Method for photocatalytic synthesis of lead sulfide quantum dots and application
By introducing light energy treatment into the halogen compounds of zinc sulfide and lead, the energy and time required for nucleation of lead sulfide quantum dots is reduced, and the problem of poor monodispersity of lead sulfide quantum dots is solved, and its optical performance and photoelectricity are improved. Conversion efficiency, suitable for photodetectors and solar absorbers.
Patent Information
- Application Number
- CN202311835482.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2024-12-03
AI Technical Summary
In the prior art, when preparing lead sulfide quantum dots, it is difficult to achieve excellent monodispersity in temperature control, resulting in inconsistent particle size and affecting the performance of optoelectronic devices.
By using light energy to treat the halogen compounds of zinc sulfide and lead in the oleic acid/oleamine reaction system, the energy and time required for quantum dot nucleation are reduced, and the size uniformity of lead sulfide quantum dots is improved.
It realizes high monodispersity of lead sulfide quantum dots, improves optical performance and photoelectric conversion efficiency, and is suitable for photodetectors and solar absorbers.
Smart Images

Figure CN119060727A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lead sulfide quantum dot preparation, and in particular to a method and application of photocatalytic synthesis of lead sulfide quantum dots. Background Art
[0002] Semiconductor quantum dots are a kind of quasi-zero-dimensional nanomaterial. When the particle size enters the nanometer scale, the size confinement will cause size effect, quantum confinement effect, macroscopic quantum tunneling effect and surface effect, thus deriving low-dimensional physical properties of nanosystems that are different from macroscopic and microscopic systems, and showing many physical and chemical properties different from macroscopic bulk materials. Lead sulfide (PbS) quantum dots, as a group IV-VI semiconductor quantum material, are important π-π bond semiconductor materials. Lead sulfide quantum dots have a narrow direct band gap. Compared with other semiconductor quantum dots, the exciton Bohr radius of lead sulfide quantum dots is larger, about 18nm, which makes it easy to obtain a strong quantum confinement effect; since the fluorescence generated by quantum dots can cover the entire transmission window, lead sulfide quantum dots have broad application prospects in optical devices, such as infrared detectors, solar absorbers, optical switches, etc.; since the multiple exciton effect has been observed on quantum dots, lead sulfide quantum dots are expected to become an important preparation material for high-efficiency photoelectric conversion devices.
[0003] The existing method for preparing lead sulfide quantum dots is mainly to make the quantum dots interact with each other by heating, thereby causing aggregation to form a cluster structure (quantum dot nucleation). The mechanism of quantum dot heating aggregation can be explained by thermodynamic and kinetic processes. During the heating process, the electrons inside the quantum dots are excited to a high-energy state, and these excited electrons have greater mobility. At the same time, heating causes the atoms or molecules on the surface of the quantum dots to vibrate thermally, increasing the dynamics of the surface. These high-energy electrons and the thermal vibrations of the surface work together to enhance the mutual attraction between the quantum dots, thereby promoting the aggregation of the quantum dots to form a cluster structure. It is precisely because quantum dots need to be heated to provide energy in the process of forming cluster structures that the time for cluster formation and the degree of reaction will be strictly affected by temperature. If the temperature is too high, it will lead to solvent volatilization and increased side reactions; if the temperature is low, the energy provided is insufficient, and in the process of continuous growth of lead sulfide quantum dots, the duration is long, which is not conducive to controlling the particle size of the quantum dot product, and ultimately leads to poor monodispersity of lead sulfide quantum dots. Poorly monodispersed quantum dots, that is, they have different sizes, will increase the energy disorder in optoelectronic devices prepared with these quantum dots as raw materials, thereby hindering their performance, which will further affect the application of lead sulfide quantum dot materials in the preparation of optical devices.
[0004] In view of this, developing a method for preparing lead sulfide quantum dots with excellent monodispersity has become a difficult problem in the prior art. Summary of the invention
[0005] In view of the deficiencies of the above-mentioned prior art, the present application provides a method and application of photocatalytic synthesis of lead sulfide quantum dots, the purpose of which is to react zinc sulfide (ZnS) with lead halogen compounds (such as lead chloride, lead bromide, lead iodide, etc.) in a reaction system such as oleic acid / oleylamine in the process of preparing lead sulfide quantum dots by cation exchange, and apply additional light energy during the reaction to reduce the energy required for the quantum dots to form a cluster structure (nucleation growth), thereby reducing the time required for quantum dot nucleation, accelerating the growth process of quantum dots, and thus improving the size uniformity (i.e., monodispersity) of the lead sulfide quantum dots.
