Preparation method of high-purity beryllium ingot

By using a copper crucible with completely slit bottom and a vacuum suspension smelting process in the preparation of beryllium ingots, the problems of low uniformity and purity of beryllium ingots are solved, and its mechanical properties and composition uniformity are significantly improved.

CN119061272AInactive Publication Date: 2024-12-03NORTHWEST RARE METALS MATERIALS RESEARCH INSTITUTE NINGXIA CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411133142.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing beryllium ingot preparation methods, the beryllium ingot has poor uniformity in tissue, high impurity content and low purity, resulting in productive defects and poor performance.

Method used

The copper crucible with completely slit at the bottom is vacuum suspended and smelted. Through preheating and down-regulating power in stages, the beryllium ingot is ensured to have no inclusions and no obvious defects inside the beryllium ingot, and the uniformity and purity of the composition are improved.

Benefits of technology

The uniform structure, low impurity content and high purity of beryllium ingots are achieved, and its mechanical properties are improved, laying a good foundation for the subsequent process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a preparation method of a high-purity beryllium ingot, and belongs to the technical field of material preparation.The preparation method comprises the steps that after a high-purity beryllium sheet is placed in a copper crucible with a slit in the bottom, the copper crucible is fixed in a smelting furnace, water cooling is conducted for 6-8 min, then vacuumizing is conducted, argon is continuously injected into the smelting furnace till the vacuum pressure in the smelting furnace ranges from-40 Pa to-30 Pa, and the high-purity beryllium ingot is obtained; adjusting a power knob to 20-40kw, keeping for 3-5 minutes, and raising the temperature to 90-110 DEG C; continuously increasing the power at the speed of 15-25kw / min until the temperature of the smelting furnace is increased to 1150-1450 DEG C, and carrying out vacuum suspension smelting to obtain a suspension smelting solution; and reducing the power by stages, cooling the suspension smelting liquid, and sequentially carrying out cooling forming, sand blasting and surface polishing treatment. The beryllium ingot prepared through the method is good in structure uniformity, free of defects, low in impurity content and high in purity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material preparation, and in particular relates to a method for preparing a high-purity beryllium ingot. Background Art

[0002] High-purity beryllium is a light rare metal. Compared with traditional beryllium materials, its purity can reach 3N5 (i.e. 99.95%) or above. It is a material with very special functions. Some of its properties, especially nuclear properties and physical properties, cannot be replaced by any other metal. It plays a very important role in the military industry and atomic energy industry.

[0003] Beryllium metal is located between lithium and boron in the periodic table. According to the diagonal principle, its chemical properties are similar to those of aluminum. It is an active element and generally does not exist as a single substance. At present, the total reserves of beryllium in the world are more than 2.6 trillion tons, but beryllium ore is very scattered, and it is difficult to mine and smelt. Due to its special physical and chemical properties, beryllium has a wide range of uses in the atomic energy industry and aerospace fields. In the atomic energy industry, due to the compactness of beryllium metal structure, it is widely used as a neutron moderator. In spacecraft, beryllium is widely used as structural parts, brackets and other components due to its light density (lighter than aluminum, magnesium, copper, etc.), large heat capacity, high specific strength and other characteristics. It is irreplaceable by any other metal. The main reasons for choosing beryllium are low impact plasma contamination, low radiation power loss, strong oxygen absorption ability, no chemical sputtering (compared with carbon dioxide), low volume tritium inventory, and the possibility of in-situ (or hot chamber) repair of damaged surfaces using plasma spraying. Its main function is to protect the active cooling wall structure from direct contact with high heat flux and plasma to meet the required component life and plasma compatibility.

[0004] At present, conventional forming processes for beryllium ingots include powder metallurgy (hot isostatic pressing or plasma sintering) and vacuum melting. The beryllium sheets prepared by these methods have poor uniformity of structure, are prone to production defects, and contain high impurities and low purity. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing a high-purity beryllium ingot. The beryllium ingot prepared by the method has good uniformity of structure, is defect-free, has a small amount of impurities in the beryllium ingot, and has high purity.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing a high-purity beryllium ingot, the method comprising:

[0008] Step S1, after placing the high-purity beryllium sheet in a copper crucible with a slit at the bottom, fix the copper crucible in a smelting furnace, water-cool for 6 to 8 minutes, evacuate, and then continue to fill the smelting furnace with argon until the vacuum pressure in the smelting furnace is -40 to -30 Pa, adjust the power knob to 20 to 40 kW, maintain for 3 to 5 minutes, and heat to 90 to 110° C.;

[0009] Step S2, continue to increase the power at a rate of 15-25 kW / min until the smelting furnace is heated to 1150-1450° C. to perform vacuum suspension smelting to obtain a suspension smelting liquid;

[0010] Step S3, reducing the power in stages to cool the suspended smelting liquid, and sequentially performing cooling molding, sandblasting and surface polishing treatments.

