Resourceful treatment method of cobalt nickel hydroxide

Through the oxidation process, the divalent manganese in nickel hydroxide is oxidized to a higher valence state, and through the staged acid leaching and separation process, the problem of insufficient separation of nickel, cobalt and manganese in the prior art is solved, and high purity is achieved , the acquisition of high-value products reduces the cost and wastewater treatment burden.

CN119061264AActive Publication Date: 2024-12-03GUANGXI CNGR NEW ENERGY SCI & TECH CO LTD +1

Patent Information

Application Number
CN202411044027.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-12-03
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The existing nickel-cobalt hydroxide treatment process cannot fully separate nickel, cobalt, manganese and other elements, resulting in limited product purity and value.

Method used

The oxidation process is used to oxidize divalent manganese into a higher valence state. Through the staged acid leaching and separation process, nickel, cobalt and manganese are gradually separated, and the optimized use of oxidants and acids are used to control the pH value and reaction conditions of the slurry to achieve nickel. , effective separation of cobalt and manganese.

Benefits of technology

It improves the purity and product value of elements such as nickel, cobalt, manganese, reduces the cost of auxiliary materials, shortens the extraction process, reduces wastewater production and treatment costs, and obtains higher product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061264A_ABST
    Figure CN119061264A_ABST
Patent Text Reader

Abstract

The invention provides a resourceful treatment method of nickel cobalt hydroxide, which comprises the following steps: an oxidation process: slurrying nickel cobalt hydroxide to obtain slurry, mixing the slurry with an oxidizing agent, and carrying out oxidation reaction to oxidize divalent manganese contained in the nickel cobalt hydroxide into manganese with higher valence in a solid state to obtain an oxidized material; a first leaching process: carrying out acid leaching on the oxidized material to obtain a first leaching solution and first leaching residues containing manganese with higher valence state; the second leaching procedure is conducted, specifically, the first leaching residues are subjected to acid leaching, second leaching liquid and second leaching residues containing manganese with the higher valence state are obtained, and the second leaching liquid is returned to the oxidation procedure and used for being mixed with nickel cobalt hydroxide to be pulpified; and a separation step of separating nickel and cobalt contained in the first leachate to obtain a nickel-containing material and a cobalt-containing material. According to the embodiment of the invention, the cobalt nickel hydroxide is firstly oxidized, and then staged leaching and separation are carried out, so that various elements such as nickel, cobalt, manganese and the like contained in the cobalt nickel hydroxide can be fully separated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of nickel cobalt hydroxide processing, and in particular to a method for resource processing of nickel cobalt hydroxide. Background Art

[0002] Nickel cobalt hydroxide (MHP) can be made from laterite nickel ore, which is then prepared through high-pressure acid leaching technology, or it can be prepared from battery black powder. If the nickel, cobalt, manganese and other elements contained in nickel cobalt hydroxide can be separated, it will effectively alleviate the demand for nickel, cobalt, manganese and other elements in the new energy field.

[0003] The current process route for treating nickel cobalt hydroxide is mainly to first reduce and leach various elements and then gradually separate them. However, this method is still insufficient for separating various elements such as nickel, cobalt, and manganese contained in nickel cobalt hydroxide. The purity of the separated product is limited, resulting in limited product value. Summary of the invention

[0004] The present application provides a method for resource processing of nickel cobalt hydroxide, which can effectively separate various elements such as nickel, cobalt, and manganese contained in nickel cobalt hydroxide.

[0005] The embodiment of the present application provides a resource processing method for nickel cobalt hydroxide, comprising the following steps: an oxidation step, slurrying the nickel cobalt hydroxide to obtain a slurry, mixing the slurry with an oxidant to carry out an oxidation reaction so that the divalent manganese contained in the nickel cobalt hydroxide is oxidized to a higher-valent manganese in a solid form, to obtain an oxidized material; a first leaching step, acid leaching the oxidized material to leach nickel and cobalt, to obtain a first leachate and a first leaching residue containing the higher-valent manganese; a second leaching step, acid leaching the first leaching residue to further leach nickel and cobalt, to obtain a second leachate and a second leaching residue containing the higher-valent manganese, wherein the second leachate is returned to the oxidation step and used for mixing with the nickel cobalt hydroxide to form a slurry; a separation step, separating the nickel and cobalt contained in the first leachate to obtain a nickel-containing material and a cobalt-containing material.

[0006] The resource recovery treatment method provided in the embodiment of the present application is to oxidize the divalent manganese contained in the nickel cobalt hydroxide into a higher valence manganese in a solid form in the oxidation process, so that manganese is difficult to be leached during the acid leaching in the first leaching process, thereby separating manganese from other possible elements such as nickel and cobalt that are more easily leached, and obtaining a first leaching solution containing nickel and cobalt and a first leaching residue containing manganese; then further leaching the first leaching residue in the second leaching process to obtain a second leaching residue containing manganese with a higher purity, and separating the first leaching solution in the separation process to separate nickel and cobalt, thereby obtaining a nickel-containing material and a cobalt-containing material. Therefore, according to the resource recovery treatment method provided in the embodiment of the present application, the nickel cobalt hydroxide is first oxidized, and then leached and separated in stages, so that various elements such as nickel, cobalt, and manganese contained in the nickel cobalt hydroxide can be fully separated, which is conducive to obtaining various products with higher purity and greater value.