[0006] To achieve the above objectives, this application provides at least the following technical solutions:
[0007] In a first aspect, the present application provides a method for photocatalytic synthesis of lead sulfide quantum dots, comprising the following steps:
[0008] (1) mixing a lead halogen compound (lead halide) and oleylamine (OLA) to form a first mixture, and placing the first mixture in an inert gas environment and under light conditions for 2 to 5 minutes;
[0009] (2) heating the first mixture to fully dissolve the lead halide in oleylamine to obtain an oleylamine solution of lead halide;
[0010] (3) placing zinc sulfide (ZnS) nanorods under light conditions for 2 to 5 minutes, injecting them into an oleylamine solution of lead halide to obtain a second mixture, wherein the reaction time of the second mixture is controlled within 10 seconds to 5 minutes; adding oleic acid to obtain a third mixture;
[0011] (4) After the reaction is completed, the third mixture is cooled to room temperature, centrifuged, and filtered to obtain lead sulfide quantum dots.
[0012] Furthermore, the halogen compound (lead halide) is at least one of lead chloride (PbCl2), lead bromide (PbBr2), and lead iodide (PbI2).
[0013] Furthermore, the inert gas is any one of nitrogen (N2), argon (Ar), helium (He), neon (Ne), krypton (kr), xenon (xe) and radon (Rn).
[0014] Furthermore, the wavelength of the light in (1) and (3) is 400 to 1100 nm; the light intensity is 10 uW to 100 mW.
[0015] Furthermore, in step (2), the first mixture is heated to a temperature of 80 to 150°C.
[0016] Preferably, in step (3), the molar ratio of the zinc sulfide nanorods to the lead halide is no more than 1:2; and the zinc sulfide (ZnS) nanorods are injected into the lead halide oleylamine solution for no more than 10 seconds.
[0017] Preferably, in step (3), the reaction temperature of the second mixture is controlled at 80-190°C.
[0018] In a second aspect, the present application provides a lead sulfide quantum dot, which is prepared by the aforementioned method.
[0019] In a third aspect, the present application provides the application of the aforementioned quantum dots in the preparation of photodetectors, solar absorbers or optical switches.
[0020] Compared with the prior art, the technical solution provided by this application has at least the following technical effects:
[0021] The technical solution provided in the present application subjects zinc sulfide and lead halogen compounds to light treatment respectively, so that both zinc sulfide and lead halogen compounds are in an excited state. In this excited state, during the cation exchange reaction between zinc sulfide and lead halogen compounds, the energy required to form clustered lead sulfide quantum dots is greatly reduced, the zinc sulfide and lead halogen compounds are increased, thereby reducing the time required for nucleation of lead sulfide quantum dots, accelerating the growth process of quantum dots, and further improving the size uniformity of lead sulfide quantum dots. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The present application will be further described in detail below in conjunction with the accompanying drawings and preferred embodiments, but those skilled in the art will appreciate that these drawings are drawn only for the purpose of explaining the preferred embodiments and therefore should not be used as a limitation on the scope of the present application. In addition, unless otherwise specified, the drawings are only schematically representing the composition or structure of the described objects and may contain exaggerated displays, and the drawings are not necessarily drawn to scale.
[0023] Figure 1 This is the light absorption curve of the lead sulfide quantum dots prepared in Example 1 of the present application.
[0024] Figure 2 This is the light absorption curve of the lead sulfide quantum dots prepared in Example 2 of the present application.
[0025] Figure 3 This is the light absorption curve of the lead sulfide quantum dots prepared in Example 3 of the present application.
[0026] Figure 4 This is the light absorption curve of the lead sulfide quantum dots prepared in Comparative Example 1 of the present application.
[0027] Figure 5This is a schematic diagram of the structure of the lead sulfide infrared quantum dot detector provided in an embodiment of the present application, wherein 1 is a bottom electrode layer, 2 is an electron blocking layer, 3 is a p-type layer, 4 is an active layer, 5 is an electron transport layer, 6 is a strong n-type layer, and 7 is a top electrode layer. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical scheme and advantages of the present application more clear, the concept of the present application and the technical effects produced are further described in detail below in conjunction with the accompanying drawings and embodiments, so as to fully understand the purpose, features and effects of the present application. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application. Other embodiments obtained by technicians in this field without creative work are all within the scope of protection of the present application.
