Neutral platinum plating solution, application and method for electroplating platinum on surface of titanium substrate

By using neutral platinum plating solution and DC electrodeposition technology with pH value adjusted to 7.0~7.5 on the surface of the titanium substrate, the uneven coating and uneven thickness problems caused by acidic or alkaline plating solution are solved, and dense and uniformity are achieved. The platinum coating reduces process costs and improves corrosion resistance and catalytic reaction efficiency.

CN119061444APending Publication Date: 2024-12-03SHANGHAI INST OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411488847.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing acidic or alkaline plating solution can easily lead to uneven coating, uneven thickness, cracks and pores when electroplating on the surface of titanium substrates, which increases the process cost.

Method used

Using neutral platinum plating solution with a pH value between 7.0 and 7.5, the addition of diammonium hydrogen phosphate, trisodium citrate dihydrate, sodium glutamate and glycol as buffering agents, conductive agents, and brightness The agent and dispersant are combined with DC electrodeposition technology to form a dense and uniform platinum coating.

Benefits of technology

The surface of the coating is flat, uniform thickness, free of cracks, low porosity, dense and fine platinum particles, which reduces process costs, and improves the corrosion resistance and catalytic reaction efficiency of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061444A_ABST
    Figure CN119061444A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of platinum electroplating, in particular to a neutral platinum plating solution and application thereof, and a method for electroplating platinum on the surface of a titanium substrate, the neutral platinum plating solution is obtained by dissolving dinitroso diammineplatinum, diammonium hydrogen phosphate, trisodium citrate dihydrate, sodium glutamate and ethylene glycol in deionized water and adjusting the pH value to 7.0-7.5; the method comprises the following steps that after a titanium base material is subjected to degreasing and acid etching treatment, platinum electroplating is conducted on the titanium base material in the neutral electroplating solution through a direct current electrodeposition method, cleaning and drying are conducted after electroplating, and the platinum-plated titanium base material is obtained. Compared with the prior art, a mixed solution of sulfuric acid and phosphoric acid is used for carrying out surface acid etching treatment on a titanium material, so that the surface binding force of a platinum plating layer and a titanium substrate is improved; and the neutral platinum plating solution can be used for plating a platinum plating layer which is smooth in surface, uniform in thickness, free of cracks, low in porosity, thin in plating layer, small in platinum particle diameter, fine in arrangement and high in adhesion degree through simple operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electroplating platinum, and in particular to a neutral platinum plating solution and application thereof, and a method for electroplating platinum on the surface of a titanium substrate. Background Art

[0002] Platinum-plated titanium technology combines the high strength, low density and excellent corrosion resistance of titanium with the excellent electrochemical inertness and catalytic properties of platinum, opening up a new field of material application. Platinum-plated titanium is used as an efficient plate material in fuel cells, which can significantly improve energy conversion efficiency and promote the development of clean energy. In the field of medical devices, platinum coating enhances the biocompatibility of titanium alloys, providing patients with safer and more reliable implant options. In addition, the corrosion-resistant coating of platinum on titanium provides additional protection for chemical equipment, extending its service life and reducing maintenance costs. The application of this technology is not limited to specific fields. It has shown important value in catalysis, sensors, and the manufacture of components in various extreme environments. It is one of the indispensable material technologies in the development of modern industry and science and technology.

[0003] The pH value of the acidic platinum plating solution is between 0.2 and 3.0. Because the solution contains a large amount of acidic solution, the cathode surface is prone to adsorb hydrogen due to chemical reactions during the electroplating process, resulting in pinholes or cracks on the plated film. The pH value of the alkaline platinum plating solution is between 9.0 and 13.5. Because there is no acidic solution to react and produce hydrogen during the electroplating process, pinholes or cracks are less likely to be produced on the surface. However, the platinum particles deposited on the surface of the titanium sheet during the electroplating process are dispersed on the surface of the titanium sheet, resulting in certain pores between the platinum particles on the surface. The presence of pores will affect the corrosion resistance and service life of the platinum coating.

[0004] Patent CN115787011A discloses an electroplating solution and an electroplating method for preparing a platinum coating on the surface of a titanium collector for hydrogen production by electrolysis of water. However, the electroplating solution is still an acidic platinum plating solution. During the platinum electroplating process, it is necessary to additionally use a large current instantaneous shock and an inert gas to improve the uniformity of the platinum coating. The inert gas is used to improve the uniformity of the platinum coating and the coating thickness exceeds 0.5 microns. The process cost is higher than that of the invention of this patent.