[0007] In some embodiments of the present application, in the oxidation process, the slurrying includes mixing a solvent with the nickel cobalt hydroxide to obtain a slurry, wherein a component of the solvent includes the second leachate.

[0008] In some embodiments of the present application, the solvent further comprises water and an acid, and the acid is preferably sulfuric acid.

[0009] In some embodiments of the present application, the usage ratio of the solvent to the nickel cobalt hydroxide is (3-5) mL: 1 g.

[0010] In some embodiments of the present application, the pH value of the slurry is 5.0-5.5.

[0011] In some embodiments of the present application, the oxidant is at least one of hydrogen peroxide, sodium persulfate, ozone, potassium permanganate, sodium permanganate, potassium persulfate, and ammonium persulfate.

[0012] In some embodiments of the present application, the amount of the oxidant used is 0.8-1.5 times the theoretical amount required to completely oxidize the divalent manganese contained in the nickel cobalt hydroxide.

[0013] In some embodiments of the present application, the temperature of the oxidation reaction is 20°C-95°C, and the time is 0.5h-3h.

[0014] In some embodiments of the present application, the acid used in the first leaching step is at least one of sulfuric acid and hydrochloric acid, preferably sulfuric acid.

[0015] In some embodiments of the present application, the acid leaching pH value of the first leaching step is 0.5-2.5.

[0016] In some embodiments of the present application, the acid leaching temperature of the first leaching step is 55°C-85°C, and the time is 1h-8h.

[0017] In some embodiments of the present application, the nickel content of the first leaching solution is 100 g / L-140 g / L.

[0018] In some embodiments of the present application, the acid leaching of the second leaching process includes leaching an acid solution mixed with the first leaching residue, wherein the acid solution includes at least one of a sulfuric acid solution and a hydrochloric acid solution.

[0019] In some embodiments of the present application, the usage ratio of the acid solution to the first leaching residue is (3-10) mL: 1 g.

[0020] In some embodiments of the present application, the acid leaching temperature of the second leaching step is 70°C-95°C, and the time is 1h-7h.

[0021] In some embodiments of the present application, the acid leaching endpoint pH value of the second leaching step is -1.0 to 0.5.

[0022] In some embodiments of the present application, the separation process includes: an iron removal process, mixing the first leaching solution with a neutralizer to react so as to precipitate iron and obtain iron-precipitated liquid and iron slag; an extraction process, extracting the iron-precipitated liquid to separate nickel and cobalt, and obtaining nickel-containing material and cobalt-containing material.

[0023] In some embodiments of the present application, the neutralizer includes at least one of calcium carbonate, calcium oxide, calcium hydroxide, magnesium oxide, and magnesium hydroxide.

[0024] In some embodiments of the present application, the reaction pH value of the iron removal process is 3.5-5.5.

[0025] In some embodiments of the present application, the reaction temperature of the iron removal process is 70°C-90°C, and the reaction time is 2h-5h.

[0026] In some embodiments of the present application, the extraction process includes: a first extraction step, using a first extractant to extract the post-iron precipitation liquid to separate nickel, cobalt, magnesium from manganese and calcium, and obtaining a first extract containing manganese and calcium and a first raffinate containing nickel, cobalt and magnesium; a second extraction step, using a second extractant to extract the first raffinate to separate nickel from cobalt and magnesium, and obtaining a second extract containing cobalt and magnesium, i.e., a cobalt-containing material, and a second raffinate containing nickel, i.e., a nickel-containing material.

[0027] In some embodiments of the present application, the first extractant includes a P204 extractant after nickel soap.

[0028] In some embodiments of the present application, the saponification rate of the P204 extractant is 15%-40%, and the extraction level is 15-35.

[0029] In some embodiments of the present application, the O / A ratio of the P204 extractant to the iron precipitation liquid is (0.5-2):1.

[0030] In some embodiments of the present application, the second extractant includes a C272 extractant after nickel soap.

[0031] In some embodiments of the present application, the saponification rate of the C272 extractant is 15%-55%, and the extraction level is 15-40.

[0032] In some embodiments of the present application, the O / A ratio of the C272 extractant to the first raffinate is (2-5):1.

[0033] In some embodiments of the present application, the resource recovery method further includes: a washing step, washing the second leaching residue to obtain a washing liquid and a manganese-containing material, wherein the washing liquid is returned to the second leaching step and used for mixed acid leaching with the first leaching residue.

[0034] In some embodiments of the present application, the washing comprises washing the second leaching residue by mixing water and an acid, and the acid is preferably sulfuric acid.

[0035] In some embodiments of the present application, the liquid-to-solid ratio of the washing is (3-10) mL: 1 g.

[0036] In some embodiments of the present application, the washing temperature is 40°C-80°C, and the washing time is 0.5h-5h.

[0037] In some embodiments of the present application, the endpoint pH value of the washing is -1.0 to 2.0.

[0038] Additional technical solutions and advantages of the present application will be partially given in the following description, and partially become apparent from the following description, or be understood through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0040] Figure 1A flow chart of a method for recycling nickel cobalt hydroxide provided in some embodiments of the present application;

[0041] Figure 2 A flow chart of a method for recycling nickel cobalt hydroxide provided in some embodiments of the present application;

[0042] Figure 3 A flow chart of a method for recycling nickel cobalt hydroxide provided in some embodiments of the present application;

[0043] Figure 4 A flow chart of a method for resource recovery of nickel cobalt hydroxide provided in some embodiments of the present application. DETAILED DESCRIPTION

[0044] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0045] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0046] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0047] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0048] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0049] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0050] In the present application, nickel cobalt hydroxide (MHP) generally refers to a mixture of hydroxides including nickel hydroxide, cobalt hydroxide and the like, which can be prepared from raw materials such as laterite nickel ore and nickel sulfide ore.

