Conductive silver adhesive with high thermal conductivity and high reliability and preparation method thereof

Through the coordinated combination of modified sheet silver powder and nano silver powder, the conductive silver glue is solved in the low silver content, and the conductive silver glue with high conductivity and weather resistance is achieved, reducing costs and suitable for Industrialized production.

CN119060668APending Publication Date: 2024-12-03COLLTECH DONGGUAN BONDING TECH CO LTD

Patent Information

Application Number
CN202411209102.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing conductive silver glue has shortcomings in terms of high conductivity and reliability, especially in low silver content, it is difficult to achieve high conductivity and weather resistance, and the cost is high, and the preparation process is complicated and not suitable for industrial production.

Method used

The coordinated combination of modified sheet silver powder and nano silver powder was used to treat spherical silver powder by gallic acid and carboxymethyl chitosan modifier, combined with the sonication of the alkyd solution, and prepared high conductivity and high temperature and humidity resistance. The modified sheet-like silver powder is combined with a small amount of nano silver powder in the conductive glue to reduce the contact resistance of the silver powder particles and improve thermal conductivity and bonding strength.

Benefits of technology

Achieve conductive silver glue with high conductivity and weather resistance at lower silver content, reducing costs, improving the toughness and bonding strength of the conductive glue, suitable for industrial production without the need for additional dispersants and defoamers .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to a conductive silver adhesive with high thermal conductivity and high reliability and a preparation method thereof. The conductive silver adhesive comprises the following raw materials in parts by mass: 10-20 parts of epoxy resin, 5-10 parts of an epoxy diluent, 5-10 parts of an anhydride curing agent, 0.1-0.3 part of a stabilizer, 0.1-0.3 part of a silane coupling agent, 1-5 parts of an accelerant, 45-60 parts of modified flake silver powder and 5-8 parts of nano silver powder. The modified flake silver powder is obtained by performing ball milling on spherical silver powder in the presence of a modifier compounded by gallic acid and carboxymethyl chitosan and then performing ultrasonic treatment with an alcohol acid mixed solution. Through reasonable compatibility of the modified flake silver powder and the nano silver powder, mutual contact of silver powder particles is increased, surface contact resistance is reduced, the conductive silver adhesive with low silver content has low volume resistivity, and thermal conductivity and weather resistance are improved. The compounded epoxy diluent can improve the toughness and bonding strength of the conductive silver adhesive after curing at the same time, and no extra defoaming agent is added.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive adhesives, and in particular relates to a conductive silver adhesive with high thermal conductivity and high reliability and a preparation method thereof. Background Art

[0002] With the advancement of science and technology, electronic components are constantly developing in the direction of miniaturization, and the integration of devices is constantly improving, requiring the connection materials to have high line resolution. The traditional connection material Pb / Sn solder can only be used for connections with a pitch below 0.65mm, which cannot meet the process requirements; the thermal stress generated by the temperature above 230℃ in the connection process will also damage the device and the substrate. In addition, the lead in Pb / Sn solder is a toxic substance. There is an urgent need for new lead-free connection materials. Conductive adhesive has emerged as a substitute for Pb / Sn solder. Conductive adhesive is an adhesive that has both conductive properties and bonding properties. It can connect a variety of conductive materials together to form an electrical path between the connected materials. Since its advent in 1966, conductive adhesive has played an increasingly important role in electronic technology. At present, conductive adhesive has been widely used in the packaging and bonding of electronic components such as printed circuit board assemblies, light-emitting diodes, liquid crystal displays, smart cards, ceramic capacitors, and integrated circuit chips. Conductive silver glue increases conductivity by adding conductive silver powder to epoxy glue, but there are the following problems: 1. Poor reliability and relatively low bonding strength. In connections with small pitches, the bonding strength directly affects the impact resistance of the components. 2. Low conductivity. For general components, most conductive glues are acceptable, but for power devices, the conductivity still cannot meet the requirements.