[0005] Based on the above problems, combined with the titanium substrate pretreatment process, it is of great significance to develop a neutral platinum plating solution that is stable, highly operable, and produces a thinner and higher-quality coating, as well as a titanium substrate platinum plating method. Summary of the invention

[0006] The purpose of the present invention is to solve at least one of the above problems and to provide a neutral platinum plating solution and its application, a method for electroplating platinum on the surface of a titanium substrate, so as to solve the problems in the prior art that the platinum plating effect of acidic or alkaline platinum plating solutions is poor, the preparation of a thick coating increases the process cost, and a platinum coating with a smooth surface, uniform thickness, no cracks, low porosity, thin coating, small platinum particle diameter, fine arrangement and high adhesion is plated on the surface of the titanium substrate.

[0007] The purpose of the present invention is achieved through the following technical solutions:

[0008] One of the technical solutions of the present invention is to provide a neutral platinum plating solution, which is prepared by dissolving dinitrosodiammine platinum (P salt), diammonium hydrogen phosphate, trisodium citrate dihydrate, sodium glutamate and ethylene glycol in deionized water, and then adjusting the pH value to 7.0-7.5 by a pH regulator.

[0009] The neutral platinum plating solution of the invention is prepared by adding diammonium hydrogen phosphate to dissolve it in deionized water with P salt and other additives to prepare a neutral platinum plating solution with a pH value between 7.0 and 7.5. Trisodium citrate dihydrate is used as a buffer and a conductive agent, sodium glutamate is used as a brightener and a complexing agent, ethylene glycol is used as a reducing agent and a dispersant, and the electroplating solution prepared by adding P salt, diammonium hydrogen phosphate and other additives has good stability and electroplating performance.

[0010] In the neutral platinum plating solution of the present invention, ethylene glycol is used as a reducing agent and a dispersing agent to reduce the cohesive force between particles, prevent the aggregation of particles in the plating solution, reduce the plating defects caused by the precipitation or separation of particles, and thus improve the consistency and smoothness of the plating layer;

[0011] Sodium glutamate is used as an auxiliary complexing agent, which has both the function of a complexing agent and a certain function of a brightener. It can combine with metal ions during the electroplating process to help the metal ions deposit evenly on the surface of the substrate, forming a smooth surface of the bright layer and reducing the roughness of the coating.

[0012] Trisodium citrate dihydrate is used as a buffer and a conductive agent. During the electroplating process, hydrogen ions are one of the products of the electroplating process, which will cause the pH value of the plating solution to decrease. Trisodium citrate dihydrate, as a buffer, can neutralize the hydrogen ions in the plating solution, maintain the pH value of the plating solution stable, and ensure the normal progress of the electroplating process. Trisodium citrate dihydrate, as a conductive agent, can also expand the current density range of the cathode, so that the metal ions in the plating solution can be more deeply deposited on the surface and inside of the workpiece, thereby improving the thickness and uniformity of the coating.

[0013] The synergistic effect of multiple additives can effectively control the deposition rate and distribution of metal ions during the electroplating process, reduce surface defects and flaws such as pores and dark spots, and improve the dispersion and deep plating ability of the plating solution, while enhancing the cathode current efficiency, so that the obtained coating has low porosity, high brightness and excellent coating quality.

[0014] The pH value of the acidic platinum plating solution is between 0.2 and 3.0. Because the solution contains a large amount of acidic solution, hydrogen is easily accumulated on the cathode surface due to chemical reactions during the electroplating process, causing the solution around the titanium sheet to be dispersed by bubbles, and the surrounding platinum ion concentration decreases, resulting in pinholes or cracks in the plated film, and the plated platinum particles will have the problem of loose arrangement and not dense.

[0015] Alkaline platinum plating solution has a high pH value, which will cause certain corrosion and pollution to the environment and equipment. At the same time, the waste liquid and waste gas generated by the alkaline platinum plating solution during the electroplating process also need to be specially treated. For some metal substrates, they are easily passivated in ammonia alkaline solution, resulting in poor coating quality. Compared with neutral platinum plating solution, the scope of application of alkaline platinum plating solution is limited;

[0016] The neutral platinum plating solution of the present invention has a pH value close to neutral, so the pollution to the environment is relatively small. The neutral platinum plating solution is suitable for electroplating of various metal substrates and has a wide range of applications. In addition, the waste liquid and waste gas generated by the neutral platinum plating solution during the electroplating process are also easier to handle.

[0017] Furthermore, the contents of the components in the platinum plating solution are: 10-20 g / L of dinitrosodiammine platinum, 30-40 g / L of diammonium hydrogen phosphate, 70-100 g / L of trisodium citrate dihydrate, 5-50 g / L of sodium glutamate, and 5-10 mL / L of ethylene glycol.