[0011] Furthermore, in the step S1, the purity of the beryllium sheet is 99.9-99.99%.

[0012] Furthermore, in the step S1, the vacuum degree in the evacuated smelting furnace is 2 to 8*10 -3 Pa.

[0013] Furthermore, in the step S1, the vacuum degree in the evacuated smelting furnace is 4 to 5*10 -3 Pa.

[0014] Furthermore, in the step S2, the vacuum suspension smelting time is 10 to 35 minutes.

[0015] Furthermore, in step S2, the rate of increasing the power is 17-22 kw / min.

[0016] Furthermore, in step S3, the process conditions for reducing the power in stages are:

[0017] The rate of power reduction in the first stage is 15-25kw / min until the power reaches 90-110kw;

[0018] The power reduction rate in the second stage is 30-40kw / min until the power reaches 0kw.

[0019] Furthermore, in the step S3, the cooling molding temperature is 180-220° C., and the cooling molding time is 20-30 minutes.

[0020] Furthermore, at -25 to 200°C, the average linear expansion coefficient of the high-purity beryllium ingot is 10.82 to 12.47×10 -6 / ℃, Rockwell hardness is 51~61.5HRB.

[0021] In summary, the technical solution of the present invention has the following technical effects:

[0022] The present invention adopts a copper crucible with a completely slit bottom, so that a strong electromagnetic field exists at the bottom of the copper crucible, which significantly improves the temperature of the molten pool at the bottom of the copper crucible, and is beneficial to improving the component uniformity of alloy smelting; by preheating the smelting furnace under argon protection and then continuing to heat up, vacuum suspension smelting is achieved, ensuring that there are no inclusions and obvious defects inside the beryllium ingot, improving the purity of the alloy smelting, and the composition is uniform and the organization state is good, and the excellent mechanical properties are provided, laying a good foundation for the subsequent research on the rolling process of the beryllium ingot; the present invention adopts a copper crucible with a completely slit, avoiding the situation that the intensity of the electromagnetic field at the bottom of the existing cold crucible without a slit at the bottom is almost 0, and the temperature is significantly lower than the middle and upper parts of the crucible; the present invention adopts staged power reduction to further improve the component uniformity of alloy smelting. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Embodiment 1:

[0025] Prepare a beryllium sheet sample with a Be content of 100 wt%, about 480 g. The beryllium raw material is a sheet metal with a purity of 3N (ie 99.9%), and the crucible is a copper petal crucible with a slit at the bottom, and the crucible size is 50*160.

[0026] 1) Raw material preparation: Weigh the high-purity beryllium sheet raw material according to the mass percentage of the smelting beryllium sheet. Place the weighed beryllium sheet in a copper crucible with a slit at the bottom, and then fix the copper crucible in the smelting furnace;

[0027] 2) Leak detection and vacuum treatment: Close the suspension furnace door, turn on the power of the control cabinet, turn on the air compressor, turn on the automatic vacuum to extract the air from the furnace, turn on the circulating water of the crucible and coil, turn on the water cooler, and after water cooling for 8 minutes, turn on the vacuum gauge and wait for leak detection and vacuum treatment until 5×10 -3 Pa;

[0028] 3) Melting operation: open the argon bottle, turn off the vacuum gauge, close the main pumping valve, continue to fill the melting furnace with argon to below -30Pa, close the charging valve, start the melting furnace control cabinet, adjust the power knob to 40kw, keep it for 5min, and heat up to 110℃.