[0051] The theoretical amount of oxidant refers to the amount of oxidant required to oxidize all divalent manganese contained in nickel cobalt hydroxide into manganese in a higher valence state. For example, in some embodiments, when hydrogen peroxide is used for oxidation, the reactions that occur include: Mn 2+ +H2O2=MnO2+2H + , the theoretical amount of oxidant required can be calculated by this formula.

[0052] Saponification rate = molar amount of the extractant reacting with the alkaline substance / total molar amount of the extractant × 100%.

[0053] O / A ratio refers to the phase ratio, that is, the volume ratio of the organic phase to the aqueous phase.

[0054] The liquid-to-solid ratio refers to the ratio of the volume of the liquid (unit: milliliter) to the mass of the solid (unit: gram). For example, the liquid-to-solid ratio can be 4mL:1g.

[0055] Solid-liquid separation refers to the process of separating solids and liquids, and the method of solid-liquid separation can be any method of separating solids and liquids known in the art. For example, in some embodiments, solid-liquid separation can be performed by centrifugation, tilting, filtration, etc., and the solid-liquid separation herein can be performed with reference to the above methods.

[0056] Reference Figure 1 As shown, the embodiment of the present application provides a method for recycling nickel cobalt hydroxide, comprising the following steps:

[0057] S100, oxidation step, slurrying the nickel cobalt hydroxide to obtain a slurry, mixing the slurry with an oxidant to carry out an oxidation reaction so that the divalent manganese contained in the nickel cobalt hydroxide is oxidized into a higher valent manganese in a solid form to obtain an oxidized material.

[0058] S200, a first leaching step, wherein the oxidized material is subjected to acid leaching to leach nickel and cobalt, thereby obtaining a first leaching solution and a first leaching residue containing manganese in a higher valence state.

[0059] S300, a second leaching process, wherein the first leaching residue is subjected to acid leaching to further leach nickel and cobalt to obtain a second leaching solution and a second leaching residue containing manganese in a higher valence state, wherein the second leaching solution is returned to the oxidation process and used for mixing with nickel cobalt hydroxide to form a slurry.

[0060] S400, a separation step of separating the nickel and cobalt contained in the first leaching solution to obtain a nickel-containing material and a cobalt-containing material.

[0061] The resource recovery treatment method provided in the embodiment of the present application is to oxidize the divalent manganese contained in the nickel cobalt hydroxide into a higher valence manganese in a solid form in the oxidation process, so that manganese is difficult to be leached during the acid leaching in the first leaching process, thereby separating manganese from other possible elements such as nickel and cobalt that are more easily leached, and obtaining a first leaching solution containing nickel and cobalt and a first leaching residue containing manganese; then further leaching the first leaching residue in the second leaching process to obtain a second leaching residue containing manganese with a higher purity, and separating the first leaching solution in the separation process to separate nickel and cobalt, thereby obtaining a nickel-containing material and a cobalt-containing material. Therefore, according to the resource recovery treatment method provided in the embodiment of the present application, the nickel cobalt hydroxide is first oxidized, and then leached and separated in stages, so that various elements such as nickel, cobalt, and manganese contained in the nickel cobalt hydroxide can be fully separated, which is conducive to obtaining various products with higher purity and greater value.

[0062] In some embodiments, in the oxidation process, slurrying includes mixing a solvent with nickel cobalt hydroxide to obtain a slurry, wherein the components of the solvent include a second leachate. Since the second leachate is recycled to be mixed with nickel cobalt hydroxide for slurrying and then circulated for the first leaching process, the nickel, cobalt and other elements contained in the second leachate can be concentrated into the first leachate through the first leaching process, so as to facilitate the subsequent centralized treatment of the first leachate, and at the same time, it is beneficial to improve the leaching effect and reduce the loss of elements such as nickel and cobalt.

[0063] In some embodiments, the solvent further comprises water and an acid, preferably sulfuric acid. In the present embodiment, the pH value of the slurry can be adjusted by adding an acid during slurrying, so that the divalent manganese contained in the nickel cobalt hydroxide can be more easily oxidized to a higher valent manganese in a solid form, thereby facilitating the separation of manganese.

[0064] In some embodiments, the ratio of the solvent to the nickel cobalt hydroxide is (3-5) mL: 1 g. At this time, the nickel cobalt hydroxide can be controlled to be dispersed in the solvent as much as possible, which is conducive to the full mixing of the nickel cobalt hydroxide and the solvent, thereby improving the effect of subsequent leaching.

[0065] In some embodiments, the pH value of the slurry is 5.0-5.5. When the pH value of the slurry is too high, a large amount of oxidant needs to be consumed, the cost of auxiliary materials is high, and part of manganese will still be leached, and the separation effect of manganese is not ideal; when the pH value of the slurry is too low, the leaching rate of manganese is high, and the separation effect of nickel, cobalt and manganese is poor. The embodiment of the present application controls the pH value of the slurry within the above-mentioned appropriate range to minimize the consumption of oxidant and reduce costs. It is also beneficial to convert divalent manganese into a higher valence state of manganese such as manganese dioxide in a solid form, thereby effectively separating manganese in the subsequent leaching stage, so as to obtain high-grade manganese products such as manganese concentrate.

