydimethylsiloxane structure, a polymaleic anhydride copolymer structure R2, and a structure R3 having an aromatic diaminodisulfide;
[0007] In the material, the weight fraction of R1 is 40-75%, the weight fraction of R2 is 20-55%, and the weight fraction of R3 is 3-15%.
[0008] The second aspect of the present invention provides a method for preparing the above-mentioned room temperature self-healing polydimethylsiloxane elastomer material, the preparation method comprising:
[0009] 1) subjecting maleic anhydride to living free radical polymerization with one or more other monomers containing double bonds to obtain a polymaleic anhydride copolymer, and preparing the copolymer into a solution;
[0010] 2) preparing solutions of diamine-containing polydimethylsiloxane and disulfide-containing aromatic diamine compound respectively;
[0011] 3) The three solutions obtained in step 1) and step 2) are mixed, reacted at room temperature, and the solvent is removed to obtain a room temperature self-healing polydimethylsiloxane elastomer material.
[0012] The material of the present invention has a polydimethylsiloxane structure and an aromatic disulfide structure, a breaking strength of 0.5-5MPa, an elongation at break of 100-800%, can be repaired at room temperature after breaking, and the repair rate can reach more than 70% after 24 hours (repair rate = breaking strength after repair / breaking strength before repair × 100%), and can reach up to 97.5%.
[0013] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 Schematic diagram of the structure of a room temperature self-healing polydimethylsiloxane elastomer material according to an embodiment.
[0015] Figure 2 Schematic diagram of the structure of another room temperature self-healing polydimethylsiloxane elastomer material according to an embodiment. DETAILED DESCRIPTION
[0016] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0017] According to a first aspect of the present invention, the present invention provides a room temperature self-healing polydimethylsiloxane elastomer material, the material is composed of a segment R1 containing a polydimethylsiloxane structure, a polymaleic anhydride copolymer structure R2 and a structure R3 having an aromatic diaminodisulfide;
[0018] In the material, the weight fraction of R1 is 40-75%, the weight fraction of R2 is 20-55%, and the weight fraction of R3 is 3-15%.
[0019] In the present invention, R1 is formed by a linear polydimethylsiloxane containing a diamino group; R2 is formed by a linear copolymer containing maleic anhydride, such as polymethacrylate-maleic anhydride copolymer and polystyrene-maleic anhydride copolymer; R3 is formed by an aromatic diamine compound containing disulfide, such as 4,4'-diaminodiphenyl disulfide and 2,2'-diaminodiphenyl disulfide.
[0020] Preferably, in the material, the weight fraction of R1 is 45-70%, the weight fraction of R2 is 20-50%, and the weight fraction of R3 is 3-10%.
[0021] According to a second aspect of the present invention, the present invention provides a method for preparing the above-mentioned room temperature self-healing polydimethylsiloxane elastomer material, the preparation method comprising:
[0022] 1) subjecting maleic anhydride to living free radical polymerization with one or more other monomers containing double bonds to obtain a polymaleic anhydride copolymer, and preparing the copolymer into a solution;
[0023] 2) preparing solutions of diamine-containing polydimethylsiloxane and disulfide-containing aromatic diamine compound respectively;
[0024] 3) The three solutions obtained in step 1) and step 2) are mixed, reacted at room temperature, and the solvent is removed to obtain a room temperature self-healing polydimethylsiloxane elastomer material.
[0025] In the present invention, the monomer containing a double bond can be selected from methyl / acrylic acid ester monomers and / or styrene monomers; the amount of maleic anhydride to the monomer containing a double bond can be 1:0.8-10, preferably 1:1-6.
[0026] According to the present invention, the living radical polymerization adopts a solution polymerization reaction, the polymerization temperature is 40-120° C., preferably 50-120° C., the polymerization time is 1-24 hours, preferably 2-16 hours, and the polymerization is carried out under an inert atmosphere.