[0029] 4) Continuous heating: The temperature is continuously increased by controlling the power adjustment knob, and the heating rate is controlled at 25kw / min until the melting furnace is heated to 1450°C. Vacuum suspension melting is performed for 35 minutes to obtain a suspended melting liquid. It is observed that the raw materials inside the crucible are fully melted and in a suspended state;

[0030] 5) Orderly cooling: adjust the control knob to continuously reduce the power. The cooling rate is controlled at 25kw / min in the first stage. After the power reaches 110kw, it enters the second cooling stage. The cooling rate is controlled at 40kw / min in the second stage until it returns to zero. Turn off the power adjustment knob and turn off the power supply of the control cabinet.

[0031] 6) Cooling and molding: Turn off the power switch, and the beryllium ingot is cooled by circulating water in the crucible at a temperature of 220° C. for 30 minutes, and then molded to obtain a beryllium sheet sample.

[0032] 7) Surface treatment: The beryllium sheet sample obtained in step 6) is subjected to surface polishing treatment.

[0033] The Be content of the beryllium sheet sample in this embodiment is 100wt%, with high purity. After testing, the average linear expansion coefficient is 10.82×10 -6 / ℃, Rockwell hardness is 51HRB.

[0034] Embodiment 2:

[0035] Prepare a beryllium sheet sample with a Be content of 100wt%, about 520g. The beryllium raw material is a sheet metal with a purity of 4N (ie 99.99%), and the crucible is a copper petal crucible with a slit at the bottom, and the crucible size is 50*200.

[0036] 1) Raw material preparation: Weigh the high-purity beryllium sheet raw material according to the mass percentage of the smelting beryllium sheet. Place the weighed beryllium sheet in a copper crucible with a slit at the bottom, and then fix the copper crucible in the smelting furnace;

[0037] 2) Leak detection and vacuum treatment: Close the suspension furnace door, turn on the power of the control cabinet, turn on the air compressor, turn on the automatic vacuum to extract the air from the furnace, turn on the circulating water of the crucible and coil, turn on the water cooler, water cool for 6 minutes, turn on the vacuum gauge, and wait for leak detection and vacuum treatment to 4×10 -3 Pa;

[0038] 3) Melting operation: open the argon bottle, turn off the vacuum gauge, close the main pumping valve, continue to fill the melting furnace with argon to below -40Pa, close the charging valve, start the melting furnace control cabinet, adjust the power knob to 20kw, keep it for 3min, and heat up to 90℃.

[0039] 4) Continuous heating: The temperature is continuously increased by controlling the power adjustment knob, and the heating rate is controlled at 15kw / min until the melting furnace is heated to 1150°C. Vacuum suspension melting is performed for 10 minutes to obtain a suspended melting liquid. It is observed that the raw materials inside the crucible are fully melted and in a suspended state;

[0040] 5) Orderly cooling: Adjust the control knob to continuously reduce the power. The cooling rate is controlled at 15kw / min in the first stage. After the power reaches 90kw, it enters the second cooling stage. The cooling rate is controlled at 30kw / min in the second stage until it returns to zero. Turn off the power adjustment knob and turn off the power supply of the control cabinet.

[0041] 6) Cooling and molding: Turn off the power switch, and the beryllium ingot is cooled for 20 minutes at a temperature of 180°C through circulating water in the crucible, and then molded to obtain a beryllium sheet sample.

[0042] 7) Surface treatment: The beryllium sheet sample obtained in step 6) is subjected to surface polishing treatment.

[0043] The Be content of the beryllium sample in this embodiment is 100wt%, with high purity. After testing, the average linear expansion coefficient is 12.47×10 -6 / ℃, Rockwell hardness is 55.2HRB.

[0044] Embodiment 3:

[0045] Prepare a beryllium sheet sample with a Be content of 100 wt%, about 440 g. The beryllium raw material is a sheet metal with a purity of 4N (99.92%), and the crucible is a copper petal crucible with a slit at the bottom, and the crucible size is 40*160.

[0046] 1) Raw material preparation: Weigh the high-purity beryllium sheet raw material according to the mass percentage of the smelting beryllium sheet. Place the weighed beryllium sheet in a copper crucible with a slit at the bottom, and then fix the copper crucible in the smelting furnace;

[0047] 2) Leak detection and vacuum treatment: Close the suspension furnace door, turn on the power of the control cabinet, turn on the air compressor, turn on the automatic vacuum to extract the air from the furnace, turn on the circulating water of the crucible and coil, turn on the water cooler, and after water cooling for 7 minutes, turn on the vacuum gauge and wait for leak detection and vacuum treatment to 4.5×10 -3 Pa;

[0048] 3) Melting operation: open the argon bottle, turn off the vacuum gauge, close the main pumping valve, continue to fill the melting furnace with argon to below -35Pa, close the charging valve, start the melting furnace control cabinet, adjust the power knob to 30kw, maintain for 4min, and heat to 100℃.