[0066] Furthermore, the relevant parameters of the oxidant and the oxidation reaction conditions within a suitable range can also be beneficial to the separation of manganese.

[0067] In some embodiments, the oxidant is at least one of hydrogen peroxide, sodium persulfate, ozone, potassium permanganate, sodium permanganate, potassium persulfate, and ammonium persulfate. The above suitable oxidant can effectively oxidize divalent manganese and convert divalent manganese into a solid form such as manganese dioxide that is not easy to leach, so as to separate manganese from elements such as nickel and cobalt that are easier to leach in the subsequent leaching stage.

[0068] In some embodiments, the amount of the oxidant is 0.8-1.5 times the theoretical amount required to oxidize all the divalent manganese contained in the nickel cobalt hydroxide. If the amount of the oxidant is too little, it is difficult to fully oxidize the divalent manganese, and the manganese separation effect is poor; if the amount of the oxidant is too much, it is easy to cause waste of the oxidant and increase the cost. The embodiment of the present application controls the amount of the oxidant within the above-mentioned appropriate range, which can not only ensure the utilization rate of the oxidant, thereby reducing costs, but also effectively oxidize divalent manganese, which is conducive to separating manganese and obtaining manganese-containing products.

[0069] In some embodiments, the temperature of the oxidation reaction is 20° C.-95° C., and the time is 0.5 h-3 h. In this embodiment, the temperature and time of the oxidation reaction are controlled within the above-mentioned suitable ranges, so that the oxidant and divalent manganese can fully react and be converted into a solid form, so as to prevent manganese from being leached in the subsequent leaching stage.

[0070] In order to increase the leaching rate of elements such as nickel and cobalt contained in nickel cobalt hydroxide while avoiding manganese leaching, the conditions of the first leaching step can be optimized.

[0071] In some embodiments, the acid used in the first leaching step is at least one of sulfuric acid and hydrochloric acid, preferably sulfuric acid. Sulfuric acid and hydrochloric acid can fully leach out the nickel, cobalt and other elements contained in the nickel cobalt hydroxide, and can avoid the introduction of anionic impurities as much as possible, which is conducive to reducing the cost of impurity removal.

[0072] In some embodiments, the acid leaching pH value of the first leaching process is 0.5-2.5. If the acid leaching pH value of the first leaching process is too high, the amount of acid may not be enough to fully leach elements such as nickel and cobalt; if the acid leaching pH value of the first leaching process is too low, the acid consumption is large. In this embodiment, by controlling the acid leaching pH value of the first leaching process within a suitable range, it is conducive to sufficient leaching, and can minimize acid consumption and reduce costs.

[0073] In some embodiments, the acid leaching temperature of the first leaching step is 55°C-85°C, and the time is 1h-8h. In this embodiment, the acid leaching temperature and time are within the above-mentioned suitable range, which can fully utilize the acid added in the first acid leaching step and effectively leach the nickel, cobalt and other elements contained in the nickel cobalt hydroxide.

[0074] In some embodiments, the nickel content of the first leachate is 100 g / L-140 g / L.

[0075] In addition, by optimizing the conditions of the second leaching process, the leaching rate of elements such as nickel and cobalt contained in nickel cobalt hydroxide can be further improved.

[0076] In some embodiments, the acid leaching of the second leaching process includes mixing an acid solution with the first leaching residue for leaching, wherein the acid solution includes at least one of a sulfuric acid solution and a hydrochloric acid solution. By adding a suitable acid leaching first leaching residue in the second leaching process, part of the nickel, cobalt and other elements that are not fully leached in the first leaching process can be further leached, so as to improve the leaching rate of the nickel, cobalt and other elements, and at the same time improve the purity of the manganese-containing product.

[0077] Illustratively, in some embodiments, when the acid used in the first leaching process and the second leaching process is sulfuric acid, the resulting leachate is a sulfate solution containing nickel, cobalt and other elements, and the leachate is then separated to obtain a nickel sulfate solution, which can be used in the battery field, for example, as a raw material for preparing a ternary positive electrode material for lithium-ion batteries.

[0078] In some embodiments, the dosage ratio of the acid solution to the first leaching residue is (3-10) mL: 1 g. In some embodiments, the acid leaching temperature of the second leaching process is 70°C-95°C, and the time is 1h-7h. In some embodiments, the acid leaching endpoint pH value of the second leaching process is -1.0 to 0.5. By controlling the conditions of the second leaching process within the above-mentioned appropriate range, all nickel, cobalt and other elements in the first leaching residue can be leached as much as possible, while high-valent manganese and other elements that are difficult to leach are enriched in the second leaching residue, thereby achieving the separation of nickel, cobalt and other elements from manganese in nickel cobalt hydroxide, and the separation efficiency of manganese is high.

[0079] Since nickel cobalt hydroxide may also contain iron, a certain amount of iron will be leached out during the leaching stage. Therefore, in order to improve the purity of nickel-containing and cobalt-containing materials, iron removal operations are required.

[0080] Reference Figure 2 As shown, in some embodiments, the separation process includes:

[0081] S410, iron removal process, mixing the first leaching solution with a neutralizing agent to react so as to precipitate iron, thereby obtaining an iron-precipitated solution and iron slag.

[0082] S420, extraction process, extracting the liquid after iron precipitation to separate nickel and cobalt, and obtaining nickel-containing material and cobalt-containing material.