[0027] Take reversible addition-fragmentation chain transfer polymerization (RAFT polymerization) as an example. Put the monomer, initiator, chain transfer agent, solvent and other compounds into the reaction vessel, replace the vacuum-inert atmosphere three times, and then raise the reaction system to the polymerization temperature to react. After the reaction is completed, the reaction solution is precipitated in methanol and dried.
[0028] In the present invention, the number average molecular weight of the polymaleic anhydride copolymer is 1000-20000, preferably 1500-15000.
[0029] According to the present invention, the number average molecular weight of the diamine-containing polydimethylsiloxane is 1000-10000. The diamine-containing polydimethylsiloxane can be purchased.
[0030] In the present invention, the disulfide-containing aromatic diamine compound may be 4,4'-diaminodiphenyl disulfide and / or 2,2'-diaminodiphenyl disulfide.
[0031] According to the present invention, the concentration of the solution obtained in step 1) and step 2) can be 10-30 wt %. The solvent for preparing the solution is a good solvent, which can be selected from at least one of dichloromethane, chloroform, tetrahydrofuran and dioxane.
[0032] In step 3) of the present invention, the amount of each material used is 0.20-0.60 mol, preferably 0.25-0.55 mol, per mol of maleic anhydride groups in the polymaleic anhydride copolymer; the amount of terminal amino groups in the diamino-containing polydimethylsiloxane is 0.40-0.90 mol, preferably 0.45-0.80 mol; the amount of diamine in the disulfide-containing aromatic diamine compound is 0.40-0.90 mol, preferably 0.45-0.80 mol.
[0033] According to the present invention, the ring-opening reaction in step 3) is a room temperature reaction, and the reaction time is 0.1-12h, preferably 0.2-8h.
[0034] The substances and parameters not limited in the present invention can be selected according to the existing technology and belong to the conventional technical means in this field.
[0035] The present invention will be further described below with reference to the following examples, but is not limited to these examples.
[0036] In the following examples and comparative examples, the relevant data were obtained as follows:
[0037] 1. Test the toughness of polydimethylsiloxane elastomer according to GB / T 1040.2-2006 method.
[0038] 2. The structure of the material was characterized by hydrogen nuclear magnetic resonance spectroscopy. The segment length was obtained by integrating the nuclear magnetic resonance spectrum. The testing instrument was a Bruker 300MHz nuclear magnetic resonance spectrometer and the solvent was CDCl3.
[0039] 3. Repair method: Prepare the material into dumbbell-shaped splines, cut the splines and quickly place them in their original shape between two smooth glass plates. Measure the mechanical properties after 24 hours.
[0040] Example 1
[0041] 7.84g (0.08mol) of maleic anhydride and 32.0g (0.32mol) of methyl methacrylate were placed in a three-necked flask, 7.28g (0.02mol) of 2-(dodecyl trithiocarbonyl)-2-methyl-propionic acid, 2.42g of azobisisobutyronitrile, and 80mL of anhydrous dioxane were added. After the system was stirred to homogeneity, N2 was purged for 20min, and the system was sealed and placed in an oil bath set at 80°C for reaction. After 6h of reaction, the reaction solution was poured into methanol, filtered and dried to obtain the product PMA1, with a number average molecular weight Mn of 2000 and a molecular weight distribution of 1.35, which was prepared into a 20wt% dichloromethane solution of PMA1.
[0042] Dissolve 20g of double-terminated amino-polydimethylsiloxane PDMS (Mn is 5000) in 75mL of dichloromethane (containing 0.008mol of amino groups), stir evenly, quickly add 50mL of 20wt% dichloromethane solution of PMA1 (containing 0.020mol of maleic anhydride groups) and 7.5mL of 20wt% dichloromethane solution of 4,4'-diaminodiphenyl disulfide (containing 0.012mol of amino groups), stir evenly and react at room temperature. The reaction ends after about 1h, and after removing the solvent, the room temperature self-healing elastomer material PDMS-E1 is obtained. The structure of the material is as follows: Figure 1 As shown, n in R1 is 66, x in R2 is 0.2, and y is 0.8. In the material, the weight fraction of R1 is 63.5%, the weight fraction of R2 is 31.7%, and the weight fraction of R3 is 4.8%.