[0029] In this application, the term "room temperature" refers to indoor temperature, normal temperature or general temperature. It should be understood that indoor temperature is not an absolute value, but fluctuates due to the influence of weather, season, indoor environment, etc., and its range is generally between 8 and 35°C.
[0030] In this application, the term "monodispersity" refers to the property of the quantum dot material particle size to maintain a uniform shape. In some contexts, "monodispersity" also refers to the degree to which the quantum dot size maintains uniformity. If the size uniformity is high, the monodispersity is good, and vice versa, the monodispersity is low. In the application of quantum dot materials, "monodispersity" quantum dots are easier to achieve precise performance control. Therefore, "monodispersity" is an important consideration in measuring the performance of quantum dot materials.
[0031] The embodiment of the present application is different from the traditional method for synthesizing lead sulfide quantum dots. It introduces light into the key step of the synthesis of lead sulfide quantum dots, reduces the energy required for the lead sulfide quantum dots to form clusters, avoids the adverse effects of excessively high or low temperatures in the reaction system, accelerates the growth of lead sulfide quantum dots, greatly reduces the nucleation time of lead sulfide quantum dots, and obtains a monodisperse lead sulfide quantum dot material with uniform particle size and good surface passivation. The prepared lead sulfide quantum dot material has a high photon absorption peak-to-valley ratio, reflecting excellent optical properties.
[0032] Based on this, an embodiment of the present application provides a method for photocatalytically synthesizing lead sulfide quantum dots, comprising the following steps: mixing a lead halogen compound (lead halide) with oleylamine (OLA) to form a first mixture, and placing the first mixture under an inert gas environment and light conditions at the same time; heating the first mixture to fully dissolve the lead halide in the oleylamine to obtain an oleylamine solution of the lead halide; placing zinc sulfide (ZnS) nanorods not exceeding 50% of the molar amount of the lead halide under light conditions, injecting them into the oleylamine solution of the lead halide to obtain a second mixture, adding oleic acid to the second mixture to obtain a third mixture, cooling the third mixture to room temperature, centrifuging, and filtering to obtain lead sulfide quantum dots.
[0033] In some embodiments, the halogen compound (lead halide) is at least one of lead chloride (PbCl2), lead bromide (PbBr2), and lead iodide (PbI2).
[0034] In some embodiments, the inert gas is any one of nitrogen (N2), argon (Ar), helium (He), neon (Ne), krypton (kr), xenon (xe) and radon (Rn).
[0035] In some embodiments, the illumination conditions are: illumination wavelength is 400-1100 nm; illumination intensity is 10 uW-100 mW, and illumination time is 2-5 min.
[0036] In certain embodiments, the first mixture is heated to a temperature of 80-150°C.
[0037] In certain embodiments, the zinc sulfide (ZnS) nanorods are injected into the lead halide oleylamine solution for a period of no more than 10 seconds.
[0038] In certain embodiments, the reaction temperature of the second mixture is controlled at 80-190°C.
[0039] Based on this, the present application provides a lead sulfide quantum dot, which is prepared by the above method.
[0040] Based on this, the present application provides the application of the aforementioned quantum dots in the preparation of photodetectors or solar absorbers or optical switches.
[0041] The technical solution of the present application will be described below through more specific embodiments.
[0042] Example 1
[0043] The present application embodiment provides a method for photocatalytic synthesis of lead sulfide quantum dot materials, and the specific steps are as follows:
[0044] A certain amount of lead chloride (PbCl2) was weighed and dissolved in oleylamine (OLA) to obtain a 0.1 mol / L lead chloride oleylamine solution, the lead chloride oleylamine solution was placed in an inert environment of nitrogen (N2) and irradiated with light, wherein the illumination wavelength was 400 nm, the illumination intensity was 10 uW, and the illumination time was 3 min; the lead chloride oleylamine solution was heated to 150°C and kept warm for 30 min, 1 / 2 of the molar amount of lead chloride was taken and placed under light, wherein the illumination wavelength was 400 nm, the illumination intensity was 10 uW, and the illumination time was 3 min; then the lead chloride oleylamine solution was placed in an inert environment of nitrogen (N2) and irradiated with light, wherein the illumination wavelength was 400 nm, the illumination intensity was 10 uW, and the illumination time was 3 min. When the temperature of the solution drops to 120°C, ZnS nanorods and oleylamine solution of lead chloride are quickly injected within 10 seconds for mixed reaction, and the reaction time is 3 minutes; when the temperature of the mixed reactant drops to 70°C, n-hexane is injected into the mixed reactant; when the temperature of the mixed reactant drops to 40°C, oleic acid is injected into the mixed reactant; after the reaction is completed, the mixed solution is cooled to room temperature, ethanol is added, centrifuged (5000r / m, 10min), then n-hexane is added, centrifuged (3000r / m, 5min), filtered, and then ethanol is added and centrifuged (5000r / m, 10min) to obtain lead sulfide quantum dots.