[0083] In the embodiment of the present application, when separating the nickel and cobalt after leaching, an iron removal process is first performed to remove the iron that may be contained in the first leaching solution; then, the iron precipitation liquid is extracted in the extraction process, so that the nickel and cobalt can be effectively separated, and nickel-containing materials and cobalt-containing materials with higher purity can be obtained.

[0084] In some embodiments, the neutralizing agent includes at least one of calcium carbonate, calcium oxide, calcium hydroxide, magnesium oxide, and magnesium hydroxide. In some embodiments, the reaction pH value of the iron removal process is 3.5-5.5. In some embodiments, the reaction temperature of the iron removal process is 70°C-90°C, and the time is 2h-5h. By controlling the conditions of the iron removal process within the above-mentioned appropriate range, the iron ions in the first leachate can be fully converted into iron hydroxide precipitates, and the loss of nickel and cobalt can be avoided as much as possible. Then, the iron can be separated from the nickel and cobalt by solid-liquid separation, so as to facilitate the subsequent extraction to obtain nickel-containing materials and cobalt-containing materials with lower impurity content.

[0085] When the nickel cobalt hydroxide also contains impurities such as magnesium and calcium, these impurities may be leached out during the leaching stage to form a first leachate containing impurities such as magnesium and calcium. In order to further remove a small amount of manganese contained in the first leachate and possible impurities such as magnesium and calcium, the extraction process may also be optimized.

[0086] Reference Figure 3 As shown, in some embodiments, the extraction process includes:

[0087] S421, a first extraction step, using a first extractant to extract the iron precipitation liquid to separate nickel, cobalt, magnesium from manganese and calcium, to obtain a first extract containing manganese and calcium and a first raffinate containing nickel, cobalt and magnesium;

[0088] S422, a second extraction step, using a second extractant to extract the first raffinate to separate nickel from cobalt and magnesium, to obtain a second extract containing cobalt and magnesium, i.e., a cobalt-containing material, and a second raffinate containing nickel, i.e., a nickel-containing material.

[0089] In the embodiment of the present application, extraction is performed in stages. First, nickel, cobalt, magnesium and manganese and calcium are separated in the first extraction step, so that manganese and calcium impurities can be removed; then, nickel is separated from cobalt and magnesium in the second extraction step, so that nickel-containing materials and cobalt-containing materials with lower impurity contents can be obtained.

[0090] In some embodiments, the first extractant includes a P204 extractant after nickel soap. In some embodiments, the second extractant includes a C272 extractant after nickel soap. Since the manganese content in the first leachate is extremely low, there is no need to perform targeted extraction of manganese in the extraction process. Therefore, the use of the above-mentioned types of extractants is conducive to reducing the construction of extraction lines and wastewater production, reducing extraction construction costs, and improving extraction efficiency. In addition, for nickel-containing products with greater value, the use of extractants after nickel soap for extraction is conducive to separating impurities, thereby improving the quality of nickel-containing materials.

[0091] For example, nickel soap can be added to the extractant to make the extractant contain nickel, such as nickel sulfate. Thus, in the extraction process, the nickel contained in the extractant can be replaced with other metal ions to extract other metal ions, thereby achieving the separation of nickel from other metal ions. For example, when nickel is separated from cobalt, the reaction between the extractant after nickel soap and cobalt may be: NiX2+Co 2+ =CoX2+Ni 2+ , wherein X is an organic anion contained in the extractant. Through the above reaction, cobalt ions can be carried out in the organic phase, while nickel ions exist in the inorganic phase, thereby achieving the separation of nickel and cobalt.

[0092] When using the selected extractant, an alkaline substance such as sodium hydroxide is generally added for saponification before extraction to facilitate the regulation of the pH value of the extraction process, thereby ensuring the extraction effect.

[0093] In some embodiments, the saponification rate of the P204 extractant is 15%-40%, and the extraction level is 15-35. In some embodiments, the O / A ratio of the P204 extractant to the iron precipitation liquid is (0.5-2): 1. In this embodiment, the saponification rate, extraction level and O / A ratio of the P204 extractant are controlled within a suitable range, which is conducive to fully separating nickel, cobalt, magnesium from manganese and calcium.

[0094] In some embodiments, the saponification rate of the C272 extractant is 15%-55%, and the number of extraction stages is 15-40. In some embodiments, the O / A ratio of the C272 extractant to the first raffinate is (2-5):1. In this embodiment, by controlling the saponification rate, extraction stage and O / A ratio of the C272 extractant within a suitable range, it is beneficial to fully separate nickel from cobalt and magnesium. In addition, by extracting with the P204 extractant and the C272 extractant, effective separation of nickel, cobalt, magnesium, manganese and calcium is achieved in a shorter extraction process, which is beneficial to reducing the impurity content of the nickel-containing material, while reducing the extraction construction cost, and reducing the wastewater output and wastewater treatment cost.

[0095] Reference Figure 4 As shown, in some embodiments, the resource processing method further includes:

[0096] S500, a washing step, washing the second leaching residue to obtain a washed liquid and a manganese-containing material, wherein the washed liquid is returned to the second leaching step and used for acid leaching mixed with the first leaching residue.