[0018] Furthermore, the contents of the components in the platinum plating solution are: 12 g / L dinitrosodiammine platinum, 35 g / L diammonium hydrogen phosphate, 76 g / L trisodium citrate dihydrate, 12 g / L sodium glutamate, and 8 mL / L ethylene glycol.

[0019] Furthermore, the pH adjuster includes one or more of ammonia water, sodium hydroxide, calcium hydroxide, trisodium phosphate, trisodium citrate and citric acid, oxalic acid, formic acid, acetic acid, sulfuric acid, phosphoric acid, hydrochloric acid, nitric acid and aminosulfonic acid.

[0020] Furthermore, the pH adjuster is preferably ammonia water and citric acid.

[0021] Furthermore, when the pH of the platinum plating solution is less than 7, ammonia water is used to adjust the pH, and a pH meter is used to measure the pH value of the solution in real time during the adjustment.

[0022] Furthermore, when the pH of the platinum plating solution is greater than 7.5, anhydrous citric acid is used to adjust the pH, and a pH meter is used to measure the pH value of the solution in real time during the adjustment.

[0023] The second technical solution of the present invention is to provide an application of the neutral platinum plating solution as described above in the field of platinum electroplating technology.

[0024] The third technical solution of the present invention is to provide a method for electroplating platinum on the surface of a titanium substrate using the neutral platinum plating solution as described above, the method comprising the following steps: after degreasing and acid etching the titanium substrate, electroplating platinum on the titanium substrate in the neutral plating solution using a direct current electrodeposition method, cleaning and drying after electroplating, and obtaining a platinum-plated titanium substrate through post-treatment.

[0025] Furthermore, the degreasing treatment specifically includes: cleaning the titanium substrate with an organic solution, and then degreasing the titanium substrate with a metal degreasing agent.

[0026] Furthermore, the organic solution is a 75% ethanol solution.

[0027] Furthermore, the acid etching solution in the acid etching process is a mixed solution of sulfuric acid and phosphoric acid.

[0028] Furthermore, the volume ratio of the mixed acid solution is preferably sulfuric acid:phosphoric acid:deionized water=(40-75 mL):(10-30 mL):150 mL.

[0029] Furthermore, the volume ratio of the mixed acid solution is sulfuric acid: phosphoric acid: deionized water = 50 mL: 20 mL: 150 mL.

[0030] Furthermore, the temperature of the mixed acid solution is 60-80° C., and the treatment time for the titanium sheet is 20-50 minutes.

[0031] Furthermore, the temperature of the mixed acid solution is preferably 70° C., and the treatment time for the titanium sheet is preferably 35 minutes.

[0032] Furthermore, in the direct current electrodeposition process, the cathode is the acid-etched titanium substrate, and the anode is a pure platinum sheet.

[0033] Furthermore, the area ratio of the anode to the cathode is 1:(1-8), preferably 1:2.

[0034] Furthermore, during the electroplating process, the temperature of the neutral platinum plating solution is 60-80°C, and the current density is 1.0-10.0 A / dm 2 , the electroplating time is 2 to 10 minutes.

[0035] Furthermore, during the electroplating process, the temperature of the neutral platinum plating solution is preferably 68°C, and the current density is preferably 3A / dm2 The electroplating time is preferably 5 minutes.

[0036] Furthermore, the cleaning and drying comprises: rinsing the platinum-plated titanium substrate with deionized water at room temperature for 2 to 10 seconds; and then placing the substrate in a drying oven for drying at a temperature of 100 to 150° C. for 20 to 30 minutes.

[0037] Furthermore, the rinsing time with deionized water at room temperature is preferably 5-6 seconds; the oven temperature is preferably 110° C., and the time is preferably 30 minutes.

[0038] Furthermore, the post-treatment is to place the dried titanium sheet into a muffle furnace and heat treat and bake it at 300-600° C. for 20-40 minutes.

[0039] Furthermore, the temperature of the heat treatment in the muffle furnace is preferably 450° C., and the heat treatment time is preferably 30 min.

[0040] Furthermore, the titanium substrate is a pure metal titanium sheet containing 99% titanium.