[0003] The prior art increases the conductivity and heat resistance of conductive silver paste by adding graphene and carbon nanotubes, such as reported in CN118406456A and CN103614098A. However, the high cost of graphene, carbon nanotubes, etc. leads to high cost of adding conductive silver paste, which is not suitable for industrial production. Increasing the amount of silver powder added can improve the conductivity, but it will also increase the cost and deteriorate other properties. In view of the problems of low conductivity, unstable contact resistance, and poor impact strength of conductive silver paste, the prior art has reported that dendritic nano silver powder replaces ordinary nano silver powder. Dendritic silver powder has the advantages of low resistivity and large specific surface area. However, its preparation process is complicated, and the process conditions and micromorphology have a great influence on the performance of conductive paste, which is also not suitable for industrial production. Flake silver powder is suitable for use as a filler for conductive silver paste due to its high conductivity and simple preparation process. In order to achieve higher tap density and thixotropy, the flaky silver powder needs to have good dispersibility, otherwise the compatibility with the resin matrix is ​​poor and the characteristics of the flaky silver powder cannot be brought into play.

[0004] CN118272020A discloses a high thermal conductivity conductive adhesive and its preparation method, using 60-70% silver powder. In order to prevent agglomeration, a dispersant, such as polyvinyl alcohol and polyphosphate, needs to be added to the conductive silver adhesive of the patent. Although the addition of these dispersants can help the silver powder disperse, it reduces the performance of the conductive adhesive. Summary of the invention

[0005] In view of the fact that the existing conductive silver paste needs to increase the silver content to achieve higher conductivity, but this will lead to poor silver powder dispersion, low bonding strength, and poor weather resistance, the present invention proposes a high reliability and high conductivity silver paste, which uses modified flaky silver powder as the main conductive filler and is compounded with a small amount of nano silver powder, which can achieve high conductivity and weather resistance at a lower silver content. The present invention achieves the above purpose through the following technical solutions.

[0006] A conductive silver paste with high thermal conductivity and high reliability comprises the following raw materials in parts by weight: 10-20 parts of epoxy resin, 5-10 parts of epoxy diluent, 5-10 parts of anhydride curing agent, 0.1-0.3 parts of stabilizer, 0.1-0.3 parts of silane coupling agent, 1-5 parts of accelerator, 45-60 parts of modified flaky silver powder and 5-8 parts of nano silver powder; the modified flaky silver powder is obtained by ball milling spherical silver powder in the presence of a modifier compounded with gallic acid and carboxymethyl chitosan, and then ultrasonically treating an alcohol-acid mixed solution, and the amount of the modifier is 3-5wt% of the spherical silver powder.

[0007] Furthermore, in the modifier, the mass ratio of gallic acid to carboxymethyl chitosan is 4-7:1, the molecular weight of carboxymethyl chitosan is 20,000 to 30,000, and the molecular weight of carboxymethyl chitosan cannot be too large, otherwise the solubility will be poor.

[0008] The preparation method of flaky silver powder in the prior art is generally to prepare spherical silver powder by reduction method, and then to obtain spherical silver powder by ball milling or sand milling in the presence of grinding aids, separation, washing and drying. The grinding aids are long-chain alkyl acids, long-chain alkylamines, etc. The presence of grinding aids protects the silver powder on the one hand and plays a dispersing role on the other hand. However, the presence of these dispersants will adhere to the surface of the silver powder even after multiple washings. The inventors found that the presence of this part of organic matter can help to grind the flaky silver powder and help to improve the compatibility with the organic resin, but it will reduce the conductivity under hot and humid conditions and reduce the thixotropy of the conductive adhesive. CN105618734A abandoned the use of conventional long-chain alkyl acids or long-chain alkylamines and other grinding aids when preparing flaky silver powder, and used succinic acid, glutaric acid, adipic acid, heptanoic acid sulfuric acid, and triethanolamine instead of grinding aids. These small molecules containing carboxyl, amino, and sulfonic acid groups were surface modified to modify the silver powder, replacing the surface lubricating layer of the previous macromolecules, not only protecting the silver powder from oxidation, but also effectively improving the conductive properties of the silver powder, and also having good compatibility with the resin, so it has good dispersion stability and interface properties. However, the inventors found that small molecule modifiers such as dibasic acids can improve the conductive properties of flaky silver powder, but will reduce the thixotropy of the conductive adhesive. After a large number of experiments, the inventor unexpectedly found that the flaky silver powder obtained by ball milling with a modifier compounded with gallic acid and carboxymethyl chitosan has good particle size uniformity and a surface morphology that is more suitable as a conductive filler for conductive adhesives. It has extremely high conductivity and also exhibits good thixotropic properties and conductive properties and high temperature and humidity resistance.