[0045] Example 2
[0046] The present application embodiment provides a method for photocatalytic synthesis of lead sulfide quantum dot materials, and the specific steps are as follows:
[0047] A certain amount of lead bromide (PbBr2) is weighed and dissolved in oleylamine (OLA) to obtain a 0.3 mol / L lead bromide oleylamine solution, the lead bromide oleylamine solution is placed in an inert environment of nitrogen (N2) and irradiated with light, wherein the illumination wavelength is 600 nm, the illumination intensity is 1 mW, and the illumination time is 3 min; the lead bromide oleylamine solution is heated to 80°C and kept warm for 30 min, 1 / 2 of the molar amount of lead bromide zinc sulfide nanorods are placed under illumination, wherein the illumination wavelength is 600 nm, the illumination intensity is 1 mW, and the illumination time is 3 min; keep the lead bromide oleylamine solution The temperature of the solution is 80°C, and an oleylamine solution of ZnS nanorods and lead bromide is quickly injected within 10 seconds for a mixed reaction, and the reaction time is 3 minutes; when the temperature of the mixed reactant drops to 70°C, n-hexane is injected into the mixed reactant; when the temperature of the mixed reactant drops to 40°C, oleic acid is injected into the mixed reactant; after the reaction is completed, the mixed solution is cooled to room temperature, ethanol is added, centrifuged (5000r / m, 10min), then n-hexane is added, centrifuged (3000r / m, 5min), filtered, and then ethanol is added and centrifuged (5000r / m, 10min) to obtain lead sulfide quantum dots.
[0048] Example 3
[0049] The present application embodiment provides a method for photocatalytic synthesis of lead sulfide quantum dot materials, and the specific steps are as follows:
[0050] A certain amount of lead iodide (PbI2) was weighed and dissolved in oleylamine (OLA) to obtain a 0.3 mol / L lead iodide oleylamine solution, the lead iodide oleylamine solution was placed in an inert environment of nitrogen (N2) and treated by light, wherein the light wavelength was 1100 nm, the light intensity was 100 mW, and the light irradiation time was 3 min; the lead iodide oleylamine solution was heated to 120°C and kept warm for 30 min, zinc sulfide nanorods with 1 / 2 the molar amount of lead iodide were placed under light, wherein the light wavelength was 1100 nm, the light intensity was 100 mW, and the light irradiation time was 3 min; When the oleylamine solution is heated to 190°C, the oleylamine solution of ZnS nanorods and lead iodide is quickly injected within 10s for a mixed reaction, and the reaction time is 3min; when the temperature of the mixed reactant drops to 70°C, n-hexane is injected into the mixed reactant; when the temperature of the mixed reactant drops to 40°C, oleic acid is injected into the mixed reactant; after the reaction is completed, the mixed solution is cooled to room temperature, ethanol is added, centrifuged (5000r / m, 10min), then n-hexane is added, centrifuged (3000r / m, 5min), filtered, and then ethanol is added and centrifuged (5000r / m, 10min) to obtain lead sulfide quantum dots.
[0051] Comparative Example 1
[0052] This comparative example provides a method for photocatalytically synthesizing lead sulfide quantum dot materials, and the specific steps are as follows:
[0053] A certain amount of lead chloride (PbCl2) was weighed and dissolved in oleylamine (OLA) to obtain a 0.1 mol / L lead chloride oleylamine solution, which was placed in an inert environment of nitrogen (N2); the lead chloride oleylamine solution was heated to 150°C and kept warm for 30 minutes, and zinc sulfide nanorods with a molar amount of 1 / 2 of the lead chloride were taken; then when the temperature of the lead chloride oleylamine solution was reduced to 120°C, ZnS nanorods were quickly injected within 10 seconds to mix with the lead chloride oleylamine solution. The method comprises the following steps: reacting the mixture for 3 minutes; when the temperature of the mixed reactant drops to 70°C, injecting n-hexane into the mixed reactant; when the temperature of the mixed reactant drops to 40°C, injecting oleic acid into the mixed reactant; after the reaction is completed, the mixed solution is cooled to room temperature, ethanol is added, and the mixture is centrifuged (5000r / m, 10min), then n-hexane is added, centrifuged (3000r / m, 5min), filtered, and then ethanol is added and centrifuged (5000r / m, 10min) to obtain lead sulfide quantum dots.