[0041] Furthermore, the step of electroplating platinum includes:

[0042] (1) The titanium substrate was ultrasonically cleaned with a 75% ethanol solution for 15 minutes, and then degreased with a 5 wt.% metal degreasing agent at 55°C for 10 minutes;

[0043] (2) using a mixed acid solution of sulfuric acid, phosphoric acid and pure water to acid-etch the titanium sheet to remove oxides on the surface of the titanium sheet, activate the surface of the titanium sheet, and increase the roughness of the surface of the titanium sheet;

[0044] (3) using the titanium substrate after acid etching in step (2) as a cathode and a pure platinum sheet as an anode, and electroplating platinum on the titanium substrate using a direct current electrodeposition method;

[0045] (4) Rinse the platinum-plated titanium sheet with deionized water at room temperature and then place it in a drying oven for drying;

[0046] (5) The dried titanium sheet is placed in a muffle furnace for post-processing and high-temperature heat treatment and baking to further improve the bonding strength of the coating.

[0047] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0048] Compared with the prior art, the present invention has the following advantages:

[0049] 1. In the central platinum plating solution of the present invention, diammonium hydrogen phosphate is added to dissolve it in deionized water with dinitrosodiammine platinum and other additives to prepare a neutral platinum plating solution with a pH value between 7.0 and 7.5. Dinitrosodiammine platinum is used as the main platinum salt, sodium glutamate is used as a brightener and complexing agent, ethylene glycol is used as a reducing agent and dispersant, trisodium citrate dihydrate is used as a buffer and a conductive agent, and diammonium hydrogen phosphate is added to enable the plating solution to obtain good electroplating ability. Under the synergistic effect of multiple additives, the neutral platinum plating solution can effectively control the deposition rate and distribution of metal ions during the electroplating process, reduce surface defects and flaws such as pores and dark spots, and can also improve the dispersibility and deep plating ability of the plating solution, while enhancing the cathode current efficiency, so that the obtained coating has low porosity, high brightness, excellent coating quality, and dense and fine platinum particles in the prepared coating.

[0050] 2. The present invention performs pre-treatment on the titanium substrate, etches the surface of the titanium substrate with sulfuric acid and phosphoric acid to remove oxides on the surface of the titanium substrate, activates the surface of the titanium sheet, improves the roughness of the surface of the titanium substrate, and enhances the bonding force between the titanium substrate and the platinum coating. The pre-treatment improves the surface defects left by mechanical processing of the titanium substrate, which is beneficial to improving the uniformity of the platinum coating.

[0051] 3. The present invention reduces the thickness of the platinum coating on the surface of the titanium substrate to less than 0.5 μm through the pretreatment of the neutral electroplating solution and the titanium substrate. The thickness is controllable within 0.5 μm, and the particle size of the platinum particles on the titanium is improved, the arrangement is tight, and the overall particle size is fine. In addition to improving the electrical conductivity and corrosion resistance of the titanium substrate, for the platinum-plated titanium plate used as a catalyst carrier, the fineness of its particles can greatly improve the efficiency and yield of the catalytic reaction.

[0052] 4. The neutral platinum plating solution disclosed in the present invention has a simple composition, a pH value close to neutral, and relatively little pollution to the environment. The neutral platinum plating solution is suitable for electroplating of various metal substrates and has a wide range of applications. In addition, the waste liquid and waste gas generated by the neutral platinum plating solution during the electroplating process are also easier to handle, and there are fewer steps for platinum plating on the surface of the titanium substrate, which is convenient to operate and easy to implement. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 This is a scanning electron microscope image of the surface of a titanium sheet that has not been acid-etched, magnified 30,000 times.

[0054] Figure 2 This is a scanning electron microscope image of the surface of the titanium sheet of Example 1 after being corroded by a mixture of sulfuric acid and phosphoric acid at a magnification of 2000 times.

[0055] Figure 3 This is a schematic diagram of the surface of the platinum-coated titanium sheet prepared in Example 1.

[0056] Figure 4This is a scanning electron microscope image of the surface of the platinum-coated titanium sheet prepared in Example 1, magnified 30,000 times.

[0057] Figure 5 The content of each element in the platinum-coated titanium sheet prepared in Example 1 under EDS point scanning is shown in Figure 1. Figure 4 As shown, (a) is the EDS point scan content map in the Spectrum7 interval, (b) is the EDS point scan content map in the Spectrum8 interval, and (c) is the EDS point scan content map in the Spectrum9 interval.

[0058] Figure 6 This is a point map taken on the surface of a sample using an XRF device to test the thickness of the platinum content in the platinum coating of the sample. DETAILED DESCRIPTION

[0059] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0060] Unless otherwise specified, the experimental reagents and raw materials used in the present invention are commercially available.

[0061] The experimental methods without specific conditions in the following implementations are all selected according to conventional methods and conditions, or according to the product instructions. Unless otherwise specified, the experimental instruments used in the present invention are all conventional experimental instruments in the laboratory.