[0009] The present invention modifies the flaky silver powder by a compounded modifier, and then uses the modified flaky silver powder obtained by alkyd solution treatment together with a small amount of nano silver powder. The two different silver powders have a synergistic compounding effect, which increases the mutual contact of the silver powder particles and reduces the surface contact resistance, thereby achieving a conductive silver paste with a lower silver content having a very low volume resistivity, and the thermal conductivity and weather resistance are also improved.

[0010] Furthermore, the modified flaky silver powder is prepared by a preparation method comprising the following steps: spherical silver powder is dispersed in an alcohol solvent, a modifier is added, ball milling is performed at 40-50° C., separation is performed after ball milling, immersion is performed in an alcohol acid solution of alcohol and concentrated nitric acid under ultrasonic conditions, treatment is performed for 10-20 minutes, washing is performed, and drying is performed to obtain the modified flaky silver powder.

[0011] Furthermore, the particle size of the spherical silver powder is 5-10 μm, the purity is ≥99%, preferably the purity is ≥99.9%; the particle size of the modified flaky silver powder obtained is 3-5 μm, and the tap density is 3.2-3.6 g / cm 3 , specific surface area 1.1-1.5m 2 / g.

[0012] Furthermore, the alcohol solvent is selected from at least one of methanol, ethanol, propanol, diethanol and propylene glycol, preferably ethanol. The inventors have found that using ethanol as a ball milling medium can improve the ball milling efficiency, the flaking speed of the silver powder is faster, and less spherical particles remain.

[0013] Furthermore, the mass ratio of the spherical silver powder, the alcohol solvent and the modifier is 1:1.2-1.6:0.03-0.05.

[0014] Furthermore, the ball milling conditions are a ball-to-material ratio of 10-20:1, a rotation speed of 400-500 rpm, and a ball milling time of 10-15 h.

[0015] Furthermore, in the preparation of the alkyd solution, the volume ratio of alcohol to concentrated nitric acid is 3-4:1, the alcohol is selected from at least one of methanol, ethanol, and isopropanol, preferably ethanol; the ultrasonic condition is 60-100kHz. There is no particular limitation on washing and drying, which are well known in the art. In a specific embodiment of the present invention, washing is washing with ethanol and deionized water, and drying is vacuum drying.

[0016] Furthermore, the epoxy resin is selected from at least one of bisphenol epoxy resin, novolac epoxy resin, bisphenol S epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin.

[0017] Furthermore, the epoxy diluent is selected from at least one of C8-C12 alkyl glycidyl ether, benzyl glycidyl ether, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, and neopentyl glycol diglycidyl ether. Preferably, C8-C12 alkyl carboxylic acid glyceryl ether and an epoxy diluent with an epoxy functionality of 2-3 are compounded in a mass ratio of 2.2-3.5:1, wherein the C8-C12 alkyl carboxylic acid glyceryl ether is selected from at least one of C8 alkyl glycidyl ether, C9 alkyl glycidyl ether, C10 alkyl glycidyl ether, C11 alkyl glycidyl ether, and C12 alkyl glycidyl ether; and the epoxy diluent with an epoxy functionality of 2-3 is selected from at least one of ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, and neopentyl glycol diglycidyl ether. The inventors have found that the above-mentioned compounded epoxy diluent can not only play a diluting role in reducing the viscosity of the conductive silver glue, but also improve the toughness and bonding strength of the conductive silver glue after curing. The long carbon chain monoepoxy diluent can improve the toughness of the glue after curing. If the amount is controlled within an appropriate range, it will not have an adverse effect on the hardness and thermal expansion coefficient of the cured product. When used in combination with a multifunctional epoxy diluent, the crosslinking density will not be reduced, the bonding strength is guaranteed, and bubbles generated during the curing process can be prevented, so there is no need to add an additional defoaming agent.