[0049] 4) Continuous heating: The temperature is continuously increased by controlling the power adjustment knob, and the heating rate is controlled at 17kw / min until the melting furnace is heated to 1300°C. Vacuum suspension melting is performed for 20 minutes to obtain a suspended melting liquid. It is observed that the raw materials inside the crucible are fully melted and in a suspended state;

[0050] 5) Orderly cooling: adjust the control knob to continuously reduce the power. The cooling rate is controlled at 20kw / min in the first stage. After the power reaches 100kw, it enters the second cooling stage. The cooling rate is controlled at 35kw / min in the second stage until it returns to zero. Turn off the power adjustment knob and turn off the power supply of the control cabinet.

[0051] 6) Cooling and molding: Turn off the power switch, and the beryllium ingot passes through circulating water in the crucible at a temperature of 200°C. After cooling for 25 minutes, it is molded to obtain a beryllium sheet sample.

[0052] 7) Surface treatment: The beryllium sheet sample obtained in step 6) is subjected to surface polishing treatment.

[0053] The Be content of the beryllium sheet sample in this embodiment is 100wt%, with high purity. After testing, the average linear expansion coefficient is 12.12×10 -6 / ℃, Rockwell hardness is 61.5HRB.

[0054] Please note that the technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. The above embodiments only express several implementation methods of the present application, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several variations and improvements can be made, which all belong to the scope of protection of the present application. Therefore, the scope of protection of the patent in this application shall be based on the attached claims.

Claims

1. A method for preparing a high-purity beryllium ingot, characterized in that: The preparation method comprises: Step S1, after placing the high-purity beryllium sheet in a copper crucible with a slit at the bottom, fix the copper crucible in a smelting furnace, water-cool for 6 to 8 minutes, evacuate, and then continue to fill the smelting furnace with argon until the vacuum pressure in the smelting furnace is -40 to -30 Pa, adjust the power knob to 20 to 40 kW, maintain for 3 to 5 minutes, and heat to 90 to 110° C.; Step S2, continue to increase the power at a rate of 15-25 kW / min until the smelting furnace is heated to 1150-1450° C. to perform vacuum suspension smelting to obtain a suspension smelting liquid; Step S3, reducing the power in stages to cool the suspended smelting liquid, and sequentially performing cooling molding, sandblasting and surface polishing treatments.

2. The preparation method according to claim 1, characterized in that: In the step S1, the purity of the beryllium sheet is 99.9-99.99%.

3. The preparation method according to claim 2, characterized in that: In step S1, the vacuum degree in the evacuated smelting furnace is 2 to 8*10 -3 Pa.

4. The preparation method according to claim 3, characterized in that: In step S1, the vacuum degree in the evacuated smelting furnace is 4 to 5*10 -3 Pa.

5. The preparation method according to claim 4, characterized in that: In the step S2, the vacuum suspension smelting time is 10 to 35 minutes.

6. The preparation method according to any one of claims 1 to 5, characterized in that: In the step S2, the rate of increasing the power is 17-22 kw / min.

7. The preparation method according to claim 6, characterized in that: In step S3, the process conditions for reducing the power in stages are: The rate of power reduction in the first stage is 15-25kw / min until the power reaches 90-110kw; The power reduction rate in the second stage is 30-40kw / min until the power reaches 0kw.

8. The preparation method according to claim 7, characterized in that: In the step S3, the cooling molding temperature is 180-220° C., and the cooling molding time is 20-30 minutes.

9. The preparation method according to claim 8, characterized in that: At -25 to 200°C, the average linear expansion coefficient of the high-purity beryllium ingot is 10.82 to 12.47×10 -6 / ℃, Rockwell hardness is 51~61.5HRB.

Citation Information

Cited By

  • Method for preparing high-purity beryllium rod by Czochralski method

    CN120210938A