[0062] This patent is dedicated to the development of a neutral platinum plating solution that combines the advantages of both acidic platinum plating solution and alkaline platinum plating solution, and uses a mixed solution of sulfuric acid and phosphoric acid to perform surface acid etching on titanium materials to improve the surface bonding force between the platinum coating and the titanium substrate. This neutral platinum plating solution is combined with a pre-treatment etching method to plate a platinum coating with a smooth surface, uniform thickness, no cracks, low porosity, and high adhesion. Figure 1-5 The present invention is further described.

[0063] Example 1

[0064] In this embodiment, a neutral platinum plating solution is first prepared, comprising the following components:

[0065] 10g / L LP salt (based on the mass of platinum metal), 30g / L diammonium hydrogen phosphate, 70g / L trisodium citrate dihydrate, 10g / L sodium glutamate, 7mL / L ethylene glycol, and the rest is added to deionized water. The main salt (P salt) and each additive are added to the deionized water according to the amount, and then the raw materials are stirred at 90°C using a heated magnetic stirrer to completely dissolve them to form a platinum plating solution.

[0066] Measure the pH value of the platinum plating solution. If the pH value is greater than 7.5, add citric acid to adjust the pH value. If the pH value is less than 7.0, add ammonia water to adjust the pH value. Use a pH meter to adjust the pH value in real time during the adjustment process. Control the pH value between 7.0 and 7.5.

[0067] In this embodiment, the method of pre-treating the surface of the titanium substrate and electroplating platinum on the surface of the titanium sheet using the neutral platinum plating solution as described above is as follows:

[0068] (1) Degreasing: Before electroplating, the titanium sheet was ultrasonically cleaned with 75% ethanol for 15 minutes, and then degreased with 5wt.% metal degreasing agent at 55°C for 10 minutes;

[0069] (2) Acid etching: 40 mL of sulfuric acid, 10 mL of phosphoric acid and 150 mL of pure water were prepared into a mixed acid solution, and the degreased titanium sheet was placed in the mixed acid solution at 70°C for 45 min of acid etching to remove the oxide on the surface of the titanium sheet, activate the surface of the titanium sheet, and improve the surface roughness of the titanium sheet;

[0070] (3) Platinum plating: After the titanium sheet has been acid-etched and rinsed with hot deionized water, it is placed in a prepared neutral platinum plating solution for electroplating. The electroplating conditions are: current density 1A / dm 2 , the plating solution temperature is 65℃, the plating time is 10min, the area ratio of the anode to the cathode is 1:2, and the pH of the plating solution is 7.1;

[0071] (4) Cleaning: Rinse the platinum-plated titanium sheet with deionized water at 65°C for 5-6 seconds, then place it in a drying oven at 110°C and dry it for 30 minutes;

[0072] (5) Post-treatment: The dried titanium sheet was placed in a muffle furnace at 450°C for high-temperature baking for 30 min to obtain a platinum-coated titanium sheet.

[0073] The titanium sheet of Example 1 was observed under a scanning electron microscope before and after acid etching. Figure 1 and Figure 2 As shown in the figure, the surface of the titanium sheet before acid etching is flat and has no pore structure, while the surface of the titanium sheet after acid etching is rough, indicating that the pretreatment of acid etching enhances the bonding force between the titanium substrate and the platinum coating. Figure 2 As shown, the surface roughness of the titanium sheet after acid etching is increased, which is beneficial to improving the bonding force between the titanium substrate and the platinum coating.

[0074] The titanium sheet of Example 1 was placed under a scanning electron microscope for observation after electroplating. The photo of the titanium sheet after electroplating is as follows: Figure 3 As shown, the scanning electron microscope image of the surface of the platinum-coated titanium sheet magnified (30,000) times is shown in Figure 4As shown, the surface of the deposited layer on the titanium sheet after electroplating is relatively dense, without peeling, cracks, and pinholes, indicating that the neutral electroplating solution electroplating method of the present invention is conducive to forming a dense and uniform platinum coating on the surface of the titanium substrate.

