Conductive polyester fiber easy to spin and preparation method thereof
By using the physical dispersion and dispersant dispersion method of rod-shaped and spherical TiO2@ATO nanoparticles, the problem of unsmooth spinning of conductive fibers is solved, and the conductivity and spinning fluency are achieved.
Patent Information
- Application Number
- CN202410982973.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-12-03
AI Technical Summary
During the spinning process, existing conductive fibers are prone to spinning not being smooth due to the entanglement of rod-shaped TiO2@ATO particles, which affects the conductive properties.
Rod-shaped and spherical TiO2@ATO nanoparticles are used to improve the degree of dispersion of particles in PET, improve the conductive pathway, and ensure spinning fluency and conductivity through physical dispersion and dispersion combination.
The spinning fluency is improved, while maintaining the resistivity of conductive polyester fibers does not change much, solving the contradiction between conductive properties and spinning fluency.
Smart Images

Figure BDA0004956609480000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of conductive materials, and in particular relates to conductive polyester fiber which is easy to spin and a preparation method thereof. Background Art
[0002] Conductive fiber is a functional fiber with charge conduction ability prepared by adding conductive fillers to the fiber-forming polymer matrix during the spinning process. With the development of science and technology, the market of smart textiles continues to grow, and conductive fibers have also penetrated into various fields such as industry, military, medical, and electronic communications. The continuous expansion of its application fields has put forward more requirements for conductive fibers. At present, conductive fibers mostly use carbon black materials as conductive fillers. Although they have good conductive effects, the prepared conductive fibers are mostly gray-black, which affects the appearance of textiles and limits their application scope. Therefore, the development of light-colored conductive fibers has been paid more and more attention. Light-colored conductive fibers refer to conductive fibers with light or white appearance. Light-colored conductive fibers mostly use semiconductors doped with metal oxides as conductive fillers. Titanium dioxide (TiO2) is a light-colored functional material with excellent physical and chemical properties. A new type of light-colored conductive material TiO2@ATO can be made by coating tin antimony oxide (ATO) on the surface of TiO2. According to the different forms of the core TiO2, it can be divided into rod-shaped, spherical, etc. Since rod-shaped TiO2@ATO is easy to entangle with each other inside the composite to form a conductive path, it is often added to a polymer to make a composite conductive material for spinning. However, when the rod-shaped TiO2@ATO entangles with each other to form a conductive path, it is also easy to block the spinneret hole, causing spinning difficulties. Therefore, a method is needed to improve the spinning smoothness while maintaining the conductivity of the conductive fiber. Summary of the invention
[0003] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0004] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0005] Therefore, the object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing conductive polyester fibers that are easy to spin.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions, including:
[0007] After the conductive material is dispersed, it is evenly mixed with PET powder and melt-spinned to obtain conductive polyester fiber;
[0008] Wherein, the conductive material is TiO2@ATO nano-hybrid particles, which are composed of rod-shaped TiO2@ATO and spherical TiO2@ATO;
[0009] The rod-shaped TiO2@ATO is prepared by high-temperature calcination of rod-shaped TiO2 and ATO conductive materials, and the spherical TiO2@ATO is prepared by high-temperature calcination of spherical TiO2 and ATO conductive materials.
[0010] As a preferred embodiment of the method for preparing the easily spinnable conductive polyester fiber of the present invention, the dispersion treatment includes physical dispersion and dispersant dispersion.
[0011] As a preferred embodiment of the method for preparing the conductive polyester fiber that is easy to spin according to the present invention, the physical dispersion is to place the TiO2@ATO nano-mixed particles in deionized water, first stir for 10 to 50 minutes at a rotation speed of 900 to 1100 r / min, then ultrasonically disperse for 10 to 50 minutes and dry.
[0012] As a preferred embodiment of the method for preparing the conductive polyester fiber that is easy to spin, the dispersant is dispersed as TiO2@ATO nano-mixed particles and the dispersant are stirred and mixed at 70-90°C, and then dried and ground after cooling.
[0013] As a preferred solution of the method for preparing the easily spinnable conductive polyester fiber of the present invention, the dispersant is a silane coupling agent, and the added amount is 0.5wt% to 2wt% of ATO.
[0014] As a preferred embodiment of the method for preparing the easily spinnable conductive polyester fiber of the present invention, the mass ratio of the rod-shaped TiO2@ATO to the spherical TiO2@ATO in the conductive material is 4:1 to 1:4.