[0043] Example 2
[0044] 7.84g (0.08mol) of maleic anhydride and 32g (0.32mol) of styrene were placed in a three-necked flask, 7.30g (0.02mol) of 2-(dodecyl trithiocarbonyl)-2-methyl-propionic acid, 2.41g of azobisisobutyronitrile, and 100mL of anhydrous dioxane were added. After the system was stirred to homogeneity, N2 was purged for 20min, and the system was sealed and placed in an oil bath set at 80°C for reaction. After 6h of reaction, the reaction solution was poured into methanol, filtered and dried to obtain the product PMA4, with a number average molecular weight Mn of 1800 and a molecular weight distribution of 1.29, which was prepared into a 20wt% dichloromethane solution of PMA4.
[0045] Dissolve 20g of double-terminated amino-polydimethylsiloxane PDMS (Mn is 5000) in 75mL of dichloromethane (containing 0.008mol of amino group), stir evenly, quickly add 50mL of 20wt% dichloromethane solution of PMA4 (containing 0.020mol of maleic anhydride group) and 7.5mL of 20wt% dichloromethane solution of 4,4'-diaminodiphenyl disulfide (containing 0.012mol of amino group), stir evenly and react at room temperature. The reaction ends after about 1h, and after removing the solvent, the room temperature self-healing elastomer material PDMS-E2 is obtained. The structure of the material is as follows Figure 2 As shown, n in R1 is 66, x in R2 is 0.2, and y is 0.8. In the material, the weight fraction of R1 is 63.5%, the weight fraction of R2 is 31.7%, and the weight fraction of R3 is 4.8%.
[0046] Example 3
[0047] 12.74g (0.13mol) of maleic anhydride and 27.0g (0.27mol) of methyl methacrylate were placed in a three-necked flask, 7.28g (0.02mol) of 2-(dodecyl trithiocarbonyl)-2-methyl-propionic acid, 2.42g of azobisisobutyronitrile, and 80mL of anhydrous dioxane were added. After the system was stirred to homogeneity, N2 was purged for 20min, and the system was sealed and placed in an oil bath set at 80°C for reaction. After 6h of reaction, the reaction solution was poured into methanol, filtered and dried to obtain the product PMA2, with a number average molecular weight Mn of 1900 and a molecular weight distribution of 1.49, which was prepared into a 20wt% dichloromethane solution of PMA2.
[0048] Dissolve 25.5g of double-terminated amino-polydimethylsiloxane PDMS (Mn is 5000) in 75mL of dichloromethane (containing 0.011mol of amino groups), stir evenly, quickly add 50mL of 20wt% dichloromethane solution of PMA2 (containing 0.033mol of maleic anhydride groups) and 13.7mL of 20wt% dichloromethane solution of 4,4'-diaminodiphenyl disulfide (containing 0.022mol of amino groups), stir evenly and react at room temperature. The reaction ends after about 1h, and after removing the solvent, the room temperature self-healing elastomer material PDMS-E3 is obtained. The structure of the material is as follows Figure 1 As shown, n in R1 is 66, x in R2 is 0.33, and y is 0.67. In the material, the weight fraction of R1 is 66.7%, the weight fraction of R2 is 26.1%, and the weight fraction of R3 is 7.2%.
[0049] Example 4
[0050] 7.84g (0.08mol) of maleic anhydride and 32.0g (0.32mol) of methyl methacrylate were placed in a three-necked flask, 1.46g (0.004mol) of 2-(dodecyl trithiocarbonyl)-2-methyl-propionic acid, 0.51g of azobisisobutyronitrile, and 100mL of anhydrous dioxane were added, the system was stirred until homogeneous, N2 was purged for 20min, and the system was sealed and placed in an oil bath set at 80°C for reaction. After 6h of reaction, the reaction solution was poured into methanol, filtered and dried to obtain the product PMA3, with a number average molecular weight Mn of 11800 and a molecular weight distribution of 1.24, which was prepared into a 20wt% dichloromethane solution of PMA3.