[0075] The platinum-coated titanium sheet prepared in Example 1 was subjected to EDS point scanning under an X-ray energy spectrometer to obtain the surface element component content distribution information of the platinum-coated titanium sheet. Figure 5 The content of each element in the platinum-coated titanium sheet prepared in Example 1 under EDS point scanning is shown in Figure 1. Figure 4 As shown, (a) is the EDS scan content map under Spectrum7 interval, (b) is the EDS scan content map under Spectrum8 interval, and (c) is the EDS scan content map under Spectrum9 interval. Table 1 and Table 2 show the surface element component content distribution of the platinum-coated titanium sheet prepared in Example 1 under EDS scan. Figure 5 It can be seen from Table 1 and Table 2 that the titanium sheet coating prepared in Example 1 has no impurities on the surface, the oxygen content is almost 0, and the platinum content is relatively high. The detection depth of EDS is generally about 1 micron. Because the platinum coating is relatively thin, the EDS measurement results include both the platinum coating within 0.5 microns and the titanium element in the titanium substrate. The prepared thinner platinum coating is conducive to reducing process costs and making commercial mass production possible.

[0076] Table 1 Distribution of surface element composition at different positions of platinum-coated titanium sheet under EDS point scanning

[0077]

[0078] Table 2 Distribution of surface element composition of platinum-coated titanium sheet under EDS point scanning

[0079] Statistics O Ti Pt Maximum 0.00 56.18 48.43 Minimum 0.00 51.57 43.82 average value 0.00 54.31 45.69 Standard Deviation 0.00 2.43 2.43

[0080] Example 2

[0081] In this embodiment, a neutral platinum plating solution is prepared, comprising the following components:

[0082] 12g / L L salt (based on the mass of platinum metal), 35g / L diammonium hydrogen phosphate, 76g / L trisodium citrate dihydrate, 12g / L sodium glutamate, 8mL / L ethylene glycol, and the rest is added with deionized water. The main salt and each additive are added to the deionized water according to the amount, and then the raw materials are stirred at 90°C using a heated magnetic stirrer to completely dissolve them to form a platinum plating solution.

[0083] Measure the pH value of the platinum plating solution. If the pH value is greater than 7.5, add citric acid to adjust it. If the pH value is less than 7.0, add ammonia water to adjust it. Use a pH meter to adjust it in real time during the adjustment process. Control the pH value between 7.0 and 7.5.

[0084] In this embodiment, the method of pre-treating the surface of the titanium substrate and electroplating platinum on the surface of the titanium substrate using the neutral platinum plating solution as described above is as follows:

[0085] (1) Degreasing: Before electroplating, the sample was ultrasonically cleaned with 75% ethanol for 15 minutes, and then degreased with 5wt.% metal degreaser at 55°C for 10 minutes;

[0086] (2) Acid etching: 50 mL of sulfuric acid, 20 mL of phosphoric acid and 150 mL of pure water were prepared into a mixed solution, and the cleaned titanium substrate was placed in the mixed solution at 70° C. for 35 min of acid etching to remove the oxide on the surface of the titanium sheet, activate the surface of the titanium sheet, and improve the surface roughness of the titanium sheet;

[0087] (3) Platinum plating: After the titanium sheet has been acid-etched and rinsed with hot deionized water, it is placed in the prepared neutral platinum plating solution for electroplating. The electroplating conditions are: current density of 3A / dm 2 , the plating solution temperature is 68℃, the plating time is 5min, the area ratio of the anode to the cathode is 1:2, and the pH of the plating solution is 7.3;

[0088] (4) Cleaning: Rinse the platinum-plated titanium sheet with deionized water at 70°C for 5-6 seconds, then place it in a drying oven at 110°C and dry it for 30 minutes;

[0089] (5) Post-treatment: The dried titanium sheet was placed in a muffle furnace at 500°C for high-temperature baking for 20 min to obtain a platinum-coated titanium sheet.

[0090] Example 3

[0091] In this embodiment, a neutral platinum plating solution is prepared, comprising the following components:

[0092] 14g / L L salt (based on the mass of platinum metal), 40g / L diammonium hydrogen phosphate, 82g / L trisodium citrate dihydrate, 14g / L sodium glutamate, 9mL / L ethylene glycol, and the rest is added with deionized water. The main salt and each additive are added to the deionized water according to the amount, and then the raw materials are stirred at 90°C using a heated magnetic stirrer to completely dissolve them to form a platinum plating solution.

[0093] Measure the pH value of the platinum plating solution. If the pH value is greater than 7.5, add citric acid to adjust it. If the pH value is less than 7.0, add ammonia water to adjust it. Use a pH meter to adjust it in real time during the adjustment process. Control the pH value between 7.0 and 7.5.