[0015] As a preferred solution of the method for preparing the conductive polyester fiber that is easy to spin according to the present invention, the amount of conductive material added to the conductive polyester fiber is 20wt% to 40wt%.
[0016] As a preferred embodiment of the method for preparing the easily spinnable conductive polyester fiber of the present invention, the temperature of the melt spinning is 280-300°C.
[0017] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a conductive polyester fiber that is easy to spin.
[0018] Beneficial effects of the present invention:
[0019] The present invention replaces the rod-shaped TiO2@ATO conductive particles usually added to the light-colored conductive polyester fiber with rod-shaped and spherical TiO2@ATO nano-mixed particles, thereby improving the problem of unsmooth spinning caused by the entanglement of the added rod-shaped TiO2@ATO particles. The dispersion of the TiO2@ATO nano-mixed particles in PET is improved by combining physical dispersion and dispersant dispersion, so that the conductive path is better formed, ensuring that the resistivity of the conductive polyester fiber does not change much while the spinning smoothness is improved. DETAILED DESCRIPTION
[0020] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0021] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0022] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0023] The raw materials used in the present invention are all commercially available unless otherwise specified.
[0024] Spherical TiO2 was purchased from Hengli;
[0025] PET was purchased from Hengli, and the viscosity of PET was 0.68 dl / g.
[0026] (1) Preparation of rod-shaped TiO2@ATO conductive powder by two-step high-temperature calcination method
[0027] 1. Raw material mixing: Nano titanium dioxide (TiO2) powder particle raw material and potassium carbonate powder are uniformly mixed according to the molar ratio of Ti:K=3:1 (potassium carbonate is prepared into an aqueous solution with a mass fraction of 50%, and then TiO2 powder is added), and the obtained mixed solution is heated at 100°C and stirred at high speed for 8 hours to make it a viscous slurry, and then placed in an oven at 100°C to dry, and after complete dehydration, ball milling is performed to make it powdery again;
[0028] 2. Primary calcination: calcine the ball-milled mixture at 1000°C for 8 hours at a heating rate of 10°C / min, and cool to room temperature after calcination to allow it to fully react;
[0029] 3. Boiling: add water to the calcined material and boil it at 100℃ for 6h, then dehydrate and dry after cooling;
[0030] 4. Pickling: Disperse the boiled material in water, heat to 70°C, then add 2 mol / L hydrochloric acid solution until the pH value of the solution stabilizes at 2.5-3, dehydrate and dry.
[0031] 5. Secondary calcination: Heat to 1000°C at a heating rate of 5°C / min and calcine for 3 hours to obtain rod-shaped TiO2 whiskers.
[0032] (2) Preparation of rod-shaped TiO2@ATO and spherical TiO2@ATO nano-conductive powders
[0033] 1. The obtained rod-shaped TiO2 and spherical TiO2 were respectively mixed with water in a mass ratio of 1:10, and the solution pH was adjusted to 3±0.5 with a 2 mol / L hydrochloric acid solution. The temperature was heated to 65°C and the stirring speed was maintained at 100 rpm to obtain a rod-shaped TiO2 suspension and a spherical TiO2 suspension.
[0034] 2. Add the ATO solution with a tin oxide coating ratio of 25% and an antimony oxide doping ratio of 7.5% and a 20% sodium hydroxide (NaOH) solution to the mixed TiO2 whisker suspension and spherical TiO2 suspension at the same time. The drop rate is 120 ml / min. Keep the pH value of the solution stable at 3 and the stirring speed is 100 rpm. After the drop addition is completed, keep the temperature at 65°C and the stirring speed is 100 rpm. Aging for 2 hours. After filtering, spray drying. After drying, in an oxygen atmosphere, heat up to 600°C at a heating rate of 10°C / min, and treat for 2 hours to obtain rod-shaped TiO2@ATO conductive powder and spherical TiO2@ATO conductive powder.
[0035] The performance of the material prepared in the embodiment of the present invention was tested as follows:
[0036] The prepared conductive polyester fiber was tested for resistivity to observe its conductivity. Detection method: At room temperature, take a 10cm fiber sample and clamp the two ends of the monofilament with the iron clamp of the high resistance meter. During the test, adjust the voltage appropriately according to the resistance value of the measured sample. Generally, the voltage is selected to be 100V, and the resistance value is read from the display. Each group of samples is tested 10 times to take the average value, and then the volume resistivity is calculated. The volume resistivity calculation formula is as follows:
[0037]
[0038] In the formula, ρ Vis the volume resistivity, Ω·cm; ρ1 is the sample linear density, dtex; ρ is the sample density, g / cm 3 .