[0018] Furthermore, the silane coupling agent is selected from at least one of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and γ-(2,3-epoxypropyloxy)propyltrimethoxysilane.

[0019] The stabilizer is selected from at least one of glutaric acid, adipic acid, benzoic acid, n-decanoic acid, salicylic acid, lauric acid, trimethyl borate, triethyl borate, and tributyl borate.

[0020] The acid anhydride curing agent is selected from at least one of hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, phthalic anhydride, hydrogenated trimellitic anhydride, tetrabromophthalic anhydride, diphenyl ether tetraacid dianhydride and methylnadic anhydride.

[0021] The curing accelerator is selected from at least one of imidazole accelerators, tertiary amine accelerators, and organic phosphine accelerators, preferably an imidazole accelerator, such as 2-methylimidazole, 2-phenylimidazole, 1,2-dimethylimidazole, and 2-ethyl-4-methylimidazole.

[0022] The present invention also provides a method for preparing the above-mentioned conductive silver paste with high thermal conductivity and high reliability, comprising the following steps:

[0023] (S1) adding epoxy resin, epoxy diluent, anhydride curing agent, stabilizer, silane coupling agent and accelerator into a stirring device, premixing and stirring at a vacuum degree of 0.05-0.1 MPa to obtain a matrix;

[0024] (S2) adding modified flaky silver powder and nano silver powder to the matrix, grinding the mixture, passing the ground product through a three-roll mill, filtering, and degassing to obtain a conductive silver paste with high thermal conductivity and high reliability.

[0025] Furthermore, the stirring speed is 1500-3000 rpm, and the stirring time is 10-30 min.

[0026] The present invention increases the mutual contact of silver powder particles and reduces the surface contact resistance through the conductive silver glue of the above formula and the reasonable compatibility of modified flaky silver powder and nano silver powder, so as to achieve a conductive silver glue with a low silver content having a very low volume resistivity, and the thermal conductivity and weather resistance are also improved. In addition, the compounded epoxy diluent plays a diluting role in reducing the viscosity of the conductive silver glue, and can also improve the toughness and bonding strength of the conductive silver glue after curing. The monoepoxy diluent with a long carbon chain can improve the toughness of the glue after curing. The dosage is controlled within a suitable range, and will not have an adverse effect on the hardness and thermal expansion coefficient of the cured product. The compounding with the multifunctional epoxy diluent will not reduce the crosslinking density, ensure the bonding strength, and prevent bubbles generated during the curing process, without the need to add an additional defoaming agent. DETAILED DESCRIPTION

[0027] The technical solution of the present invention is further explained below with specific implementation methods. Unless otherwise specified, the "parts" in the embodiments of the present invention are all parts by mass, and the "%" are all percentages by mass.

[0028] Preparation Example 1

[0029] 1 part by mass of spherical silver powder (D50 = 5.7 μm, purity ≥ 99.9%) is dispersed in 1.5 parts by mass of anhydrous ethanol, 0.03 parts of modifier (the modifier is gallic acid and carboxymethyl chitosan with a molecular weight of 20,000 in a mass ratio of 4:1) are added, and after mixing evenly, ball milling is performed at 40°C. The ball milling conditions are a ball-to-material ratio of 12:1, a rotation speed of 500 rpm, and a ball milling time of 15 hours. After the ball milling is completed, the solid is separated and immersed in an alcoholic acid solution mixed with ethanol and concentrated nitric acid in a volume ratio of 3:1 under 60kHz ultrasonic conditions. The solid is ultrasonically treated for 10, washed with ethanol and deionized water until neutral, and vacuum dried at 70°C and 0.1Mpa to obtain modified flaky silver powder. After testing, the modified flaky silver powder prepared in Preparation Example 1 has a particle size of 3-5 μm and a tap density of 3.4 g / cm 3 , specific surface area 1.2m 2 / g.