[0054] The lead sulfide quantum dots prepared in Examples 1 to 3 and Comparative Example 1 were taken, and the optical absorption properties of each lead sulfide quantum dot were measured by fluorescence spectrometer.
[0055] The absorption spectrum of quantum dots refers to the spectrum of photon absorption by a substance, which reflects the absorption capacity of quantum dots for light of different wavelengths. The peak of the absorption spectrum refers to the position where the absorption intensity of a certain wavelength of light reaches the maximum when the quantum dots absorb photons, that is, when the wavelength of light and the energy level gap of the quantum dots match, the absorption of light by the quantum dots reaches the maximum. The trough of the absorption spectrum is the position on the spectrum graph where the corresponding light intensity is the lowest. The monodispersity of Gaussian distributed quantum dots is closely related to the peak-to-valley ratio. Monodisperse quantum dots have consistency in size, energy level, shape, etc., making their optical properties more uniform. This uniformity directly affects the spectral characteristics, making monodisperse quantum dots present clearer and sharper peaks in the absorption or emission spectrum, while deepening the adjacent troughs. The larger the peak-to-valley ratio (ratio of peak value to valley value), the better the monodispersity performance of the quantum dots.
[0056] Figures 1 to 4 The optical absorption spectra of lead sulfide quantum dots prepared in Examples 1 to 3 and Comparative Example 1 are respectively. It can be seen from the figures that the peak-to-valley ratios of the absorption spectra of the lead sulfide quantum dots prepared in Examples 1 to 3 are 7.5, 7.2, and 6.5, respectively; all of which are much higher than the peak-to-valley ratio of 5.1 of the absorption spectrum of the lead sulfide quantum dots prepared in Comparative Example 1; the above results show that the lead sulfide quantum dots prepared by the method for photocatalytic synthesis of lead sulfide quantum dot materials provided in the embodiments of the present application have uniform particle size and better monodispersity.
[0057] Through analysis, the reasons for the above results are as follows: According to the nucleation equation of quantum dots (Arrhenius): I = I0exp(-E a / kT), where I is the nucleation rate, I0 is a temperature-independent constant representing the nucleation rate before thermal activation, and E a is the nucleation activation energy, k is the Boltzmann constant, and T represents the temperature (Kelvin); in this equation, the temperature T is the parameter that mainly affects the nucleation rate. However, in the embodiment of the present application, after the light treatment, the nucleation activation energy E of the quantum dots is a In addition, light can provide additional energy besides temperature heating, resulting in a significant reduction in the energy provided by the required temperature during the actual reaction process. Therefore, the degree of reaction between zinc sulfide and lead halide in the cation exchange process can be increased, and the nucleation time of lead sulfide quantum dots can be reduced, thereby achieving lead sulfide quantum dots with excellent monodispersity.
[0058] In addition, if the zinc sulfide nanorods are injected into the lead halide solution for too long (more than 10 seconds), the injection rate is too fast, or the total amount of zinc sulfide injected is too much (more than 1 / 2 of the molar amount of lead halide), it will cause insufficient reaction between zinc sulfide and lead halide, lower reaction activity, longer growth time, etc., which will ultimately lead to poor monodispersity of the generated lead sulfide quantum dot material.
[0059] Example 4
[0060] The present application provides an infrared photoelectric detector, such as Figure 2 As shown, it includes: a bottom electrode layer 1, and an electron blocking layer 2, a p-type layer 3, an active layer 4, an electron transport layer 5, a strong n-type layer 6, and a top electrode layer 7 arranged in sequence in a direction away from the bottom electrode layer 1. The material of the active layer 4 is the lead sulfide quantum dots prepared in the above-mentioned embodiment. The materials of the bottom electrode layer 1 and the top electrode layer 7 are indium tin oxide thin films (ITO), the material of the electron blocking layer 2 is NiO2 or NiO3, the material of the p-type 3 is PbS-1,2-ethanedithiol (PbS-EDT), the material of the electron transport layer 5 is C60, and the material of the strong n-type layer 6 is a SnO2 layer.