[0039] Example 1
[0040] This embodiment provides a method for preparing conductive polyester fibers that are easy to spin, specifically:
[0041] (1) Conductive materials, i.e., rod-shaped TiO2@ATO and spherical TiO2@ATO nano-hybrid particles, are dispersed by combining physical dispersion and dispersant dispersion. Physical dispersion: Weigh rod-shaped TiO2@ATO and spherical TiO2@ATO nano-particles at a weight ratio of 3:2, respectively, mix them, place them in deionized water, and mechanically stir them for 30 minutes at a speed of 1000r / min. Subsequently, the physically dispersed TiO2@ATO nano-hybrid particles are ultrasonically treated for 30 minutes, and then dried and ground to obtain preliminarily dispersed TiO2@ATO nano-hybrid particles. Dispersant dispersion: Stir and mix the preliminarily dispersed TiO2@ATO nano-hybrid particles with a KH560 aqueous solution containing 1wt% KH560 at 80°C, cool them, dry them, and grind them to obtain TiO2@ATO nano-hybrid particles with good dispersibility.
[0042] (2) Polyethylene terephthalate (PET) slices were crushed into powder in a ball mill, and then mixed with the mixed and dispersed TiO2@ATO nano-mixed particles, with the addition amount of TiO2@ATO nano-mixed particles being 30wt%. The mixture of PET powder and TiO2@ATO nano-mixed particles was then placed in a 100°C oven and dried for 1h, and then added to a twin-screw extruder for melt spinning, with the twin-screw temperature set at 290°C, to smoothly spin out conductive polyester fibers.
[0043] Example 2
[0044] The difference between this embodiment and embodiment 1 is that the mass ratio of rod-shaped TiO2@ATO and spherical TiO2@ATO nanoparticles is adjusted to 4:1, and the rest of the preparation process is the same as that of embodiment 1 to obtain conductive polyester fiber.
[0045] The spinning hole is easily clogged and spinning is not smooth.
[0046] Example 3
[0047] The difference between this embodiment and embodiment 1 is that the mass ratio of rod-shaped TiO2@ATO and spherical TiO2@ATO nanoparticles is adjusted to 1:4, and the rest of the preparation process is the same as that of embodiment 1 to obtain conductive polyester fiber.
[0048] The spinning was smooth and fluent, but the fiber conductivity was poor.
[0049] The performance of the material prepared in the above embodiment was tested, and the comparison results with those in Example 1 are shown in Table 1.
[0050] Table 1
[0051] Resistivity of polyester fiber (kΩ·cm) Example 1 <![CDATA[1.15×10 4 ]]> Example 2 <![CDATA[1.5×10 3 ]]> Example 3 <![CDATA[3×10 4 ]]>
[0052] It can be seen from Table 1 that changing the mixing ratio of rod-shaped TiO2@ATO and spherical TiO2@ATO nano-mixed particles will affect the conductivity and spinning smoothness of the polyester fiber finally prepared. If the spinning is smooth, the conductivity of the fiber remains basically unchanged, while if the spinning is not smooth, its conductivity will be affected. When the proportion of rod-shaped TiO2@ATO nanoparticles is too high, the conductivity of the polyester fiber is improved, but the spinning holes are easily blocked, resulting in unsmooth spinning; when the proportion of spherical TiO2@ATO nanoparticles is too high, the polyester fiber is spun smoothly but the conductivity is poor. In summary, in the present invention, the best technical effect is obtained when the mass ratio of rod-shaped TiO2@ATO and spherical TiO2@ATO nanoparticles is 3:2.
[0053] Example 4
[0054] The difference between this embodiment and embodiment 1 is that the physical stirring time is adjusted to 10 minutes, and the rest of the preparation process is the same as that of embodiment 1 to obtain conductive polyester fiber.
[0055] Example 5
[0056] The difference between this embodiment and embodiment 1 is that the physical stirring time is adjusted to 50 minutes, and the rest of the preparation process is the same as that of embodiment 1 to obtain conductive polyester fiber.
[0057] Example 6
[0058] The difference between this embodiment and embodiment 1 is that the ultrasonic dispersion time is adjusted to 10 minutes, and the rest of the preparation process is the same as that of embodiment 1 to obtain conductive polyester fiber.
[0059] Example 7
[0060] The difference between this embodiment and embodiment 1 is that the ultrasonic dispersion time is adjusted to 50 minutes, and the rest of the preparation process is the same as that of embodiment 1 to obtain conductive polyester fiber.