[0094] In this embodiment, the method of pre-treating the surface of the titanium substrate and electroplating platinum on the surface of the titanium substrate using the neutral platinum plating solution as described above is as follows:

[0095] (1) Degreasing: Before electroplating, the sample was ultrasonically cleaned with 75% ethanol for 15 minutes, and then degreased with 5wt.% metal degreaser at 55°C for 10 minutes;

[0096] (2) Acid etching: 55 mL of sulfuric acid, 30 mL of phosphoric acid and 150 mL of pure water were prepared into a mixed solution, and the cleaned titanium substrate was placed in the mixed solution at 66° C. for 25 min of acid etching to remove the oxide on the surface of the titanium sheet, activate the surface of the titanium sheet, and improve the surface roughness of the titanium sheet;

[0097] (3) Platinum plating: After the titanium sheet has been acid-etched and rinsed with hot deionized water, it is placed in the prepared neutral platinum plating solution for electroplating. The electroplating conditions are: current density 5A / dm 2 , the plating solution temperature was 71°C, the plating time was 8 min, the area ratio of the anode to the cathode was 1:2, and the pH of the plating solution was measured to be 7.4;

[0098] (4) Cleaning: Rinse the platinum-plated titanium sheet with deionized water at 70°C for 5-6 seconds, then place it in a drying oven at 110°C and dry it for 30 minutes;

[0099] (5) Post-treatment: The dried titanium sheet was placed in a muffle furnace at 400°C for high-temperature baking for 40 min to obtain a platinum-coated titanium sheet.

[0100] Example 4

[0101] In this embodiment, a neutral platinum plating solution is prepared, comprising the following components:

[0102] 16g / L L salt (based on the mass of platinum metal), 45g / L diammonium hydrogen phosphate, 88g / L trisodium citrate dihydrate, 16g / L sodium glutamate, 10mL / L ethylene glycol, and the rest is added with deionized water. The main salt and each additive are added to the deionized water according to the amount, and then the raw materials are stirred at 90°C using a heated magnetic stirrer to completely dissolve them to form a platinum plating solution.

[0103] Measure the pH value of the platinum plating solution. If the pH value is greater than 7.5, add citric acid to adjust it. If the pH value is less than 7.0, add ammonia water to adjust it. Use a pH meter to adjust it in real time during the adjustment process. Control the pH value between 7.0 and 7.5.

[0104] In this embodiment, the method of pre-treating the surface of the titanium substrate and electroplating platinum on the surface of the titanium substrate using the neutral platinum plating solution as described above is as follows:

[0105] (1) Degreasing: Before electroplating, the sample was ultrasonically cleaned with 75% ethanol for 15 minutes, and then degreased with 5wt.% metal degreaser at 55°C for 10 minutes;

[0106] (2) Acid etching: 75 mL of sulfuric acid, 30 mL of phosphoric acid and 150 mL of pure water were prepared into a mixed solution, and the cleaned titanium substrate was placed in the mixed solution at 63° C. for 20 min of acid etching to remove the oxide on the surface of the titanium sheet, activate the surface of the titanium sheet, and improve the surface roughness of the titanium sheet;

[0107] (3) Platinum plating: After the titanium sheet has been acid-etched and rinsed with hot deionized water, it is placed in the prepared neutral platinum plating solution for electroplating. The electroplating conditions are: current density 10A / dm 2 , the plating solution temperature is 73°C, the plating time is 2 min, the area ratio of the anode to the cathode is 1:2, and the pH of the plating solution is measured to be 7.1;

[0108] (4) Cleaning: Rinse the platinum-plated titanium sheet with deionized water at 70°C for 5-6 seconds, then place it in a drying oven at 110°C and dry it for 30 minutes;

[0109] (5) Post-treatment: The dried titanium sheet was placed in a muffle furnace at 350°C for high-temperature baking for 50 min to obtain a platinum-coated titanium sheet.

[0110] The platinum plating solution formulas of the above Examples 1-4 and the parameters selected in the platinum plating step are shown in Table 3 and Table 4:

[0111] Table 3: Platinum plating solution formula in Examples 1-4

[0112] Components Example 1 Example 2 Example 3 Example 4 Dinitrosodiammineplatinum (P salt) 10g / L 12g / L 14g / L 16g / L Diammonium phosphate 30g / L 35g / L 40g / L 45g / L Trisodium citrate dihydrate 70g / L 76g / L 82g / L 88g / L Monosodium Glutamate 10g / L 12g / L 14g / L 16g / L Ethylene glycol 7mL / L 8mL / L 9mL / L 10mL / L