[0030] Preparation Example 2

[0031] Other conditions and operations were the same as those in Preparation Example 1, except that the mass ratio of spherical silver powder, anhydrous ethanol and modifier was changed from 1:1.5:0.03 to 1:1.6:0.05, and the molecular weight of carboxymethyl chitosan was 30,000.

[0032] Comparative Preparation Example 1

[0033] Other conditions and operations were the same as those in Preparation Example 1, except that the modifier was gallic acid.

[0034] Comparative Preparation Example 2

[0035] Other conditions and operations were the same as those in Preparation Example 1, except that the modifier was carboxymethyl chitosan with a molecular weight of 20,000.

[0036] Example 1

[0037] (S1) adding 15 parts of phenolic epoxy resin, 7 parts of epoxy diluent (compounded by C8 alkyl glycidyl ether and ethylene glycol diglycidyl ether in a mass ratio of 3:1), 8 parts of methyl hexahydrophthalic anhydride, 0.2 parts of trimethyl borate, 0.3 parts of γ-aminopropyl triethoxysilane, and 3 parts of 2-ethyl-4-methylimidazole into a stirring device, premixing, stirring for 20 minutes under a vacuum degree of 0.05 MPa, and mixing uniformly to obtain a matrix;

[0038] (S2) 50 parts of the modified flaky silver powder prepared in Preparation Example 1 and 6 parts of nano silver powder (particle size 200 nm) are added to the matrix, the mixture is ground, and the ground product is passed through a three-roll mill twice, filtered, and degassed to obtain a conductive silver paste with high thermal conductivity and high reliability.

[0039] Example 2

[0040] (S1) adding 20 parts of hydantoin epoxy resin, 10 parts of epoxy diluent (compounded in a mass ratio of 4:1 of C12 alkyl glycidyl ether and butanediol diglycidyl ether), 10 parts of tetrahydrophthalic anhydride, 0.3 parts of trimethyl borate, 0.3 parts of γ-aminopropyltriethoxysilane, and 5 parts of 2-ethyl-4-methylimidazole into a stirring device, stirring for 20 minutes under a vacuum degree of 0.05 MPa after premixing, and mixing uniformly to obtain a matrix;

[0041] (S2) 60 parts of the modified flaky silver powder of Preparation Example 1 and 8 parts of nano silver powder (particle size 200 nm) are added to the matrix, the mixture is ground, and the ground product is passed through a three-roll mill twice, filtered, and degassed to obtain a conductive silver paste with high thermal conductivity and high reliability.

[0042] Example 3

[0043] (S1) adding 10 parts of hydantoin epoxy resin, 5 parts of epoxy diluent (compounded with C8 alkyl glycidyl ether and trimethylolpropane triglycidyl ether in a mass ratio of 5:1), 5 parts of methyl hexahydrophthalic anhydride, 0.1 parts of trimethyl borate, 0.2 parts of γ-aminopropyl triethoxysilane, and 3 parts of 2-ethyl-4-methylimidazole into a stirring device, premixing, stirring for 20 minutes under a vacuum degree of 0.05 MPa, and mixing uniformly to obtain a matrix;

[0044] (S2) 45 parts of the modified flaky silver powder prepared in Preparation Example 1 and 5 parts of nano silver powder (particle size 200 nm) are added to the matrix, the mixture is ground, and the ground product is passed through a three-roll mill twice, filtered, and degassed to obtain a conductive silver paste with high thermal conductivity and high reliability.

[0045] Example 4

[0046] The other conditions are the same as those in Example 1, except that in step (S2), the modified flaky silver powder of Preparation Example 1 is replaced by that of Preparation Example 2.

[0047] Example 5

[0048] Other conditions are the same as those in Example 1, except that in step (S1), all 7 parts of epoxy diluent are C8 alkyl glycidyl ether.

[0049] Example 6

[0050] Other conditions are the same as those in Example 1, except that in step (S1), all 7 parts of epoxy diluent are ethylene glycol diglycidyl ether.