[0097] In the embodiment of the present application, washing the second leaching residue can remove soluble metal ions such as nickel and cobalt carried by the second leaching residue, thereby obtaining a manganese-containing material with higher purity. In addition, the washed liquid containing soluble metal ions such as nickel and cobalt is returned to the second leaching process, so that nickel and cobalt can be further recovered, and the loss of nickel and cobalt can be reduced, so as to improve the leaching rate of nickel and cobalt.

[0098] In some embodiments, washing includes washing with water and acid mixed with the second leaching residue, and the acid is preferably sulfuric acid. By adding acid, the soluble components such as nickel and cobalt that are not fully leached contained in the second leaching residue can be converted into ionic form, which is conducive to further improving the leaching rate of metals such as nickel and cobalt.

[0099] In some embodiments, the liquid-to-solid ratio of washing is (3-10) mL: 1 g. In some embodiments, the washing temperature is 40°C-80°C, and the washing time is 0.5h-5h. In some embodiments, the end point pH of washing is -1.0 to 2.0. By controlling the washing conditions within the above-mentioned appropriate range, the soluble components contained in the second leaching residue can be fully washed away, which is beneficial to improving the quality of the manganese-containing material and also beneficial to improving the leaching rate of elements such as nickel and cobalt.

[0100] The following examples describe the disclosure of the present application in more detail, and these examples are only used for illustrative purposes, because it is obvious to those skilled in the art that various modifications and variations are made within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are based on mass, and all reagents and raw materials used in the examples are commercially available or synthesized according to conventional methods, and the instruments used in the examples are commercially available.

[0101] The following examples and comparative examples use nickel cobalt hydroxide produced by Tok as a raw material. The composition of the nickel cobalt hydroxide used is shown in Table 1 below.

[0102] Table 1. Composition of nickel cobalt hydroxide

[0103] element Ni Co Mn Fe Mg Moisture content / % 39.33 2.78 6.03 0.162 1.35 48.71

[0104] In the following examples and comparative examples, the calculation method of the leaching rate is as follows:

[0105] Slag leaching rate = (mass of nickel cobalt hydroxide - mass of manganese slag) / mass of nickel cobalt hydroxide × 100%.

[0106] Example 1

[0107] This embodiment provides a method for recycling nickel cobalt hydroxide, comprising the following steps:

[0108] In the oxidation process, 300 g of nickel cobalt hydroxide raw material and 250 mL of production water were taken into a 1-liter beaker, and slurried for 15 minutes at a temperature of 25°C and a stirring speed of 300 rpm. During the slurrying process, sulfuric acid was added to control the pH value of the slurrying end point at 5.5. After the slurrying was completed, potassium persulfate was added for oxidation reaction. The amount of potassium persulfate added was 1.0 times the theoretical amount required to completely oxidize the divalent manganese contained in the nickel cobalt hydroxide. After the addition, the reaction was carried out for 1.5 hours to obtain the oxidized material.

[0109] In the first leaching step, concentrated sulfuric acid is added to the oxidized material to maintain the pH value at 2.0, and the reaction is first carried out at room temperature for 1 hour, and then the temperature is raised to 85°C and kept warm for 1 hour. After the insulation is completed, solid-liquid separation is carried out to obtain the first leachate and the first leach residue.

[0110] In the second leaching process, the first leaching residue is placed in a 1L beaker, 180mL of produced water and 36mL of concentrated sulfuric acid are added, the mixture is stirred for 5min and the temperature is set to 90°C. After reacting for 2.5h, solid-liquid separation is performed to obtain a second leaching solution and a second leaching residue. The second leaching solution is returned to the oxidation process and used for mixing with nickel cobalt hydroxide into slurry.

[0111] In the iron removal process, the first leaching solution is taken into a 2L beaker, the temperature is raised to 80°C, and calcium carbonate powder is slowly added to control the pH value at 4.5. After reacting for 2 hours, solid-liquid separation is performed to obtain iron-precipitated liquid and iron slag.

[0112] In the first extraction step, 50 mL of the liquid after iron precipitation is taken into a 500 mL extraction bottle, and P204 organic extractant after nickel soap is added at an O / A ratio of 1:1 to perform 16-stage extraction to obtain P204 raffinate, which is the first raffinate.

[0113] In the second extraction step, 100 mL of the first raffinate is taken into a 500 mL extraction bottle, and C272 organic extractant after nickel soap is added at an O / A ratio of 4:1 to perform 18-stage extraction to obtain C272 raffinate, i.e., the second raffinate.

[0114] In the washing process, the second leaching residue is placed in a 1L beaker, 100mL of produced water and 5mL of concentrated sulfuric acid are added, and the reaction is stirred at 50°C for 50min, and the pH of the washing end point is controlled to be -1.0-2.0. After the stirring is completed, solid-liquid separation is performed to obtain a washed liquid and a manganese slag, i.e., a manganese-containing material, wherein the washed liquid is returned to the second leaching process and used for mixed acid leaching with the first leaching residue.

[0115] Table 2. Leaching test results of this example

[0116]

[0117] Table 3, extraction test results of this embodiment

[0118]

[0119] Example 2

[0120] The difference from Example 1 is that the oxidants used in the oxidation process are sodium persulfate and hydrogen peroxide, the amount of sodium persulfate added is 0.8 times the theoretical amount required to completely oxidize the divalent manganese contained in the nickel cobalt hydroxide, and the amount of hydrogen peroxide added is 0.3 times the theoretical amount required to completely oxidize the divalent manganese contained in the nickel cobalt hydroxide.