[0113] Table 4: Parameters selected in the platinum plating step of Examples 1-4

[0114] Components Example 1 Example 2 Example 3 Example 4 Volume of sulfuric acid in the etching solution / mL 40mL 50mL 55mL 75mL Phosphoric acid volume in the etching solution / mL 10mL 20mL 30mL 30mL Acid etching solution temperature / ℃ 70℃ 70℃ 66℃ 63℃ Acid etching time for titanium base / min 45min 35min 25min 20min <![CDATA[Electroplating current density / A / dm 2 > <![CDATA[1A / dm 2 ]]> <![CDATA[3A / dm 2 ]]> <![CDATA[5A / dm 2 ]]> <![CDATA[10A / dm 2 ]]> Plating solution temperature / ℃ 65℃ 68℃ 71℃ 73℃ Plating time / min 10min 5min 8min 2min Plating solution pH 7.1 7.3 7.4 7.1 Deionized water temperature / ℃ 65℃ 70℃ 70℃ 70℃ Muffle furnace baking temperature / ℃ 450℃ 500℃ 400℃ 350℃ Muffle furnace baking time / min 30min 20min 40min 50min

[0115] The platinum-coated titanium sheets prepared in Examples 1-4 were measured for coating thickness using an X-ray fluorescence spectrometer (XRF) instrument model XAU. 16 points were taken on each side of the platinum-coated titanium sheet to test its thickness. By comparing the average value and standard deviation data, the thickness distribution of the platinum coating on the sample was systematically characterized. The thickness distribution of the platinum coating on the platinum-coated titanium sheets prepared in Examples 1-4 is shown in Table 5:

[0116] Table 5: Average platinum coating thickness of platinum-plated samples measured by XRF in Examples 1-4

[0117]

[0118] It can be seen from Table 5 that the thickness of the platinum coating on the platinum-plated titanium sheets obtained in Examples 1-4 is less than 0.5 μm, the standard deviation is 0.01-0.02, and the difference between the maximum value and the minimum value in Examples 1-3 does not exceed 0.05 microns, indicating that the central platinum plating solution of the present invention has strong all-plating ability and deep plating ability, the plating solution is stable, the electroplating performance is excellent, and the platinum coating obtained by electroplating is uniform.

[0119] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A neutral platinum plating solution, characterized in that The neutral platinum plating solution is prepared by dissolving dinitrosodiammine platinum, diammonium hydrogen phosphate, trisodium citrate dihydrate, sodium glutamate and ethylene glycol in deionized water, and adjusting the pH value to 7.0-7.5 by a pH regulator.

2. A neutral platinum plating solution according to claim 1, characterized in that: The contents of the components in the platinum plating solution are: 10-20 g / L of dinitrosodiammine platinum, 30-40 g / L of diammonium hydrogen phosphate, 70-100 g / L of trisodium citrate dihydrate, 5-50 g / L of sodium glutamate, and 5-10 mL / L of ethylene glycol.

3. A neutral platinum plating solution according to claim 1, characterized in that: The pH regulator includes one or more of ammonia water, sodium hydroxide, calcium hydroxide, trisodium phosphate, trisodium citrate, citric acid, oxalic acid, formic acid, acetic acid, sulfuric acid, phosphoric acid, hydrochloric acid, nitric acid and aminosulfonic acid.

4. An application of the neutral platinum plating solution as claimed in claim 1 in the field of platinum electroplating technology.

5. A method for electroplating platinum on a titanium substrate surface using the neutral platinum plating solution as claimed in claim 1, characterized in that: The method comprises the following steps: degreasing and acid etching the titanium substrate, electroplating platinum on the titanium substrate in the neutral electroplating solution by using a direct current electrodeposition method, washing and drying after electroplating, and obtaining a platinum-plated titanium substrate through post-treatment.

6. A method for electroplating platinum on the surface of a titanium substrate according to claim 5, characterized in that: The degreasing treatment specifically includes: using an organic solution to clean the titanium substrate, and then using a metal degreasing agent to degrease the titanium substrate.

7. The method for electroplating platinum on the surface of a titanium substrate according to claim 5, characterized in that: The acid etching solution in the acid etching process is a mixed solution of sulfuric acid and phosphoric acid.

8. The method for electroplating platinum on the surface of a titanium substrate according to claim 7, characterized in that: The volume ratio of the mixed acid solution is sulfuric acid:phosphoric acid:deionized water=(40-75 mL):(10-30 mL):150 mL.

9. The method for electroplating platinum on the surface of a titanium substrate according to claim 5, characterized in that: In the direct current electrodeposition process, the cathode is the acid-etched titanium substrate, and the anode is the pure platinum sheet.

10. The method for electroplating platinum on the surface of a titanium substrate according to claim 9, characterized in that: The area ratio of the anode to the cathode is 1:(1-8).

Citation Information

Cited By

  • Composite preparation method of wear-resistant, high-toughness and oxidation-resistant coating with gradient nano mixed phase structure