[0051] Comparative Example 1

[0052] The other conditions are the same as those in Example 1, except that in step (S2), the modified flaky silver powder of Preparation Example 1 is replaced by the one prepared in Comparative Preparation Example 1.

[0053] Comparative Example 2

[0054] The other conditions are the same as those in Example 1, except that in step (S2), the modified flaky silver powder of Preparation Example 1 is replaced by that of Comparative Preparation Example 2.

[0055] Comparative Example 3

[0056] The other conditions were the same as those in Example 1, except that in step (S2), the modified flaky silver powder of Preparation Example 1 was replaced with commercial flaky silver powder (Xingxin Material Technology Co., Ltd., particle size 3-5 μm, tap density 3.5 g / cm 3 ).

[0057] Comparative Example 4

[0058] Other conditions are the same as those in Example 1, except that in step (S2), no nano silver powder is added, and the amount of modified flaky silver powder added in Preparation Example 1 is changed to 56 parts.

[0059] Application Examples

[0060] The conductive silver pastes prepared in the above examples and comparative examples were subjected to the following performance tests, and the results are shown in Table 1.

[0061] Thermal conductivity test refers to ASTM E1461-13.

[0062] Dispensing stability: Through the die bong machine dispensing test, 100 2*2 cross samples are dispensed to judge the dispensing stability. The qualified rate ≥ 99% is excellent, 99%>qualified rate ≥ 95% is good, and 95%>qualified rate ≥ 90% is fair.

[0063] The volume resistivity test refers to GB / T6146-2010.

[0064] Thixotropic value: Use 2-20RPM, use Brookfield lamella viscometer, and calculate TI according to HG / T3660-1999 to test the sample viscosity at 25℃

[0065] Die shear strength is measured with reference to GB7124-86. A 2mm×2mm silicon die is dipped with 40μm glue and attached to a copper chip for curing at 150℃ / 30min. The test is conducted on a thrust machine.

[0066] Table 1 Performance test results

[0067]

[0068]

Claims

1. A conductive silver paste with high thermal conductivity and high reliability, characterized in that: The invention comprises the following raw materials in parts by weight: 10-20 parts of epoxy resin, 5-10 parts of epoxy diluent, 5-10 parts of anhydride curing agent, 0.1-0.3 parts of stabilizer, 0.1-0.3 parts of silane coupling agent, 1-5 parts of accelerator, 45-60 parts of modified flaky silver powder and 5-8 parts of nano silver powder; the modified flaky silver powder is obtained by ball milling spherical silver powder in the presence of a modifier compounded with gallic acid and carboxymethyl chitosan, and then ultrasonically treating an alcohol-acid mixed solution; the amount of the modifier used is 3-5wt% of the spherical silver powder.

2. The conductive silver paste with high thermal conductivity and high reliability according to claim 1, characterized in that: The mass ratio of gallic acid to carboxymethyl chitosan is 4-7:1, and the molecular weight of carboxymethyl chitosan is 20,000 to 30,000.

3. The conductive silver paste with high thermal conductivity and high reliability according to claim 1, characterized in that: The modified flaky silver powder is prepared by a preparation method comprising the following steps: dispersing spherical silver powder in an alcohol solvent, adding a modifier, ball milling at 40-50° C., separating after ball milling, immersing in an alcohol acid solution of alcohol and concentrated nitric acid under ultrasonic conditions, treating for 10-20 minutes, washing, and drying to obtain the modified flaky silver powder.

4. The conductive silver paste with high thermal conductivity and high reliability according to claim 3, characterized in that: The particle size of the spherical silver powder is 5-10 μm, the purity is ≥99%, preferably the purity is ≥99.9%; the particle size of the modified flaky silver powder is 3-5 μm, and the tap density is 3.2-3.6 g / cm 3 , specific surface area 1.1-1.5m 2 / g.