[0061] Example 8
[0062] The difference between this embodiment and embodiment 1 is that the addition amount of the dispersant is adjusted to 0.5 wt %, and the rest of the preparation process is the same as that of embodiment 1 to obtain conductive polyester fiber.
[0063] Example 9
[0064] The difference between this embodiment and embodiment 1 is that the addition amount of the dispersant is adjusted to 2 wt %, and the rest of the preparation process is the same as that of embodiment 1, to obtain conductive polyester fiber.
[0065] The performance of the material prepared in the above embodiment was tested, and the comparison results with those in Example 1 are shown in Table 2.
[0066] Table 2
[0067] Resistivity of polyester fiber (kΩ·cm) Example 1 <![CDATA[1.15×10 4 ]]> Example 4 <![CDATA[2×10 4 ]]> Example 5 <![CDATA[1.15×10 4 ]]> Example 6 <![CDATA[2.5×10 4 <!-- 4 -->]]> Example 7 <![CDATA[1.15×10 4 ]]> Example 8 <![CDATA[2×10 4 ]]> Example 9 <![CDATA[2.2×10 4 ]]>
[0068] It can be seen from Table 2 that changing the dispersion of TiO2@ATO nano-hybrid particles will affect the conductivity of the polyester fiber finally prepared. When the dispersion is insufficient, the conductive paths in the polyester fiber finally spun are unevenly distributed and the conductivity is poor. In the physical dispersion stage, too long mechanical stirring and ultrasonic treatment will not greatly improve the conductivity of polyester fibers; in the dispersant dispersion stage, adding too much silane coupling agent will hinder the formation of conductive paths due to its own poor conductivity. When the mechanical stirring is 30 minutes, the ultrasonic treatment is 30 minutes, and the amount of silane coupling agent added is 1wt%, the comprehensive effect is the best.
[0069] Example 10
[0070] The difference between this embodiment and embodiment 1 is that the addition amount of TiO2@ATO nano-mixed particles is adjusted to 20wt%, and the rest of the preparation process is the same as that of embodiment 1 to obtain conductive polyester fibers.
[0071] There are few conductive pathways in polyester fibers and their conductivity is poor.
[0072] Embodiment 11
[0073] The difference between this embodiment and embodiment 1 is that the addition amount of TiO2@ATO nano-mixed particles is adjusted to 40wt%, and the rest of the preparation process is the same as that of embodiment 1 to obtain conductive polyester fibers.
[0074] The conductive polyester fiber obtained in this embodiment is difficult to spin due to the low proportion of PET.
[0075] The performance of the material prepared in the above embodiment was tested, and the comparison results with those in Example 1 are shown in Table 3.
[0076] Table 3
[0077] Resistivity of polyester fiber (kΩ·cm) Example 1 <![CDATA[1.15×10 4 ]]> Example 10 <![CDATA[5×10 4 ]]> Embodiment 11 <![CDATA[1×10 3 ]]>
[0078] It can be seen from Table 3 that changing the amount of TiO2@ATO nano-hybrid particles added will affect the conductivity of the polyester fiber finally prepared. When the amount of TiO2@ATO nano-hybrid particles added is too small, there are few conductive paths in the polyester fiber and the conductivity is poor; when the amount of TiO2@ATO nano-hybrid particles added is too much, although the conductivity of the polyester fiber is very good, it is difficult to spin due to the low proportion of PET. When the amount of TiO2@ATO nano-hybrid particles added in Example 1 is 30wt%, the comprehensive effect is the best.
[0079] Comparative Example 1
[0080] The difference between this comparative example and Example 1 is that only rod-shaped TiO2@ATO nanoparticles are selected as the conductive material, and the rest of the preparation process is the same as that of Example 1 to obtain conductive polyester fibers.
[0081] Comparative Example 2
[0082] The difference between this comparative example and Example 1 is that only spherical TiO2@ATO nanoparticles are selected as the conductive material, and the rest of the preparation process is the same as that of Example 1 to obtain conductive polyester fibers.
[0083] Comparative Example 3
[0084] The difference between this comparative example and Example 1 is that the addition amount of TiO2@ATO nano-mixed particles is adjusted to 10wt%, and the rest of the preparation process is the same as that of Example 1 to obtain conductive polyester fibers.
[0085] Comparative Example 4
[0086] The difference between this comparative example and Example 1 is that the addition amount of TiO2@ATO nano-mixed particles is adjusted to 50wt%, and the rest of the preparation process is the same as that of Example 1 to obtain conductive polyester fibers.