[0051] Dissolve 25.5g of double-terminated amino-polydimethylsiloxane PDMS (Mn is 5000) in 75mL of dichloromethane (containing 0.011mol of amino groups), stir evenly, quickly add 50mL of 20wt% dichloromethane solution of PMA3 (containing 0.033mol of maleic anhydride groups) and 13.7mL of 20wt% dichloromethane solution of 4,4'-diaminodiphenyl disulfide (containing 0.022mol of amino groups), stir evenly and react at room temperature. The reaction ends after about 1h, and after removing the solvent, the room temperature self-healing elastomer material PDMS-E4 is obtained. The structure of the material is as follows Figure 1 As shown, n in R1 is 66, x in R2 is 0.2, and y is 0.8. In the material, the weight fraction of R1 is 66.7%, the weight fraction of R2 is 26.1%, and the weight fraction of R3 is 7.2%.
[0052] Example 5
[0053] A 20 wt % dichloromethane solution of PMA1 was prepared in the same manner as in Example 1.
[0054] Dissolve 12g of double-terminated amino-polydimethylsiloxane PDMS (Mn is 3000) in 75mL of dichloromethane (containing 0.008mol of amino group), stir evenly, quickly add 50mL of 20wt% dichloromethane solution of PMA1 (containing 0.020mol of maleic anhydride group) and 7.5mL of 20wt% dichloromethane solution of 4,4'-diaminodiphenyl disulfide (containing 0.012mol of amino group), stir evenly and react at room temperature. The reaction ends after about 1h, and after removing the solvent, the room temperature self-healing elastomer material PDMS-E5 is obtained. The structure of the material is as follows Figure 1 As shown, n in R1 is 40, x in R2 is 0.2, and y is 0.8. In the material, the weight fraction of R1 is 51.1%, the weight fraction of R2 is 42.6%, and the weight fraction of R3 is 6.3%.
[0055] Example 6
[0056] A 20 wt% dichloromethane solution of PMA4 was prepared using the same method as in Example 2.
[0057] Dissolve 12g of double-terminated amino-polydimethylsiloxane PDMS (Mn is 3000) in 75mL of dichloromethane (containing 0.008mol of amino group), stir evenly, quickly add 50mL of 20wt% PMA4 solution (containing 0.020mol of maleic anhydride group) and 7.5mL of 20wt% 4,4'-diaminodiphenyl disulfide dichloromethane solution (containing 0.012mol of amino group), stir evenly and react at room temperature. The reaction ends after about 1h, and after removing the solvent, the room temperature self-healing elastomer material PDMS-E6 is obtained. The structure of the material is as follows Figure 2 As shown, n in R1 is 40, x in R2 is 0.2, and y is 0.8. In the material, the weight fraction of R1 is 51.1%, the weight fraction of R2 is 42.6%, and the weight fraction of R3 is 6.3%.
[0058] Example 7
[0059] A 20 wt % dichloromethane solution of PMA1 was prepared in the same manner as in Example 1.
[0060] Dissolve 10g of double-terminated amino-polydimethylsiloxane PDMS (Mn is 2000) in 50mL of dichloromethane (containing 0.01mol of amino group), stir evenly, quickly add 50mL of 20wt% dichloromethane solution of PMA1 (containing 0.020mol of maleic anhydride group) and 6.2mL of 20wt% dichloromethane solution of 4,4'-diaminodiphenyl disulfide (containing 0.010mol of amino group), stir evenly and react at room temperature. The reaction ends after about 1h, and after removing the solvent, the room temperature self-healing elastomer material PDMS-E7 is obtained. The structure of the material is as follows: Figure 1 As shown, n in R1 is 25, x in R2 is 0.2, and y is 0.8. In the material, the weight fraction of R1 is 47.1%, the weight fraction of R2 is 47.1%, and the weight fraction of R3 is 5.8%.