[0121] Table 4. Leaching test results of this embodiment

[0122]

[0123] Table 5. Extraction test results of this example

[0124]

[0125] Example 3

[0126] The difference from Example 1 is that the amount of potassium persulfate added is 0.8 times the theoretical amount required to completely oxidize the divalent manganese contained in the nickel cobalt hydroxide.

[0127] Table 6. Leaching test results of this example

[0128]

[0129] Table 7. Extraction test results of this embodiment

[0130]

[0131] Example 4

[0132] The difference from Example 1 is that the amount of potassium persulfate added is 0.2 times the theoretical amount required to completely oxidize the divalent manganese contained in the nickel cobalt hydroxide.

[0133] Table 8. Leaching test results of this example

[0134]

[0135] Example 5

[0136] The difference from Example 1 is that the pH value of the slurry endpoint of the oxidation process is controlled at 3.0.

[0137] Table 9. Leaching test results of this example

[0138]

[0139] Example 6

[0140] The difference from Example 1 is that the pH value of the slurry endpoint of the oxidation process is controlled at 6.5.

[0141] Table 10, leaching test results of this example

[0142]

[0143] Comparative Example 1

[0144] The difference from Example 1 is that a method for reducing and leaching nickel cobalt hydroxide is adopted, and the specific steps are as follows:

[0145] 300 g of nickel cobalt hydroxide raw material and 320 mL of produced water were placed in a 1 L beaker and slurried for 15 min at a temperature of 25° C. and a stirring speed of 300 rpm.

[0146] After slurrying, concentrated sulfuric acid and sodium sulfite are added to the beaker to maintain the pH value at 2.0. The mixture is reacted at room temperature for 1 hour, and then the temperature is raised to 85°C and kept warm for 1 hour. After the solution becomes clear and the pH value does not change within half an hour, solid-liquid separation is performed to obtain the leachate.

[0147] The leaching solution was placed in a 1L beaker, the temperature was raised to 80°C, and calcium carbonate powder was slowly added to control the pH value at 4.5. After reacting for 2 hours, solid-liquid separation was performed to obtain iron precipitate liquid and iron slag.

[0148] Take 150 mL of the liquid after iron precipitation in a 500 mL extraction bottle, add P204 organic extractant after nickel soap at an O / A ratio of 1:1, and perform 16-stage extraction to obtain P204 raffinate, which is the first raffinate.

[0149] Take 100 mL of P204 raffinate in a 500 mL extraction bottle, add C272 organic extractant after nickel soap at an O / A ratio of 4:1, and perform 18-stage extraction to obtain C272 raffinate, which is the second raffinate.

[0150] Table 11. Extraction test results of this comparative example

[0151]

[0152] Referring to Tables 1 to 11, it can be seen from Examples 1 to 6 and Comparative Example 1 that the amount of manganese leached by the resource recovery treatment method provided in the embodiments of the present application is extremely low, and the impurity content of the obtained nickel-containing material, i.e., the second raffinate, and the manganese-containing material, i.e., the manganese slag, is extremely low, and the quality is good. However, the amount of manganese leached by the "reduction leaching" process in Comparative Example 1 is relatively high, and the nickel-containing material finally obtained contains more manganese, which affects the quality of the nickel-containing material. It can be seen from Examples 1 to 3 and Example 4 that the manganese leaching rate of Example 4 is higher than that of Examples 1 to 3, and when the amount of oxidant added in Examples 1 to 3 is within the preferred range of the present application, manganese and nickel can be better separated at this time. It can be seen from Examples 1 to 3 and Examples 5 to 6 that the manganese leaching rates of Examples 5 to 6 are all higher than those of Examples 1 to 3, and when the slurry pH value of Examples 1 to 3 is within the preferred range of the present application, manganese and nickel can be better separated at this time.

[0153] It can be seen that in the embodiment of the present application, through the process of first oxidation, then two-stage leaching and separation, manganese can be effectively separated from metal elements such as nickel and cobalt, the manganese leaching rate can be reduced to less than 1%, and the nickel leaching rate can reach more than 99.9%, which is conducive to obtaining nickel-containing materials and manganese-containing materials with better quality. In addition, the resource processing method of the embodiment of the present application greatly reduces the cost of auxiliary materials, shortens the extraction process, reduces the extraction construction cost, and also reduces the wastewater output and wastewater treatment costs.

[0154] The various technical features described above can be combined arbitrarily. Although all possible combinations of these technical features are not described, any combination of these technical features should be considered to be covered by this specification as long as there is no contradiction in such combination.

[0155] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for recycling nickel cobalt hydroxide, characterized in that: The following steps are involved: An oxidation step, slurrying the nickel cobalt hydroxide to obtain a slurry, mixing the slurry with an oxidant to carry out an oxidation reaction so that the divalent manganese contained in the nickel cobalt hydroxide is oxidized to a higher valent manganese in a solid form, to obtain an oxidized material; A first leaching step, wherein the oxidized material is subjected to acid leaching to leach nickel and cobalt, thereby obtaining a first leaching solution and a first leaching residue containing the manganese in a higher valence state; a second leaching step, subjecting the first leaching residue to acid leaching to further leach nickel and cobalt, to obtain a second leaching solution and a second leaching residue containing the manganese in a higher valence state, wherein the second leaching solution is returned to the oxidation step and used for mixing with the nickel and cobalt hydroxides to form a slurry; The separation step is to separate the nickel and cobalt contained in the first leaching solution to obtain a nickel-containing material and a cobalt-containing material.