[0087] Because the PET content is too low, spinning is extremely difficult and it is difficult to form fibers.
[0088] The performance of the material obtained in the above comparative example was tested, and the comparison results with those of Example 1 are shown in Table 4.
[0089] Table 4
[0090] Resistivity of polyester fiber (kΩ·cm) Example 1 <![CDATA[1.15×10 4 kΩ·cm]]> Comparative Example 1 <![CDATA[1.3×10 3 kΩ·cm]]> Comparative Example 2 <![CDATA[3.5×10 4 kΩ·cm]]> Comparative Example 3 <![CDATA[1×10 6 kΩ·cm]]> Comparative Example 4 <![CDATA[5×10 2 kΩ·cm]]>
[0091] It can be seen from Table 4 that in the process of preparing easy-to-spin conductive polyester fibers, with the continuous increase of spherical particles in the TiO2@ATO nano-hybrid particles, the original phenomenon of poor spinning caused by the entanglement of rod-shaped particles was changed in the final produced polyester fibers; however, when there are too many spherical particles, it is difficult to establish a conductive path in the polyester fiber and the conductivity is greatly reduced.
[0092] During the spinning process, as the amount of TiO2@ATO nano-hybrid particles added increases, the conductivity of polyester fibers gradually improves because TiO2@ATO is a conductive material; but when the amount of TiO2@ATO nano-hybrid particles added is too much, PET accounts for a very small proportion and is difficult to form fibers.
[0093] In summary, currently, the agglomeration is reduced by improving the dispersibility of TiO2@ATO conductive powder, thereby improving the phenomenon of poor spinning, but the effect is not ideal. The rod-shaped whisker structure conductive powder improves the spinning performance by dispersion, but the effect is minimal. The present invention replaces the rod-shaped TiO2@ATO conductive particles usually added to the light-colored conductive polyester fiber with rod-shaped and spherical TiO2@ATO nano-mixed particles, which improves the poor spinning caused by the entanglement of the added rod-shaped TiO2@ATO particles. And the dispersion of TiO2@ATO nano-mixed particles in PET is improved by combining physical dispersion and dispersant dispersion, so that it can better form a conductive path, ensuring that while the spinning fluency is improved, the resistivity of the conductive polyester fiber does not change much.
[0094] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. A method for preparing conductive polyester fiber that is easy to spin, characterized in that: include, After the conductive material is dispersed, it is evenly mixed with PET powder and melt-spinned to obtain conductive polyester fiber; Wherein, the conductive material is TiO2@ATO nano-hybrid particles, which are composed of rod-shaped TiO2@ATO and spherical TiO2@ATO; The rod-shaped TiO2@ATO is prepared by high-temperature calcination of rod-shaped TiO2 and ATO conductive materials, and the spherical TiO2@ATO is prepared by high-temperature calcination of spherical TiO2 and ATO conductive materials.
2. The method for preparing the conductive polyester fiber that is easy to spin as claimed in claim 1, characterized in that: The dispersion treatment includes physical dispersion and dispersant dispersion.
3. The method for preparing the conductive polyester fiber that is easy to spin as claimed in claim 2, characterized in that: The physical dispersion is to place the TiO2@ATO nano-mixed particles in deionized water, first stir for 10 to 50 minutes at a rotation speed of 900 to 1100 r / min, then ultrasonically disperse for 10 to 50 minutes and dry.
4. The method for preparing the easily spinnable conductive polyester fiber according to claim 2, characterized in that: The dispersant is dispersed by stirring and mixing the TiO2@ATO nano-mixed particles and the dispersant at 70-90° C., and drying and grinding after cooling.
5. The method for preparing the easily spinnable conductive polyester fiber according to claim 4, characterized in that: The dispersant is a silane coupling agent.
6. The method for preparing the easily spinnable conductive polyester fiber according to claim 4, characterized in that: The added amount of the dispersant is 0.5wt% to 2wt% of ATO.
7. The method for preparing the easily spinnable conductive polyester fiber according to claim 1, characterized in that: The mass ratio of rod-shaped TiO2@ATO to spherical TiO2@ATO in the conductive material is 4:1 to 1:
4.
8. The method for preparing the easily spinnable conductive polyester fiber according to claim 1, characterized in that: The added amount of the conductive material in the conductive polyester fiber is 20wt% to 40wt%.
9. The method for preparing the easily spinnable conductive polyester fiber according to claim 1, characterized in that: The temperature of the melt spinning is 280-300°C.
10. An easily spinnable conductive polyester fiber prepared by the method according to any one of claims 1 to 9.