[0061] Example 8
[0062] A 20 wt% dichloromethane solution of PMA4 was prepared using the same method as in Example 2.
[0063] Dissolve 10g of double-terminated amino-polydimethylsiloxane PDMS (Mn is 2000) in 50mL of dichloromethane (containing 0.01mol of amino group), stir evenly, quickly add 50mL of 20wt% dichloromethane solution of PMA4 (containing 0.020mol of maleic anhydride group) and 6.2mL of 20wt% dichloromethane solution of 4,4'-diaminodiphenyl disulfide (containing 0.01mol of amino group), stir evenly and react at room temperature. The reaction ends after about 1h, and after removing the solvent, the room temperature self-healing elastomer material PDMS-E8 is obtained. The structure of the material is as follows Figure 2 As shown, n in R1 is 25, x in R2 is 0.2, and y is 0.8. In the material, the weight fraction of R1 is 47.1%, the weight fraction of R2 is 47.1%, and the weight fraction of R3 is 5.8%.
[0064] Comparative Example 1
[0065] A 20 wt % dichloromethane solution of PMA1 was prepared in the same manner as in Example 1.
[0066] Dissolve 50g of double-terminated amino-polydimethylsiloxane PDMS (Mn is 5000) in 100mL of dichloromethane (containing 0.020mol of amino group), stir evenly, quickly add 50mL of 20wt% dichloromethane solution of PMA1 (containing 0.020mol of maleic anhydride group), stir evenly, and react at room temperature. The reaction ends after about 1h, and the elastomeric material is obtained after removing the solvent.
[0067] Comparative Example 2
[0068] A 20 wt % dichloromethane solution of PMA1 was prepared in the same manner as in Example 1.
[0069] Dissolve 3g of double-terminated amino-polydimethylsiloxane PDMS (Mn is 600) in 20mL of dichloromethane (containing 0.01mol of amino group), stir evenly, quickly add 50mL of 20wt% dichloromethane solution of PMA1 (containing 0.02mol of maleic anhydride group) and 6.2mL of 20wt% dichloromethane solution of 4,4'-diaminodiphenyl disulfide (containing 0.01mol of amino group), stir evenly and react at room temperature. The reaction ends after about 1h, and the elastomeric material is obtained after removing the solvent.
[0070] Comparative Example 3
[0071] 19.3g (0.2mol) of maleic anhydride and 20.2g (0.2mol) of methyl methacrylate were placed in a three-necked flask, 0.73g (0.002mol) of 2-(dodecyl trithiocarbonyl)-2-methyl-propionic acid, 0.25g of azobisisobutyronitrile, and 80mL of anhydrous dioxane were added. After the system was stirred to a homogeneous phase, N2 was purged for 20min, and the system was sealed and placed in an oil bath set at 80°C for reaction. After 8h of reaction, the reaction solution was poured into methanol, filtered and dried to obtain the product PMA5, with a number average molecular weight Mn of 21000 and a molecular weight distribution of 1.23, which was prepared into a 20wt% dichloromethane solution of PMA5.
[0072] Dissolve 50g of double-terminated amino-polydimethylsiloxane PDMS (Mn is 5000) in 75mL of dichloromethane (containing 0.02mol of amino group), stir evenly, quickly add 50mL of 20wt% dichloromethane solution of PMA5 (containing 0.05mol of maleic anhydride group) and 18.6mL of 20wt% dichloromethane solution of 4,4'-diaminodiphenyl disulfide (containing 0.03mol of amino group), stir evenly and react at room temperature. The reaction ends after about 1h, and the elastomeric material is obtained after removing the solvent.
[0073] The parameters of the raw materials and other parameters of the materials synthesized in the embodiments and comparative examples are shown in Table 1, and the properties of the materials are shown in Table 2.
[0074] Table 1
[0075]
[0076]
[0077] Table 2
[0078]
[0079] It can be seen from Table 2 that the room temperature self-healing material of the present invention has a fracture strength of 0.5-5 MPa, an elongation at break of 100-800%, can be repaired at room temperature after fracture, and the repair rate can reach more than 70% after 24 hours.