[0061] The present application embodiment provides a method for preparing the above infrared photoelectric detector, and the specific steps are as follows:
[0062] (1) preparing an electron blocking layer 2 on the bottom electrode layer 1 by a magnetron sputtering method;
[0063] (2) preparing a p-type layer 3 on the electron blocking layer 2 by spin coating layer by layer: uniformly mixing a 10-40 mg / mL quantum dot solution with tetramethylsilane as solvent and PbS as solute with an acetonitrile solution with a 1,2-ethanedithiol content of 0.01% to 1% to prepare a p-type layer 3 material precursor solution, placing the p-type layer 3 material precursor solution on the electron blocking layer 2 by spin coating layer by layer, wherein the spin coating thickness is 20 nm; oxidizing in a high oxygen environment for 10 to 20 h to increase the doping concentration of PbS;
[0064] (3) preparing lead sulfide quantum dots by referring to the method of Examples 1 to 3, that is, preparing the precursor of the active layer 4 material;
[0065] (4) preparing an active layer 4 on the p-type layer 3 by spin coating;
[0066] (5) Preparing an electron transport layer 5 on the active layer 4: placing the active layer 4 on a thermal evaporation instrument; adjusting the current, and controlling the rate of thermal evaporation of the C60 source by a film thickness meter, and thermally evaporating the C60 to a thickness of 10 to 20 nm to complete the thermal evaporation, thereby forming the electron transport layer 5;
[0067] (6) Preparing a strong n-type layer 6 on the electron transport layer 5: placing the electron transport layer 5 on an atomic layer deposition platform and evacuating the layer; heating the device substrate platform and the tin source to a preset temperature and then performing atomic layer deposition; after reaching the number of cycles, a 20 to 40 nm thick SnO2 layer is obtained to form a strong n-type layer 6; closing the device and taking out the device;
[0068] (7) The top electron layer 7 is prepared by magnetron sputtering on the strong n-type layer 6: the magnetron sputtering method is used to prepare the top electron layer 7. -3 ~10 -2 The top electron layer 7 was prepared by sputtering indium tin oxide at 1 pa, wherein the oxygen-argon ratio was 0.3:66.3, the sputtering power was 80 W, and the sputtering time was 20 min. Finally, the following was obtained: Figure 2 Infrared photodetector shown.
[0069] After testing, the infrared photodetector's external quantum efficiency reached 65%, and the specific detection rate exceeded 10 12 Jones.
[0070] In summary, the detection performance of quantum dot infrared detectors prepared by photocatalytic passivation can be significantly improved compared with traditional quantum dot infrared detectors.
[0071] The present application is described in detail above. Specific examples are used in the present application to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the present application and its core ideas. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present application, several improvements and modifications can be made to the present application, and these improvements and modifications also fall within the scope of protection of the claims of the present application.
Claims
1. A method for photocatalytic synthesis of lead sulfide quantum dots, characterized in that: The following steps are involved: (1) mixing lead halide and oleylamine to form a first mixture, and placing the first mixture in an inert gas environment and under light conditions for 2 to 5 minutes; (2) heating the first mixture to fully dissolve the lead halide in oleylamine to obtain an oleylamine solution of lead halide; (3) placing the zinc sulfide nanorods under light conditions for 2 to 5 minutes, injecting them into an oleylamine solution of lead halide to obtain a second mixture, wherein the reaction time of the second mixture is controlled within 10 seconds to 5 minutes; adding oleic acid to obtain a third mixture; (4) After the reaction is completed, the third mixture is cooled to room temperature, centrifuged, and filtered to obtain lead sulfide quantum dots.
2. The method according to claim 1, characterized in that The lead halide is at least one of lead chloride, lead bromide and lead iodide.
3. The method according to claim 1, characterized in that The inert gas is any one of nitrogen, argon, helium, neon, krypton, xenon and radon.
4. The method according to claim 1, characterized in that: The wavelength of the light in (1) and (3) is 400 to 1100 nm; the light intensity is 10 uW to 100 mW.
5. The method according to claim 1, characterized in that: In step (2), the first mixture is heated to a temperature of 80 to 150°C.
6. The method according to claim 1, characterized in that In step (3), the molar ratio of the zinc sulfide nanorods to the lead halide is no more than 1:2, and the zinc sulfide nanorods are injected into the lead halide oleylamine solution for no more than 10 seconds.
7. The method according to claim 1, characterized in that The reaction temperature of the second mixture is controlled at 80-190°C.
8. The method according to claim 1, characterized in that The method further comprises the step (3) of injecting n-hexane into the second mixture before adding oleic acid.
9. A lead sulfide quantum dot, characterized in that: The method is prepared by any one of claims 1 to 8.
10. Use of the lead sulfide quantum dots according to claim 9 in preparing photodetectors, solar absorbers or optical switches.