2. The method for recycling nickel cobalt hydroxide according to claim 1, characterized in that: In the oxidation process, the slurrying includes mixing a solvent with the nickel cobalt hydroxide to obtain a slurry, wherein the solvent comprises the second leachate; Optionally, the solvent further comprises water and an acid, and the acid is preferably sulfuric acid; Optionally, the ratio of the solvent to the nickel cobalt hydroxide is (3-5) mL: 1 g; Optionally, the pH value of the slurry is 5.0-5.5; Optionally, the oxidant is at least one of hydrogen peroxide, sodium persulfate, ozone, potassium permanganate, sodium permanganate, potassium persulfate, and ammonium persulfate; Optionally, the amount of the oxidant is 0.8-1.5 times the theoretical amount required to completely oxidize the divalent manganese contained in the nickel cobalt hydroxide; Optionally, the oxidation reaction temperature is 20°C-95°C, and the time is 0.5h-3h.

3. The method for recycling nickel cobalt hydroxide according to claim 1, characterized in that: The acid used in the first leaching step is at least one of sulfuric acid and hydrochloric acid, preferably sulfuric acid; Optionally, the acid leaching pH value of the first leaching step is 0.5-2.5; Optionally, the acid leaching temperature of the first leaching step is 55°C-85°C, and the time is 1h-8h; Optionally, the nickel content of the first leaching solution is 100 g / L-140 g / L.

4. The method for recycling nickel cobalt hydroxide according to claim 1, characterized in that: The acid leaching of the second leaching step includes mixing an acid solution with the first leaching residue for leaching, wherein the acid solution includes at least one of a sulfuric acid solution and a hydrochloric acid solution; Optionally, the dosage ratio of the acid solution to the first leached residue is (3-10) mL: 1 g; Optionally, the acid leaching temperature of the second leaching step is 70°C-95°C, and the time is 1h-7h; Optionally, the acid leaching endpoint pH value of the second leaching step is -1.0 to 0.

5.

5. The method for recycling nickel cobalt hydroxide according to claim 1, characterized in that: The separation process comprises: An iron removal step, mixing the first leaching solution with a neutralizing agent to react so as to precipitate iron, thereby obtaining an iron-precipitated solution and iron slag; The extraction step is to extract the liquid after iron precipitation to separate nickel and cobalt to obtain nickel-containing material and cobalt-containing material.

6. The method for recycling nickel cobalt hydroxide according to claim 5, characterized in that: The neutralizing agent includes at least one of calcium carbonate, calcium oxide, calcium hydroxide, magnesium oxide, and magnesium hydroxide; Optionally, the reaction pH value of the iron removal process is 3.5-5.5; Optionally, the reaction temperature of the iron removal process is 70°C-90°C and the reaction time is 2h-5h.

7. The method for recycling nickel cobalt hydroxide according to claim 5, characterized in that: The extraction process comprises: The first extraction step is to extract the iron precipitation liquid with a first extractant to separate nickel, cobalt, magnesium from manganese and calcium to obtain a first extract containing manganese and calcium and a first raffinate containing nickel, cobalt and magnesium; In the second extraction step, the first raffinate is extracted with a second extractant to separate nickel from cobalt and magnesium, thereby obtaining a second extract containing cobalt and magnesium, i.e., a cobalt-containing material, and a second raffinate containing nickel, i.e., a nickel-containing material.

8. The method for recycling nickel cobalt hydroxide according to claim 7, characterized in that: The first extractant includes a P204 extractant after nickel soap; Optionally, the saponification rate of the P204 extractant is 15%-40%, and the extraction level is 15-35; Optionally, the O / A ratio of the P204 extractant to the iron precipitation liquid is (0.5-2):

1.

9. The method for recycling nickel cobalt hydroxide according to claim 7, characterized in that: The second extractant includes a C272 extractant after nickel soap; Optionally, the saponification rate of the C272 extractant is 15%-55%, and the extraction level is 15-40; Optionally, the O / A ratio of the C272 extractant to the first raffinate is (2-5):

1.

10. The method for recycling nickel cobalt hydroxide according to claim 1, characterized in that: The resource processing method also includes: A washing step, washing the second leaching residue to obtain a washed liquid and a manganese-containing material, wherein the washed liquid is returned to the second leaching step and used for acid leaching mixed with the first leaching residue; Optionally, the washing comprises washing the second leaching residue by mixing water and an acid, wherein the acid is preferably sulfuric acid; Optionally, the liquid-to-solid ratio of the washing is (3-10) mL: 1 g; Optionally, the washing temperature is 40°C-80°C, and the washing time is 0.5h-5h; Optionally, the endpoint pH value of the washing is -1.0 to 2.0.

Citation Information

Patent Citations

  • Step-by-step leaching method of nickel and cobalt from mixture of nickel, cobalt and manganese

    CN109868373A

  • Refining method of high-impurity nickel sulfate

    CN116903055A

  • Method for recovering manganese dioxide from nickel-cobalt-manganese mixture

    CN117327902A

  • Method for separating manganese from crude metal hydroxide, manganese-silicon composite material and application of manganese-silicon composite material

    CN117604278A

  • Process for preparing a high-purity nickel sulphate solution

    WO2024042115A1

Cited By

  • MHP short-process nickel-cobalt-manganese purification liquid preparation technology

    CN120290878A

  • Method for enriching scandium and manganese and extracting and separating nickel and cobalt

    CN121496206A