[0080] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A room temperature self-healing polydimethylsiloxane elastomer material, It is characterized in that The material is composed of a segment R1 containing a polydimethylsiloxane structure, a polymaleic anhydride copolymer structure R2, and a structure R3 having an aromatic diaminodisulfide; In the material, the weight fraction of R1 is 40-75%, preferably 45-70%, the weight fraction of R2 is 20-55%, preferably 20-50%, and the weight fraction of R3 is 3-15%, preferably 3-10%.
2. The preparation method of the room temperature self-healing polydimethylsiloxane elastomer material according to claim 1, It is characterized in that The preparation method comprises: 1) subjecting maleic anhydride to living free radical polymerization with one or more other monomers containing double bonds to obtain a polymaleic anhydride copolymer, and preparing the copolymer into a solution; 2) preparing solutions of diamine-containing polydimethylsiloxane and disulfide-containing aromatic diamine compound respectively; 3) The three solutions obtained in step 1) and step 2) are mixed, reacted at room temperature, and the solvent is removed to obtain a room temperature self-healing polydimethylsiloxane elastomer material.
3. The method for preparing the room temperature self-healing polydimethylsiloxane elastomer material according to claim 2, in, The monomer containing a double bond is selected from methyl / acrylic acid ester monomers and / or styrene monomers; the amount of maleic anhydride to the monomer containing a double bond is 1:0.8-10, preferably 1:1-6.
4. The method for preparing the room temperature self-healing polydimethylsiloxane elastomer material according to claim 2 or 3, in, In step 1), the polymerization temperature is 40-120° C., preferably 50-120° C.; the polymerization time is 1-24 h, preferably 2-16 h.
5. The method for preparing the room temperature self-healing polydimethylsiloxane elastomer material according to claim 2, in, The number average molecular weight of the polymaleic anhydride copolymer is 1,000-20,000, preferably 1,500-15,000.
6. The method for preparing the room temperature self-healing polydimethylsiloxane elastomer material according to claim 2, in, The number average molecular weight of the diamine-containing polydimethylsiloxane is 1000-10000.
7. The method for preparing the room temperature self-healing polydimethylsiloxane elastomer material according to claim 2, in, The disulfide-containing aromatic diamine compound is 4,4'-diaminodiphenyl disulfide and / or 2,2'-diaminodiphenyl disulfide.
8. The method for preparing the room temperature self-healing polydimethylsiloxane elastomer material according to claim 2, in, The concentration of the solution obtained in step 1) and step 2) is 10-30 wt %; the solvent for preparing the solution is selected from at least one of dichloromethane, chloroform, tetrahydrofuran and dioxane.
9. The method for preparing the room temperature self-healing polydimethylsiloxane elastomer material according to claim 2, in, In step 3), the amount of terminal amino groups in the diamino-containing polydimethylsiloxane is 0.20-0.60 mol, preferably 0.25-0.55 mol, based on each mol of maleic anhydride groups in the polymaleic anhydride copolymer; the amount of diamine in the disulfide-containing aromatic diamine compound is 0.40-0.90 mol, preferably 0.45-0.80 mol.
10. The method for preparing the room temperature self-healing polydimethylsiloxane elastomer material according to claim 2, in, The reaction time in step 3) is 0.1-12 h, preferably 0.2-8 h.
Citation Information
Patent Citations
Reversible covalent crosslinking polysiloxane elastomer, preparation method therefor and application thereof
CN105111470A
Application of polysiloxane elastomer based on aryl disulfide bond and imine bond as self-healing material
CN109384927A
Polydimethylsiloxane self-repairing material based on disulfide exchange reaction and preparation method thereof
CN110204678A
Self-repairing modified silicone rubber and preparation method thereof
CN110218330A
Heat-resistant room temperature fast self-repairing elastomer and preparation method and use thereof
CN110551269A