5. The conductive silver paste with high thermal conductivity and high reliability according to claim 3, characterized in that: The alcohol solvent is selected from at least one of methanol, ethanol, propanol, diethanol and propylene glycol, preferably ethanol; Further, the mass ratio of the spherical silver powder, the alcohol solvent and the modifier is 1:1.2-1.6:0.03-0.05; Furthermore, the conditions for ball milling are a ball-to-material ratio of 10-20:1, a rotation speed of 400-500 rpm, and a ball milling time of 10-15 h; Furthermore, in the preparation of the alkyd solution, the volume ratio of alcohol to concentrated nitric acid is 3-4:1, the alcohol is selected from at least one of methanol, ethanol, and isopropanol, preferably ethanol; and the ultrasonic condition is 60-100 kHz.

6. The conductive silver paste with high thermal conductivity and high reliability according to claim 1, characterized in that: The epoxy resin is selected from at least one of bisphenol epoxy resin, novolac epoxy resin, bisphenol S epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin.

7. The conductive silver paste with high thermal conductivity and high reliability according to claim 1, characterized in that: The epoxy diluent is selected from at least one of C8-C12 alkyl glycidyl ether, benzyl glycidyl ether, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, and neopentyl glycol diglycidyl ether.

8. The conductive silver paste with high thermal conductivity and high reliability according to claim 1, characterized in that: The epoxy diluent is a compound of C8-C12 alkyl carboxylic acid glyceryl ether and an epoxy diluent with an epoxy functionality of 2-3 in a mass ratio of 2.2-3.5:1; the C8-C12 alkyl carboxylic acid glyceryl ether is selected from at least one of C8 alkyl glycidyl ether, C9 alkyl glycidyl ether, C10 alkyl glycidyl ether, C11 alkyl glycidyl ether, and C12 alkyl glycidyl ether; the epoxy diluent with an epoxy functionality of 2-3 is selected from at least one of ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, and neopentyl glycol diglycidyl ether.

9. The conductive silver paste with high thermal conductivity and high reliability according to claim 1, characterized in that: The silane coupling agent is selected from at least one of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane and γ-(2,3-epoxypropyloxy)propyltrimethoxysilane; and / or The stabilizer is selected from at least one of glutaric acid, adipic acid, benzoic acid, n-decanoic acid, salicylic acid, lauric acid, trimethyl borate, triethyl borate, and tributyl borate; and / or The anhydride curing agent is selected from at least one of hexahydrophthalic anhydride, methyl hexahydrophthalic anhydride, tetrahydrophthalic anhydride, methyl tetrahydrophthalic anhydride, phthalic anhydride, hydrogenated trimellitic anhydride, tetrabromophthalic anhydride, diphenyl ether tetraacid dianhydride and methyl nadic anhydride; and / or The curing accelerator is selected from at least one of imidazole accelerators, tertiary amine accelerators, and organic phosphine accelerators, preferably an imidazole accelerator, such as 2-methylimidazole, 2-phenylimidazole, 1,2-dimethylimidazole, and 2-ethyl-4-methylimidazole.

10. The method for preparing the conductive silver paste with high thermal conductivity and high reliability according to any one of claims 1 to 9, characterized in that: The following steps are involved: (S1) adding epoxy resin, epoxy diluent, anhydride curing agent, stabilizer, silane coupling agent and accelerator into a stirring device, premixing and stirring at a vacuum degree of 0.05-0.1 MPa to obtain a matrix; (S2) adding modified flaky silver powder and nano silver powder to the matrix, grinding the mixture, passing the ground product through a three-roll mill, filtering, and degassing to obtain a conductive silver paste with high thermal conductivity and high reliability.

Citation Information

Patent Citations

  • Functional graphene-doped epoxy resin conductive adhesive and preparation method thereof

    CN103614098A

  • Method for surface modification of flaky silver powder

    CN105618734A

  • High-thermal-conductivity and high-electric-conductivity adhesive and preparation method thereof

    CN118272020A

  • Preparation process of modified epoxy resin conductive adhesive

    CN118406456A

Cited By

  • High-thermal-conductivity sintered conductive adhesive and preparation method thereof

    CN120464349A

  • Conductive paste containing carbon nanotubes and application of conductive paste in LED chips

    CN121938691A

  • Low-silver conductive adhesive containing inorganic filler and preparation method thereof

    CN122445306A